Preparation process of ultra-high-density ITO (Indium Tin Oxide) target material
By adding graphene oxide and composite dispersant to the ITO target preparation process, the bonding density of indium oxide and tin oxide powder is improved, the problem of low density of traditional target materials is solved, and the target with high density and low resistivity is achieved Material performance.
Patent Information
- Application Number
- CN202411200559.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-19
AI Technical Summary
The traditional indium tin oxide target has a low density, which affects the performance of subsequent sputtering products.
After sand grinding with tin oxide powder and indium oxide powder, graphene oxide and composite dispersant are added to obtain a preform by spray granulation and cold pressing, and then sintered at normal pressure to improve the density and conductivity of the target material.
It significantly improves the density of ITO target and reduces resistivity, meets the requirements of high density and low resistivity, and improves the performance of the target.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of target materials, and in particular to a process for preparing an ultra-high-density ITO target material. Background Art
[0002] ITO (Tin-doped Indium Oxide) target material is an indium tin composite oxide ceramic and an important optoelectronic functional material. It is often used as a magnetron sputtering target to prepare transparent conductive films on glass, plastic and other substrate materials. It is used in the production of flat-panel display devices such as liquid crystal displays and touch screens.
[0003] With the continuous rise of the flat-panel display equipment industry such as LCDs and touch screens, the performance of displays is constantly improving and the cost is constantly decreasing, and the target coating power is also increasing; however, as the target coating power increases, the requirements for target density are also getting higher and higher.
[0004] Patent technical document CN202010997876.3 discloses a method for preparing indium tin tantalum oxide target. The invention mainly includes six process steps, namely: first ball milling of raw materials, drying and crushing, powder sintering, re-ball milling, pressing and molding, and high-temperature sintering. The sintering is specifically to put the blank into the sintering device for re-sintering, first dehydration, and then heating to 1300-1450℃ at a rate of 0.1-0.5℃ / min for heat preservation and sintering in different temperature stages, and then continue to heat to 1500-1600℃ at a rate of 0.1-0.5℃ / min for heat preservation and sintering in different temperature stages, and nitrogen is introduced during the process; finally, the temperature is lowered to obtain indium tin tantalum oxide target. The indium tin tantalum oxide target of the invention has the characteristics of high purity, high transparency, high conductivity and high mobility, and is a good new type of coating material, but its relative density is between 70%-75%, and the relative density is low, which is bound to affect the performance of the subsequent sputtering products of the target. Summary of the invention
[0005] In view of this, the purpose of the present invention is to propose an ultra-high density ITO target preparation process to solve the problem of low density of traditional indium tin oxide targets.
[0006] Based on the above purpose, the present invention provides a process for preparing an ultra-high density ITO target, comprising the following steps:
[0007] S1: The specific area of tin oxide powder is 8-11m 2 / g, the specific surface area of indium oxide powder is 6-9m 2 / g;
[0008] S2: Mix equal amounts of tin oxide powder and deionized water and sand grind them to obtain a preliminary sand grinding slurry;
[0009] S3: adding graphene oxide to the primary sand-milled slurry, adding a composite dispersant, and ball-milling for 1-3 hours to obtain a secondary sand-milled slurry;
[0010] S4: adding equal amounts of indium oxide powder and deionized water to the secondary sand-milled slurry, and then adding a binder and a defoamer, and sand-milling to obtain a mixed slurry;
[0011] S5: spray granulating the mixed slurry to obtain composite powder;
[0012] S6: cold pressing the composite powder to obtain a preform;
[0013] S7: sintering the preform to obtain an ultra-high density ITO target;
[0014] Preferably, the composite dispersant in step S3 is a mixture of ammonium polyacrylate and sodium dodecylbenzene sulfonate in a weight ratio of 10:0.5-1.
[0015] Preferably, the weight ratio of the tin oxide powder to the indium oxide powder in step S1 is 1:9.
[0016] Preferably, the amount of graphene oxide added in step S3 is 0.5%-2% of the total mass of indium oxide and tin oxide.
[0017] Preferably, the amount of the composite dispersant added in step S3 is 0.5%-1% of the total mass of indium oxide and tin oxide.
[0018] Preferably, the amount of the adhesive added in step S4 is 1%-5% of the total mass of indium oxide and tin oxide.
[0019] Preferably, the adhesive in step S4 is polyvinyl alcohol.
[0020] Preferably, the amount of the defoaming agent added in step S4 is 0.05%-0.1% of the total mass of indium oxide and tin oxide.
[0021] Preferably, the defoaming agent in step S4 is polydimethylsiloxane.
[0022] Preferably, in step S4, the sand mill main machine speed is 579-850 rpm, the double tank grinding number is 4-7 times, and the grinding time is 6-8 hours.
[0023] Preferably, the air inlet temperature of the spray granulation in step S5 is 220-230°C, and the air outlet temperature is 105-115°C.
[0024] Preferably, the molding pressure of the cold press molding in step S6 is 200-250 MPa, and the molding time is 40-60 min.
[0025] Preferably, the sintering in step S7 is normal pressure sintering, first heating to 300°C at a heating rate of 0.3-2.1°C / min for primary dehydration; then heating from 300°C to 650°C at a heating rate of 1.6-2.85°C / min for secondary dehydration; after introducing oxygen, heating from 650°C to 900-1200°C at a heating rate of 4-6°C / min for insulation, and insulation for 1-2h; continuing to heat from 900-1200°C to 1580-1590°C at a heating rate of 0.5-2°C / min for insulation, insulation for 5-40h, cooling, and obtaining an ultra-high density ITO target.
[0026] Preferably, the diameter of the grinding medium used in the sand mill is 0.1-0.8 mm.
[0027] Beneficial effects of the present invention:
[0028] (1) The present invention mixes graphene oxide with raw materials and ball-mills them so that graphene oxide is doped between the raw materials. In the subsequent sintering process, graphene oxide can serve as a binder to make indium oxide and tin oxide powders more tightly combined, thereby further improving the density of the target material obtained. In addition, graphene oxide has good conductivity, which further reduces the resistivity of the target material.
[0029] (2) The present invention further makes the graphene oxide dispersed more evenly and prevents agglomeration by compounding two different dispersants into a composite dispersant. During the sintering process, it can be dispersed more evenly, thereby making the indium oxide and tin oxide powders more closely combined, thereby further improving the density of the final target material. In addition, the graphene oxide has good conductivity, which further reduces the resistivity of the target material. DETAILED DESCRIPTION
[0030] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0031] Example 1: A process for preparing an ultra-high density ITO target material, the specific steps are as follows:
[0032] (1) Select the specific area as 8m 2 / g of tin oxide powder and a specific surface area of 6m 2 / g of indium oxide powder;
[0033] (2) 10 g of tin oxide powder and 10 g of deionized water were mixed and sand-milled until the particle size of the tin oxide powder was D50 ≤ 0.5 μm to obtain a preliminary sand-milled slurry;
[0034] (3) mixing 10 g of ammonium polyacrylate and 0.5 g of sodium dodecylbenzene sulfonate to obtain a composite dispersant;
[0035] (4) adding 0.5 g of graphene oxide to the primary sand-milled slurry, adding 0.5 g of a composite dispersant, and ball-milling at 300 rpm for 1 h to obtain a secondary sand-milled slurry;
[0036] (5) adding 90 g of indium oxide powder and 90 g of deionized water to the secondary sand-milled slurry, and then adding 1 g of polyvinyl alcohol and 0.05 g of polydimethylsiloxane, and sand-milling to obtain a mixed slurry, wherein the diameter of the grinding medium is 0.1 mm, the sand mill main machine speed is 579 rpm, the double-tank grinding number is 4 times, and the grinding time is 6 h;
[0037] (6) spray granulating the mixed slurry to obtain a composite powder, wherein the inlet air temperature of the spray granulation is 220° C. and the outlet air temperature is 105° C.;
[0038] (7) cold pressing the composite powder to obtain a preform, wherein the cold pressing pressure is 200 MPa and the molding time is 40 min;
[0039] (8) The preform is sintered at normal pressure, first heated to 300°C at a heating rate of 0.3°C / min for primary dehydration; then heated from 300°C to 650°C at a heating rate of 1.6°C / min for secondary dehydration; after introducing oxygen, the temperature is then increased from 650°C to 900°C at a heating rate of 4°C / min for insulation for 1-2 hours; the temperature is then increased from 900°C to 158°C at a heating rate of 0.5°C / min for insulation for 5 hours, and the temperature is then lowered to obtain an ultra-high density ITO target.
[0040] Example 2: A process for preparing an ultra-high density ITO target material, the specific steps are as follows:
[0041] (1) Select a specific area of 10m 2 / g of tin oxide powder and a specific surface area of 7.5m 2 / g of indium oxide powder;
[0042] (2) 10 g of tin oxide powder and 10 g of deionized water were mixed and sand-milled until the particle size of the tin oxide powder was D50 ≤ 0.5 μm to obtain a preliminary sand-milled slurry;
[0043] (3) mixing 10 g of ammonium polyacrylate and 0.75 g of sodium dodecylbenzene sulfonate to obtain a composite dispersant;
[0044] (4) adding 1.5 g of graphene oxide to the primary sand-milled slurry, adding 0.75 g of a composite dispersant, and ball-milling at 350 rpm for 2 h to obtain a secondary sand-milled slurry;
[0045] (5) adding 90 g of indium oxide powder and 90 g of deionized water to the secondary sand-milled slurry, and then adding 3 g of polyvinyl alcohol and 0.75 g of polydimethylsiloxane, and sand-milling to obtain a mixed slurry, wherein the diameter of the grinding medium is 0.4 mm, the sand mill main machine speed is 820 rpm, the double-tank grinding number is 5 times, and the grinding time is 7 h;
[0046] (6) spray granulating the mixed slurry to obtain a composite powder, wherein the inlet air temperature of the spray granulation is 225° C. and the outlet air temperature is 110° C.;
[0047] (7) cold pressing the composite powder to obtain a preform, wherein the cold pressing pressure is 230 MPa and the molding time is 50 min;
[0048] (8) The preform is sintered at normal pressure, first heated to 300°C at a heating rate of 1.5°C / min for primary dehydration; then heated from 300°C to 650°C at a heating rate of 2.2°C / min for secondary dehydration; after introducing oxygen, the temperature is then heated from 650°C to 1050°C at a heating rate of 5°C / min and kept warm for 1 hour; the temperature is further heated from 1050°C to 1585°C at a heating rate of 1.5°C / min and kept warm for 20 hours, and then cooled to obtain an ultra-high density ITO target.
[0049] Embodiment 3: A process for preparing an ultra-high density ITO target material, the specific steps are as follows:
[0050] (1) Select a specific area of 10m 2 / g of tin oxide powder and a specific surface area of 8m 2 / g of indium oxide powder;
[0051] (2) 10 g of tin oxide powder and 10 g of deionized water were mixed and sand-milled until the particle size of the tin oxide powder was D50 ≤ 0.5 μm to obtain a preliminary sand-milled slurry;
[0052] (3) mixing 10 g of ammonium polyacrylate and 0.8 g of sodium dodecylbenzene sulfonate to obtain a composite dispersant;
[0053] (4) adding 1.8 g of graphene oxide to the primary sand-milled slurry, adding 0.8 g of a composite dispersant, and ball-milling at 380 rpm for 2 h to obtain a secondary sand-milled slurry;
[0054] (5) adding 90 g of indium oxide powder and 90 g of deionized water to the secondary sand-milled slurry, and then adding 4 g of polyvinyl alcohol and 0.1 g of polydimethylsiloxane, and sand-milling to obtain a mixed slurry, wherein the diameter of the grinding medium is 0.6 mm, the sand mill main machine speed is 840 rpm, the double-tank grinding number is 7 times, and the grinding time is 7 h;
[0055] (6) spray granulating the mixed slurry to obtain a composite powder, wherein the inlet air temperature of the spray granulation is 220° C. and the outlet air temperature is 115° C.;
[0056] (7) cold pressing the composite powder to obtain a preform, wherein the cold pressing pressure is 250 MPa and the molding time is 60 min;
[0057] (8) The preform is sintered at normal pressure, first heated to 300°C at a heating rate of 2°C / min for primary dehydration; then heated from 300°C to 650°C at a heating rate of 2.5°C / min for secondary dehydration; after introducing oxygen, the temperature is then heated from 650°C to 1100°C at a heating rate of 5°C / min and kept warm for 1 hour; then the temperature is further heated from 1100°C to 1590°C at a heating rate of 2°C / min and kept warm for 30 hours, and then cooled to obtain an ultra-high density ITO target.
[0058] Embodiment 4: A process for preparing an ultra-high density ITO target material, the specific steps are as follows:
[0059] (1) Select a specific area of 11m 2 / g of tin oxide powder and a specific surface area of 9m 2 / g of indium oxide powder;
[0060] (2) 10 g of tin oxide powder and 10 g of deionized water were mixed and sand-milled until the particle size of the tin oxide powder was D50 ≤ 0.5 μm to obtain a preliminary sand-milled slurry;
[0061] (3) mixing 10 g of ammonium polyacrylate and 1 g of sodium dodecylbenzene sulfonate to obtain a composite dispersant;
[0062] (4) adding 2 g of graphene oxide to the primary sand-milled slurry, adding 1 g of a composite dispersant, and ball-milling at 400 rpm for 3 h to obtain a secondary sand-milled slurry;
[0063] (5) adding 90 g of indium oxide powder and 90 g of deionized water to the secondary sand-milled slurry, and then adding 5 g of polyvinyl alcohol and 0.1 g of polydimethylsiloxane, and sand-milling to obtain a mixed slurry, wherein the diameter of the grinding medium is 0.8 mm, the sand mill main machine speed is 850 rpm, the double-tank grinding number is 7 times, and the grinding time is 8 h;
[0064] (6) spray granulating the mixed slurry to obtain a composite powder, wherein the inlet air temperature of the spray granulation is 230° C. and the outlet air temperature is 115° C.;
[0065] (7) cold pressing the composite powder to obtain a preform, wherein the cold pressing pressure is 250 MPa and the molding time is 60 min;
[0066] (8) The preform is sintered at normal pressure, first heated to 300°C at a heating rate of 2.1°C / min for primary dehydration; then heated from 300°C to 650°C at a heating rate of 2.85°C / min for secondary dehydration; after introducing oxygen, the temperature is then heated from 650°C to 1200°C at a heating rate of 6°C / min and kept warm for 2 hours; then the temperature is further heated from 1200°C to 1590°C at a heating rate of 2°C / min and kept warm for 5-40 hours, and then the temperature is lowered to obtain an ultra-high density ITO target.
[0067] Comparative Example 1: A process for preparing an ITO target material, the specific steps are as follows:
[0068] (1) Select a specific area of 10m 2 / g of tin oxide powder and a specific surface area of 7.5m 2 / g of indium oxide powder;
[0069] (2) 10 g of tin oxide powder and 10 g of deionized water were mixed and sand-milled until the particle size of the tin oxide powder was D50 ≤ 0.5 μm to obtain a preliminary sand-milled slurry;
[0070] (3) mixing 10 g of ammonium polyacrylate and 0.75 g of sodium dodecylbenzene sulfonate to obtain a composite dispersant;
[0071] (4) adding 0.75 g of the composite dispersant to the primary sand-milled slurry, and ball-milling at 350 rpm for 2 h to obtain a secondary sand-milled slurry;
[0072] (5) adding 90 g of indium oxide powder and 90 g of deionized water to the secondary sand-milled slurry, and then adding 3 g of polyvinyl alcohol and 0.75 g of polydimethylsiloxane, and sand-milling to obtain a mixed slurry, wherein the diameter of the grinding medium is 0.4 mm, the sand mill main machine speed is 820 rpm, the double-tank grinding number is 5 times, and the grinding time is 7 h;
[0073] (6) spray granulating the mixed slurry to obtain a composite powder, wherein the inlet air temperature of the spray granulation is 225° C. and the outlet air temperature is 110° C.;
[0074] (7) cold pressing the composite powder to obtain a preform, wherein the cold pressing pressure is 230 MPa and the molding time is 50 min;
[0075] (8) The preform is sintered at normal pressure, first heated to 300°C at a heating rate of 1.5°C / min for primary dehydration; then heated from 300°C to 650°C at a heating rate of 2.2°C / min for secondary dehydration; after introducing oxygen, the temperature is then heated from 650°C to 1050°C at a heating rate of 5°C / min and kept warm for 1 hour; the temperature is further heated from 1050°C to 1585°C at a heating rate of 1.5°C / min and kept warm for 20 hours, and then cooled to obtain an ultra-high density ITO target.
[0076] Comparative Example 2: A process for preparing an ITO target material, the specific steps are as follows:
[0077] (1) Select a specific area of 10m 2 / g of tin oxide powder and a specific surface area of 7.5m 2 / g of indium oxide powder;
[0078] (2) 10 g of tin oxide powder and 10 g of deionized water were mixed and sand-milled until the particle size of the tin oxide powder was D50 ≤ 0.5 μm to obtain a preliminary sand-milled slurry;
[0079] (3) adding 1.5 g of graphene oxide to the primary sand-milled slurry, adding 0.75 g of ammonium polyacrylate, and ball-milling at 350 rpm for 2 h to obtain a secondary sand-milled slurry;
[0080] (4) adding 90 g of indium oxide powder and 90 g of deionized water to the secondary sand-milled slurry, and then adding 3 g of polyvinyl alcohol and 0.75 g of polydimethylsiloxane, and sand-milling to obtain a mixed slurry, wherein the diameter of the grinding medium is 0.4 mm, the sand mill main machine speed is 820 rpm, the double-tank grinding number is 5 times, and the grinding time is 7 h;
[0081] (5) spray granulating the mixed slurry to obtain a composite powder, wherein the inlet air temperature of the spray granulation is 225° C. and the outlet air temperature is 110° C.;
[0082] (6) cold pressing the composite powder to obtain a preform, wherein the cold pressing pressure is 230 MPa and the molding time is 50 min;
[0083] (7) The preform is sintered at normal pressure, first heated to 300°C at a heating rate of 1.5°C / min for primary dehydration; then heated from 300°C to 650°C at a heating rate of 2.2°C / min for secondary dehydration; after introducing oxygen, the temperature is then heated from 650°C to 1050°C at a heating rate of 5°C / min and kept warm for 1 hour; the temperature is further heated from 1050°C to 1585°C at a heating rate of 1.5°C / min and kept warm for 20 hours, and then cooled to obtain an ultra-high density ITO target.
[0084] Comparative Example 3: A process for preparing an ITO target material, the specific steps are as follows:
[0085] (1) Select a specific area of 10m 2 / g of tin oxide powder and a specific surface area of 7.5m 2 / g of indium oxide powder;
[0086] (2) 10 g of tin oxide powder and 10 g of deionized water were mixed and sand-milled until the particle size of the tin oxide powder was D50 ≤ 0.5 μm to obtain a preliminary sand-milled slurry;
[0087] (3) adding 90 g of indium oxide powder and 90 g of deionized water to the primary sand-milled slurry, and then adding 3 g of polyvinyl alcohol and 0.75 g of polydimethylsiloxane, and sand-milling to obtain a mixed slurry, wherein the diameter of the grinding medium is 0.4 mm, the sand mill main machine speed is 820 rpm, the double-tank grinding number is 5 times, and the grinding time is 7 h;
[0088] (4) spray granulating the mixed slurry to obtain a composite powder, wherein the inlet air temperature of the spray granulation is 225° C. and the outlet air temperature is 110° C.;
[0089] (5) cold pressing the composite powder to obtain a preform, wherein the cold pressing pressure is 230 MPa and the molding time is 50 min;
[0090] (6) The preform is sintered at normal pressure, first heated to 300°C at a heating rate of 1.5°C / min for primary dehydration; then heated from 300°C to 650°C at a heating rate of 2.2°C / min for secondary dehydration; after introducing oxygen, the temperature is then heated from 650°C to 1050°C at a heating rate of 5°C / min and kept warm for 1 hour; the temperature is further heated from 1050°C to 1585°C at a heating rate of 1.5°C / min and kept warm for 20 hours, and then cooled to obtain an ultra-high density ITO target.
[0091] Performance Testing
[0092] Density: The actual density of the target materials prepared in the embodiment and the comparative example was tested by the Archimedean drainage method. The test results are shown in Table 1.
[0093] Resistivity test: The resistivity of the target materials prepared in the embodiment and the comparative example was tested using a SDY-4 four-probe tester. The test results are shown in Table 1.
[0094] Table 1 Performance test results
[0095] <![CDATA[Density / g·m 3 > Resistivity / Ω·cm Example 1 7.282 <![CDATA[2.55×10 -4 ]]> Example 2 7.323 <![CDATA[1.80×10 -4 ]]> Example 3 7.252 <![CDATA[2.76×10 -4 ]]> Example 4 7.243 <![CDATA[3.23×10 -4 ]]> Comparative Example 1 7.153 <![CDATA[9.45×10 -4 ]]> Comparative Example 2 7.215 <![CDATA[5.35×10 -4 ]]> Comparative Example 3 7.145 <![CDATA[11.23×10 -4 ]]>
[0096] Data analysis: It can be seen from Examples 1-4 that the ultra-high density ITO target material preparation process of the present invention can achieve a target material density of 7.323 g·m 3 , and has low resistivity and good conductivity, which can meet the requirements of target material performance in the field of measurement and control sputtering.
[0097] It can be seen from Example 2 and Comparative Examples 1 and 3 that the present invention adds graphene oxide to the raw materials for mixed ball milling, so that the graphene oxide is doped between the raw materials. In the subsequent sintering process, it can be used as a binder to make the indium oxide and tin oxide powders more closely combined, thereby further improving the density of the target material obtained, and the graphene oxide has good conductivity, which further reduces the resistivity of the target material;
[0098] It can be seen from Example 2 and Comparative Examples 1 and 3 that the present invention further makes the graphene oxide dispersed more evenly and prevents agglomeration by compounding two different dispersants into a composite dispersant. During the sintering process, it can be dispersed more evenly, thereby making the indium oxide and tin oxide powders more closely combined, thereby further improving the density of the final target material, and the graphene oxide has good conductivity, which further reduces the resistivity of the target material.
[0099] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention (including the claims) is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
[0100] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A process for preparing an ultra-high density ITO target, characterized in that: The following steps are involved: S1: The specific area of tin oxide powder is 8-11m 2 / g, the specific surface area of indium oxide powder is 6-9m 2 / g; S2: Mix equal amounts of tin oxide powder and deionized water and sand grind them to obtain a preliminary sand grinding slurry; S3: adding graphene oxide to the primary sand-milled slurry, adding a composite dispersant, and ball-milling for 1-3 hours to obtain a secondary sand-milled slurry; S4: adding equal amounts of indium oxide powder and deionized water to the secondary sand-milled slurry, and then adding a binder and a defoamer, and sand-milling to obtain a mixed slurry; S5: spray granulating the mixed slurry to obtain composite powder; S6: cold pressing the composite powder to obtain a preform; S7: sintering the preform to obtain an ultra-high density ITO target; The composite dispersant in step S3 is a mixture of ammonium polyacrylate and sodium dodecylbenzene sulfonate in a weight ratio of 10:0.5-1.
2. The process for preparing an ultra-high density ITO target according to claim 1, characterized in that: The weight ratio of the tin oxide powder to the indium oxide powder in step S1 is 1:
9.
3. The process for preparing an ultra-high density ITO target according to claim 1, characterized in that: The amount of graphene oxide added in step S3 is 0.5%-2% of the total mass of indium oxide and tin oxide.
4. The process for preparing an ultra-high density ITO target according to claim 1, characterized in that: The amount of the composite dispersant added in step S3 is 0.5%-1% of the total mass of indium oxide and tin oxide.
5. The process for preparing an ultra-high density ITO target according to claim 1, characterized in that: In step S4, the amount of the adhesive added is 1%-5% of the total mass of indium oxide and tin oxide, and the amount of the defoaming agent added is 0.05%-0.1% of the total mass of indium oxide and tin oxide.
6. The process for preparing an ultra-high density ITO target according to claim 1, characterized in that: The amount of the defoaming agent added in step S4 is 0.05%-0.1% of the total mass of indium oxide and tin oxide.
7. The process for preparing an ultra-high density ITO target according to claim 1, characterized in that: The inlet air temperature of the spray granulation in step S5 is 220-230°C, and the outlet air temperature is 105-115°C.
8. The process for preparing an ultra-high density ITO target according to claim 1, characterized in that: The molding pressure of the cold press molding in step S6 is 200-250 MPa, and the molding time is 40-60 min.
9. The process for preparing an ultra-high density ITO target according to claim 1, characterized in that: The sintering in step S7 is normal pressure sintering, first heating to 300°C at a heating rate of 0.3-2.1°C / min for primary dehydration; then heating from 300°C to 650°C at a heating rate of 1.6-2.85°C / min for secondary dehydration; after introducing oxygen, heating from 650°C to 900-1200°C at a heating rate of 4-6°C / min for insulation, and insulation for 1-2h; continuing to heat from 900-1200°C to 1580-1590°C at a heating rate of 0.5-2°C / min for insulation, insulation for 5-40h, cooling, and obtaining an ultra-high density ITO target.
10. The process for preparing an ultra-high density ITO target according to claim 1, characterized in that: The diameter of the grinding medium used in the sand mill is 0.1-0.8 mm.
Citation Information
Patent Citations
Preparation method of indium tin tantalum oxide target
CN112110721A
Preparation method of graphene composite conductive oxide target and transparent conductive film thereof
CN103741094A
Method of fabricating sputtering target, sputtering target using the method, and method of manufacturing organic light-emitting display apparatus using the sputtering target
CN104278240A
Lithium battery separator and preparation method thereof
CN109244325A
Slurry-impregnated conductive composite material and preparation method thereof
CN116444988A