Method and system for solving skip plating of MLCC small-size electroplating
By cutting, pre-treating, and hydrophilicizing MLCC workpieces, a pre-plating layer is constructed and electroplating conditions are optimized, solving the problem of incomplete electroplating in small-sized MLCCs and improving the heat resistance and solderability of the products.
Patent Information
- Application Number
- CN202411116261.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-19
AI Technical Summary
Small-sized MLCC products are prone to plating defects during the electroplating process, which can lead to poor product appearance and reduced heat resistance or solderability.
By analyzing the conductive path of MLCC workpieces, cutting and pre-treatment are performed, hydrophilic treatment is added, a pre-plating layer is constructed, and electroplating is carried out under electrolytic conditions to optimize the plating performance, ultimately forming a stable tin plating layer.
It improves the heat resistance and solderability of MLCC products, solves the problem of incomplete electroplating, and ensures that the products achieve the expected performance.
Smart Images

Figure CN118978409A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of workpiece management, and in particular to a method for solving the problem of electroplating leakage in small-size MLCCs. Background Art
[0002] Electroplating skipping refers to the failure of some areas to deposit the expected metal coating during the electroplating process. This is usually caused by uneven current distribution, insufficient surface preparation, and problems with the composition of the plating solution. For example, when electroplating small-sized MLCC (multilayer ceramic capacitor) products, if the surface is not clean or activated enough, it may hinder the adhesion of metal ions, resulting in electroplating skipping. Skipping plating may result in poor product appearance, especially in situations where the electroplating layer is required to provide corrosion protection or conductivity. Skipping plating will reduce the quality and durability of the product.
[0003] In the prior art, the MLCC products to be plated need to be placed in a specific tooling, and then the MLCC products are completely immersed in the plating solution, and the metal ends are plated on the surface of the MLCC product ends using the principle of electrolysis to increase the heat resistance or solderability of the MLCC products. However, during the electroplating liquid injection process, because the small-sized MLCC products are not completely hydrophilic after washing, the small bubbles between the products float up and bring the products to the surface of the liquid. In addition, the surface tension of the products is too large, and some products are always floating and cannot contact the cathode, and thus cannot be plated with the required metal ends, resulting in the failure to achieve the heat resistance or solderability required by the MLCC products, which easily leads to the problem of electroplating leakage of MLCC products. Summary of the invention
[0004] The present invention provides a method for solving the problem of electroplating leakage in small-size MLCC products, and its main purpose is to solve the problem of electroplating leakage in MLCC products.
[0005] To achieve the above object, the present invention provides a method for solving the problem of electroplating leakage in small-sized MLCC, comprising:
[0006] Obtaining an MLCC workpiece, analyzing a conductive path of the MLCC workpiece, cutting the MLCC workpiece based on the conductive path to obtain an MLCC cut surface, pre-treating the MLCC cut surface to obtain a pre-treated MLCC surface, and performing a hydrophilic treatment on the pre-treated MLCC surface to obtain an MLCC hydrophilic surface;
[0007] Performing a hydrophilic post-treatment on the hydrophilic surface of the MLCC to obtain a surface of the MLCC to be electroplated, constructing a pre-plating layer on the surface of the MLCC to be electroplated, and performing a pre-plating post-treatment on the pre-plating layer to obtain a pre-plating layer on the surface of the MLCC;
[0008] Defining a nickel plating solution for the MLCC surface pre-plating layer, and constructing electrolysis conditions for the nickel plating solution, and electroplating the MLCC surface pre-plating layer based on the electrolysis conditions to obtain an MLCC nickel plating layer;
[0009] Detecting the plating performance of the MLCC nickel-plated layer, and when the plating performance is greater than a preset performance, performing nickel-plating post-treatment on the MLCC nickel-plated layer to obtain a target nickel-plated surface of the MLCC;
[0010] The target nickel-plated surface of the MLCC is activated to obtain an active MLCC nickel-plated surface, and an MLCC electroplated tin layer of the active MLCC nickel-plated surface is constructed. The surface attachment elements of the MLCC electroplated tin layer are analyzed, and the surface attachment elements are optimized to obtain the target MLCC electroplated layer.
[0011] Optionally, pre-treating the cut surface of the MLCC to obtain a pre-treated MLCC surface includes:
[0012] Obtaining a non-destructive surface of the cut surface of the MLCC, and cleaning the non-destructive surface to obtain a pure MLCC surface;
[0013] The pure MLCC surface is dried to obtain a dry MLCC surface; the dry MLCC surface is activated to obtain a pre-treated MLCC surface.
[0014] Optionally, the activating treatment of the dried MLCC surface to obtain a pre-treated MLCC surface comprises:
[0015] Obtaining a plasma treatment device for drying the surface of the MLCC; constructing a plasma on the surface of the dried MLCC based on the plasma treatment device;
[0016] The plasma is used to perform surface modification treatment on the surface of the dried MLCC to obtain a pretreated MLCC surface.
[0017] Optionally, the pre-treated MLCC surface is subjected to a hydrophilic treatment to obtain a hydrophilic MLCC surface, comprising:
[0018] Preparing a hydrophilic agent for pretreating the surface of the MLCC;
[0019] Coating the hydrophilic agent on the surface of the pretreated MLCC to obtain a hydrophilic coating surface;
[0020] The hydrophilic coating surface is subjected to post-coating treatment to obtain a hydrophilic MLCC surface.
[0021] Optionally, the surfactant mixture for defining the pre-treatment of the MLCC surface comprises:
[0022] Analyze the hydrophilicity of the MLCC surface;
[0023] Based on the hydrophilic purpose, construct the ionic surfactant for pre-treating the MLCC surface, and define the type of solubilizer for the ionic surfactant;
[0024] Based on the type of the solvent, dissolving the ionic surfactant to obtain a mixed solution;
[0025] The mixed solution is filtered to obtain the surfactant mixture.
[0026] Optionally, the hydrophilic surface of the MLCC is subjected to a hydrophilic post-treatment to obtain a surface of the MLCC to be electroplated, comprising:
[0027] constructing a cleaning layer on the hydrophilic surface of the MLCC, and performing oxidation treatment on the cleaning layer to obtain an oxidation layer;
[0028] Based on the oxide layer, the MLCC workpiece is dried to obtain the MLCC surface to be electroplated.
[0029] Optionally, constructing a pre-plating layer on the surface of the MLCC to be electroplated includes:
[0030] Selecting a pre-plated metal on the surface of the MLCC to be electroplated, and analyzing the material properties of the pre-plated metal;
[0031] Based on the material properties, setting pre-plating parameters of the surface of the MLCC to be electroplated;
[0032] Based on the pre-plating parameters, the pre-plated metal is placed in a preset electroplating tank for electroplating to obtain the pre-plated layer.
[0033] Optionally, based on the electrolysis conditions, electroplating the pre-plated layer on the surface of the MLCC to obtain the MLCC nickel-plated layer comprises:
[0034] Based on the electrolysis conditions, setting the power supply conditions of the MLCC surface pre-plating layer;
[0035] Under the power supply condition, setting the electrode properties of the surface pre-plating layer and the preset nickel plating solution;
[0036] Based on the electrode properties, the surface pre-plating layer and the preset nickel plating solution are electroplated to obtain an MLCC nickel plating layer.
[0037] Optionally, the detecting the plating performance of the MLCC nickel plating layer includes:
[0038] The deposition rate of the nickel plating solution in the MLCC nickel plating layer is calculated using the following formula:
[0039]
[0040] Wherein, V represents the deposition rate, M1 represents the weight of the sample of the nickel electroplating solution in the MLCC nickel-plated layer before nickel plating, M2 represents the weight of the sample of the nickel electroplating solution in the MLCC nickel-plated layer after nickel plating, and t represents the electroplating time of the nickel electroplating solution in the nickel-plated layer;
[0041] The current efficiency of the nickel plating solution in the MLCC nickel plating layer is calculated using the following formula:
[0042]
[0043] Among them, S k represents the current efficiency, m represents the weight gain of the nickel electroplating solution in the nickel plating sample in the MLCC nickel plating layer, I represents the nickel plating current of the nickel electroplating solution in the MLCC nickel plating layer, and k represents the electrochemical equivalent of the nickel electroplating solution in the MLCC nickel plating layer;
[0044] The dispersion of the nickel plating solution in the MLCC nickel plating layer is calculated using the following formula:
[0045]
[0046] Where, T represents the dispersion, S represents the distance ratio between the cathode and the anode of the nickel plating solution in the MLCC nickel plating layer, and M represents the 近 Indicates the weight gain of the nickel plating solution near the cathode in the nickel plating layer of MLCC, M 远 It indicates the weight gain of the nickel plating solution far from the cathode in the nickel plating layer of MLCC;
[0047] The plating performance of the MLCC nickel plating layer is determined according to the deposition speed, the current efficiency and the dispersion.
[0048] A system for solving the problem of electroplating leakage in small-size MLCC, characterized in that the system comprises:
[0049] A hydrophilic treatment module is used to obtain an MLCC workpiece, analyze a conductive path of the MLCC workpiece, cut the MLCC workpiece based on the conductive path to obtain an MLCC cut surface, pre-treat the MLCC cut surface to obtain a pre-treated MLCC surface, and perform a hydrophilic treatment on the pre-treated MLCC surface to obtain an MLCC hydrophilic surface;
[0050] A workpiece pre-plating module is used to perform a hydrophilic post-treatment on the hydrophilic surface of the MLCC to obtain a surface of the MLCC to be electroplated, construct a pre-plating layer on the surface of the MLCC to be electroplated, and perform a pre-plating post-treatment on the pre-plating layer to obtain a pre-plating layer on the surface of the MLCC;
[0051] An electroplating treatment module, used to define a nickel plating solution for the MLCC surface pre-plating layer, and to construct an electrolysis condition for the nickel plating solution, and to electroplating the MLCC surface pre-plating layer based on the electrolysis condition to obtain an MLCC nickel plating layer;
[0052] A nickel plating treatment module, used for detecting the plating performance of the MLCC nickel plating layer, and when the plating performance is greater than a preset performance, performing nickel plating post-treatment on the MLCC nickel plating layer to obtain a target nickel plating surface of the MLCC;
[0053] The electroplating optimization module is used to activate the target nickel-plated surface of the MLCC to obtain an active MLCC nickel-plated surface, and to construct an MLCC electroplated tin layer of the active MLCC nickel-plated surface, analyze the surface attachment elements of the MLCC electroplated tin layer, and optimize the surface attachment elements to obtain the target MLCC electroplated layer.
[0054] The present invention first obtains an MLCC workpiece and analyzes the conductive path of the MLCC workpiece to clarify the electrode structure of the MLCC workpiece, provides a conductive path for MLCC electroplating, and pre-treats the MLCC cut surface to obtain a pre-treated MLCC surface, thereby removing MLCC surface pollutants and improving surface adsorption. The pre-treated MLCC surface is hydrophilically treated to obtain a hydrophilic MLCC surface, thereby enhancing the adhesion of the MLCC surface. Secondly, the present invention performs a hydrophilic post-treatment on the MLCC hydrophilic surface to obtain an MLCC surface to be electroplated, constructs a pre-plating layer on the MLCC surface to be electroplated, and performs a pre-plating post-treatment on the pre-plating layer to obtain an MLCC surface pre-plating layer, thereby providing an intermediate transition layer for nickel electroplating and increasing the adhesion between the nickel layer and the ceramic substrate, thereby solving the problem that during the electroplating liquid injection process, the small-sized MLCC products are not completely hydrophilic after washing, and the small bubbles between the products float up and bring the products to the liquid surface. Furthermore, the present invention defines a nickel plating solution for the MLCC surface pre-plating layer and constructs the electrolysis conditions of the nickel plating solution. Based on the electrolysis conditions, the MLCC surface pre-plating layer is electroplated to obtain an MLCC nickel-plated layer, which can improve the adhesion between the metal and the ceramic substrate, and ensure that the MLCC product can achieve the required heat resistance or weldability. By detecting the plating performance of the MLCC nickel-plated layer, when the plating performance is greater than the preset performance, the MLCC nickel-plated layer is post-processed with nickel plating to obtain an MLCC target nickel-plated surface, which can remove the contamination factor of the MLCC nickel-plated layer, improve the adsorption force between the MLCC nickel-plated layer and other metal layers, and further ensure that the MLCC product can achieve the required heat resistance or weldability. Finally, the embodiment of the present invention activates the MLCC target nickel-plated surface to obtain an active MLCC nickel-plated surface, and constructs an MLCC electroplated tin layer of the active MLCC nickel-plated surface, which can improve the welding performance of the MLCC workpiece. By analyzing the surface attachment elements of the MLCC electroplated tin layer and optimizing the surface attachment elements, the MLCC target electroplated layer is obtained, which can optimize the performance and appearance of the plating and ensure that the MLCC product can achieve the required heat resistance or weldability. Therefore, the method and system for solving the problem of electroplating leakage in small-size MLCCs provided in the embodiments of the present invention can ensure that MLCC products achieve the required heat resistance or weldability, thereby solving the problem of electroplating leakage in MLCC products. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 A schematic flow chart of a method for solving the problem of electroplating leakage in small-sized MLCCs provided in one embodiment of the present invention;
[0056] Figure 2 A functional module diagram of a system for solving the problem of electroplating leakage in small-sized MLCCs provided in one embodiment of the present invention.
[0057] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0058] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.
[0059] The embodiment of the present application provides a method for solving the problem of MLCC small-size electroplating leakage. In the embodiment of the present application, the execution subject of the method for solving the problem of MLCC small-size electroplating leakage includes but is not limited to at least one of the electronic devices such as the server and the terminal that can be configured to execute the method provided by the embodiment of the present application. In other words, the method for solving the problem of MLCC small-size electroplating leakage can be executed by software or hardware installed on the terminal device or the server device, and the software can be a blockchain platform. The server includes but is not limited to: a single server, a server cluster, a cloud server or a cloud server cluster, etc. The server can be an independent server, or it can be a cloud server that provides cloud services, cloud databases, cloud computing, cloud functions, cloud storage, network services, cloud communications, middleware services, domain name services, security services, content delivery networks (Content Delivery Network, CDN), and basic cloud computing services such as big data and artificial intelligence platforms.
[0060] Reference Figure 1 FIG. 1 is a flow chart of a method for solving the problem of electroplating leakage in small-sized MLCCs according to an embodiment of the present invention. In this embodiment, the method for solving the problem of electroplating leakage in small-sized MLCCs includes steps S1 to S5.
[0061] S1. Obtain an MLCC workpiece, analyze the conductive path of the MLCC workpiece, cut the MLCC workpiece based on the conductive path to obtain an MLCC cut surface, pre-treat the MLCC cut surface to obtain a pre-treated MLCC surface, and perform a hydrophilic treatment on the pre-treated MLCC surface to obtain a hydrophilic MLCC surface.
[0062] The embodiment of the present invention obtains an MLCC workpiece and analyzes the conductive path of the MLCC workpiece, so as to clarify the electrode structure of the MLCC workpiece and provide a conductive path for MLCC electroplating. The MLCC workpiece refers to a compact multilayer ceramic capacitor formed by stacking many alternating ceramic dielectric layers and metal electrode layers through high-temperature sintering. The conductive path refers to the charge flow path formed between the internal and external electrodes of the capacitor.
[0063] As an embodiment of the present invention, the analysis of the conductive path of the MLCC workpiece includes: querying the electrode components of the MLCC workpiece and analyzing the distribution structure of the electrode components; based on the distribution structure, combining the electrode components, and then constructing the conductive path of the MLCC workpiece.
[0064] Among them, the electrode component refers to the electrode component of the MLCC workpiece, including internal electrodes and external electrodes. The internal electrode is an internal electrode formed by printing metal paste (usually palladium silver or nickel paste) on a ceramic dielectric sheet inside the MLCC workpiece to form an internal electrode layer and laminating and sintering. In order to provide external conductive contact, the edge of the MLCC will be cut or drilled to expose the internal electrode. The distribution structure refers to the position distribution structure of the internal electrode and the external electrode.
[0065] Optionally, the query of the electrode components of the MLCC workpiece can be obtained by querying the MLCC manufacturing process, the analysis of the distribution structure of the electrode components can be achieved using a microscope, and the combination of the electrode components based on the distribution structure to form the conductive path of the MLCC workpiece can be achieved by electroplating.
[0066] Furthermore, the present invention can lead out the external electrodes of the MLCC workpiece by cutting the MLCC workpiece based on the conductive path, and the MLCC cutting surface refers to the surface of the MLCC workpiece where the internal electrodes are exposed.
[0067] Optionally, the MLCC workpiece is cut based on the conductive path to obtain an MLCC cutting surface, which can be achieved by using a laser cutting machine.
[0068] Furthermore, the embodiment of the present invention pre-treats the cut surface of the MLCC to obtain a pre-treated MLCC surface, thereby removing pollutants from the MLCC surface and improving surface adsorption. The pre-treated MLCC surface refers to the MLCC surface after decontamination treatment.
[0069] As an embodiment of the present invention, the pretreatment of the MLCC cut surface to obtain a pretreated MLCC surface includes: obtaining a lossless surface of the MLCC cut surface, and cleaning the lossless surface to obtain a pure MLCC surface; drying the pure MLCC surface to obtain a dry MLCC surface; activating the dry MLCC surface to obtain a pretreated MLCC surface.
[0070] Among them, the lossless surface refers to the surface of the MLCC workpiece without damage and cracks, the pure MLCC surface refers to the clean surface after removing the contaminants on the MLCC surface, the dry MLCC surface refers to the dry surface after the MLCC surface is air-dried, and the pretreated MLCC surface refers to the surface of the MLCC workpiece that improves the chemical reaction or physical adsorption force between the MLCC workpiece and other substances through specific chemical or physical methods.
[0071] Optionally, the acquisition of the damage-free surface of the MLCC workpiece can be achieved by observation under a microscope, the cleaning of the damage-free surface to obtain a pure MLCC surface can be obtained by immersion cleaning, and the drying of the pure MLCC surface to obtain a dry MLCC surface can be achieved by hot air drying technology.
[0072] Furthermore, in another optional embodiment of the present invention, the activation treatment of the dry MLCC surface to obtain a pretreated MLCC surface includes: obtaining a plasma treatment device for the dry MLCC surface; based on the plasma treatment device, constructing a plasma on the dry MLCC surface, and using the plasma to perform surface modification treatment on the dry MLCC surface to obtain a pretreated MLCC surface.
[0073] Among them, the plasma processing equipment refers to a special equipment that ionizes a specific gas (such as argon, oxygen, nitrogen, fluorinated gas or a mixed gas containing chemical substances) to form a plasma state. The plasma refers to a mixture of various active substances such as ions, electrons, free radicals, etc. formed by the ionization of gas molecules under the action of a high electric field. The surface modification treatment refers to the process operation in which the surface properties change after being bombarded by plasma.
[0074] Optionally, the plasma treatment equipment for obtaining the dry MLCC surface can be obtained through the active treatment requirements of the MLCC surface, the plasma for constructing the dry MLCC surface based on the plasma treatment equipment can be achieved by high-voltage ionization, and the surface modification treatment of the MLCC surface using the plasma can be obtained by bombarding the MLCC surface with the plasma.
[0075] Furthermore, the embodiment of the present invention can enhance the adhesion of the MLCC surface by performing a hydrophilic treatment on the pre-treated MLCC surface to obtain a hydrophilic MLCC surface. The hydrophilic MLCC surface refers to the MLCC surface that can fully combine with the liquid after the hydrophilic treatment.
[0076] As an embodiment of the present invention, the pre-treated MLCC surface is subjected to a hydrophilic treatment to obtain a hydrophilic MLCC surface, comprising: preparing a hydrophilic agent for the pre-treated MLCC surface; coating the hydrophilic agent on the pre-treated MLCC surface to obtain a hydrophilic coating surface; and performing a post-coating treatment on the hydrophilic coating surface to obtain a hydrophilic MLCC surface.
[0077] The hydrophilic agent refers to a chemical additive that can form a chemical bond with the surface of the MLCC, and the hydrophilic coating surface refers to a MLCC coating surface that can attract and easily wet water or other polar liquids.
[0078] Optionally, the hydrophilic agent is coated on the pretreated MLCC surface to obtain a hydrophilic coating surface, which can be achieved using a coating brush. The hydrophilic coating surface is post-treated to obtain a hydrophilic MLCC surface, which can be obtained by washing and then naturally drying.
[0079] Furthermore, in another optional embodiment of the present invention, coating the hydrophilic agent on the surface of the pretreated MLCC to obtain a hydrophilic coating surface includes: defining a surfactant mixture on the surface of the pretreated MLCC, and setting a dipping time and a dipping temperature of the surfactant mixture; based on the dipping time and the dipping temperature, dipping the surfactant mixture on the surface of the pretreated MLCC to obtain a hydrophilic coating surface.
[0080] Among them, the surfactant mixture refers to a mixture composed of two or more surfactants, the dipping time refers to the time for fully immersing the MLCC surface in the solution, the dipping temperature refers to the ambient temperature and the dipping solution temperature during the dipping process of the MLCC surface, and the MLCC coated surface refers to the MLCC surface after coating the surfactant mixture.
[0081] As an embodiment of the present invention, the definition of the surfactant mixture for pre-treating the MLCC surface includes: analyzing the hydrophilic purpose of the MLCC surface; based on the hydrophilic purpose, constructing an ionic surfactant for pre-treating the MLCC surface, and defining a solubilizer type for the ionic surfactant; based on the solubilizer type, dissolving the ionic surfactant to obtain a mixed solution; and filtering the mixed solution to obtain the surfactant mixture.
[0082] Among them, the hydrophilic purpose refers to the intention of performing hydrophilic treatment on the surface of MLCC, the ionic surfactant refers to a surfactant whose molecules can dissociate in the solution to produce ions, such as anionic surfactants and cationic surfactants, the solvent type refers to the liquid type that can dissolve the surfactant, such as water and alcohol, and the mixed solution refers to the solution after the surfactant is fused with the solvent.
[0083] Furthermore, based on the hydrophilic purpose, the ionic surfactant for pre-treating the surface of the MLCC is constructed, including: based on the hydrophilic purpose, obtaining anionic surfactants and cationic surfactants for pre-treating the surface of the MLCC; defining the volume ratio of the anionic surfactant and the cationic surfactant; based on the volume ratio, dissolving the anionic surfactant and the cationic surfactant separately to obtain classified dissolution results; mixing the classified dissolution results to obtain the ionic surfactant for pre-treating the surface of the MLCC.
[0084] Among them, the anionic surfactant refers to a class of surfactants that can dissociate and form negatively charged ions in water or other polar solvents, such as sodium dodecyl sulfate (SDS) and sodium lauryl polyoxyethylene ether sulfate (AES); the cationic surfactant refers to a class of surfactants that can dissociate and form positively charged ions in water or other polar solvents, such as cetyltrimethylammonium bromide (CTAB) and quaternary ammonium salt softeners; the volume ratio refers to the component ratio of the anionic surfactant and the cationic surfactant; the classified dissolution result refers to the result of the anionic surfactant and the cationic surfactant being dissolved in the corresponding solvents respectively.
[0085] Optionally, the volume ratio of the anionic surfactant to the cationic surfactant may be defined by a volume ratio of 1:2, and based on the volume ratio, the anionic surfactant and the cationic surfactant are dissolved separately to obtain a classified dissolution result, which can be obtained through a dissolution experiment.
[0086] S2. Performing hydrophilic post-treatment on the hydrophilic surface of the MLCC to obtain the surface of the MLCC to be electroplated, constructing a pre-plating layer on the surface of the MLCC to be electroplated, and performing pre-plating post-treatment on the pre-plating layer to obtain the pre-plating layer on the surface of the MLCC.
[0087] The embodiment of the present invention performs a hydrophilic post-treatment on the hydrophilic surface of the MLCC to obtain the MLCC surface to be electroplated, constructs a pre-plated layer on the MLCC surface to be electroplated, and performs a pre-plating post-treatment on the pre-plated layer to obtain the MLCC surface pre-plated layer, which can provide an intermediate transition layer for nickel electroplating, increase the adhesion between the nickel layer and the ceramic substrate, thereby solving the problem that during the electroplating liquid injection process, the small-sized MLCC products are not completely hydrophilic after washing, and the small bubbles between the products float up and bring the products to the liquid surface. The MLCC surface to be electroplated refers to a pure MLCC surface waiting for electroplating, the pre-plated layer refers to a thin metal film deposited on the surface of the substrate before formal electroplating, and the MLCC surface pre-plated layer refers to the pre-plated layer after decontamination and drying treatment.
[0088] As an embodiment of the present invention, the hydrophilic surface of the MLCC is subjected to a hydrophilic post-treatment to obtain the MLCC surface to be electroplated, comprising: constructing a cleaning layer on the hydrophilic surface of the MLCC, oxidizing the cleaning layer to obtain an oxide layer; and based on the oxide layer, drying the MLCC workpiece to obtain the MLCC surface to be electroplated.
[0089] The cleaning layer refers to the surface layer of the MLCC after the contaminants on the surface of the MLCC workpiece are removed, and the oxide layer refers to the film formed on the surface of the MLCC workpiece after the MLCC workpiece is oxidized.
[0090] Optionally, the cleaning layer for constructing the hydrophilic surface of the MLCC can be obtained by a cleaning device, the oxidation treatment of the cleaning layer to obtain an oxide layer can be achieved by chemical oxidation, and the drying treatment of the MLCC workpiece based on the oxide layer to obtain the MLCC surface to be electroplated can be obtained by a drying device, such as an air dryer.
[0091] As another embodiment of the present invention, constructing a pre-plated layer on the surface of the MLCC to be electroplated includes: selecting a pre-plated metal on the surface of the MLCC to be electroplated, and analyzing the material properties of the pre-plated metal; based on the material properties, setting pre-plating parameters on the surface of the MLCC to be electroplated; based on the pre-plating parameters, placing the pre-plated metal into a preset electroplating tank for electroplating to obtain the pre-plated layer.
[0092] Among them, the pre-plated metal refers to a thin layer of metal deposited on the substrate before the main electroplating, the material properties refer to the inherent physical and chemical properties of the metal, the pre-plating parameters refer to a series of variable parameters controlled during the pre-plating process, and the preset electroplating tank refers to a device used to contain the electroplating solution and carry the workpiece to be plated.
[0093] Optionally, the selection of the pre-plated metal on the surface of the MLCC to be electroplated can be obtained by nickel or copper, the analysis of the material properties of the pre-plated metal can be achieved by physical measurement and chemical testing, and the post-pre-plating treatment of the pre-plated layer to obtain the pre-plated layer on the MLCC surface can be obtained by decontamination and drying.
[0094] S3, define the nickel plating solution of the MLCC surface pre-plating layer, and construct the electrolysis conditions of the nickel plating solution, based on the electrolysis conditions, electroplate the MLCC surface pre-plating layer to obtain the MLCC nickel plating layer
[0095] The embodiment of the present invention defines the nickel plating solution of the MLCC surface pre-plating layer, constructs the electrolysis conditions of the nickel plating solution, and electroplates the MLCC surface pre-plating layer based on the electrolysis conditions to obtain the MLCC nickel plating layer, which can improve the adhesion between the metal and the ceramic substrate and ensure that the MLCC product achieves the required heat resistance or weldability. Among them, the nickel plating solution refers to an electrolyte containing nickel ions and other auxiliary components, the electrolysis conditions refer to the electroplating equipment and electroplating parameter conditions for operating the electroplating of the MLCC workpiece, and the MLCC nickel plating layer refers to the nickel metal layer formed on the surface of the MLCC by electrochemical deposition technology.
[0096] Exemplarily, the nickel plating solution for pre-plating the surface of the MLCC comprises: weighing nickel sulfate by amount and pouring it into a clean beaker, adding one-third of the measured distilled water, and then weighing the required amount of sodium citrate into a clean beaker, usually 10%-20% of the amount of nickel sulfate, stirring vigorously until it is dissolved, adding acetic acid or ammonia water to adjust the pH value of the solution, usually the target pH value is between 4.0-5.5, weighing 5%-15% of the amount of nickel sulfate of sodium hypophosphite into a beaker, and stirring until completely dissolved, sodium hypophosphite is a reducing agent for nickel ions, which reduces nickel ions to nickel metal on the electrode, and then adding 1%-5% of the amount of nickel sulfate of polyethylene glycol to stabilize the plating solution, and continuously stirring the solution to ensure that all components are evenly distributed.
[0097] As an embodiment of the present invention, the electrolysis conditions of the nickel plating solution are constructed, including: obtaining the electroplating process requirements of the nickel plating solution, and setting the electroplating parameters of the nickel plating solution based on the electroplating process requirements; based on the electroplating parameters, setting the electrolysis device of the nickel plating solution, and determining the electrode positions of the electrolysis device, and determining the electrolysis conditions of the nickel plating solution according to the electrode positions.
[0098] Among them, the electroplating process requires a series of specifications and guidelines to ensure that the MLCC electroplating process is effective, efficient and reliable. The electroplating parameters refer to different parameters that control the electroplating process, such as electroplating time and electroplating current. The electrolysis device, also known as an electrolytic cell, is a device used to implement the electrolysis process. The electrode position refers to the position of the cathode and anode during the electrolysis process.
[0099] Optionally, the electroplating parameters of the nickel plating solution are set based on the electroplating process requirements, which can be obtained by using parameter measurement tools, such as an electroplating parameter tester and a coating thickness measuring instrument. The electrode positions of the electrolytic device are determined by the charged properties of the electroplating material.
[0100] As another embodiment of the present invention, the MLCC surface pre-plating layer is electroplated based on the electrolysis conditions to obtain an MLCC nickel-plated layer, including: setting the power supply conditions of the MLCC surface pre-plating layer based on the electrolysis conditions; setting the electrode properties of the surface pre-plating layer and the preset nickel plating solution under the power supply conditions; and performing electroplating on the surface pre-plating layer and the preset nickel plating solution based on the electrode properties to obtain the MLCC nickel-plated layer.
[0101] The power supply condition refers to the condition of a power supply device that can provide low voltage and high current, and the electrode properties refer to the cathode properties of the surface pre-plating layer and the anode properties represented by the preset nickel plating solution.
[0102] Optionally, the power supply conditions for the MLCC surface pre-plating layer are set based on the electrolysis conditions, which can be obtained through a precision electroplating power supply; the electrode properties of the surface pre-plating layer and the preset nickel plating solution are set under the power supply conditions, which can be achieved using historical experimental data; the electroplating treatment of the surface pre-plating layer and the preset nickel plating solution is performed based on the electrode properties to obtain the MLCC nickel-plated layer, which can be obtained through an electroplating tank.
[0103] S4, detecting the coating performance of the MLCC nickel-plated layer, and when the coating performance is greater than the preset performance, performing nickel-plating post-treatment on the MLCC nickel-plated layer to obtain the MLCC target nickel-plated surface
[0104] The embodiment of the present invention detects the plating performance of the MLCC nickel plating layer. When the plating performance is greater than the preset performance, the MLCC nickel plating layer is subjected to nickel plating post-treatment to obtain the MLCC target nickel plating surface. The contamination factor of the MLCC nickel plating layer can be removed, and the adsorption force between the MLCC nickel plating layer and other metal layers can be improved, thereby further ensuring that the MLCC product can achieve the required heat resistance or weldability. The plating performance refers to the characteristics of the metal or alloy layer formed on the surface of the MLCC workpiece by electroplating processing technology.
[0105] Optionally, the detecting the plating performance of the MLCC nickel plating layer includes:
[0106] The deposition rate of the nickel plating solution in the MLCC nickel plating layer is calculated using the following formula:
[0107]
[0108] Wherein, V represents the deposition rate, M1 represents the weight of the sample of the nickel electroplating solution in the MLCC nickel-plated layer before nickel plating, M2 represents the weight of the sample of the nickel electroplating solution in the MLCC nickel-plated layer after nickel plating, and t represents the electroplating time of the nickel electroplating solution in the nickel-plated layer;
[0109] The current efficiency of the nickel plating solution in the MLCC nickel plating layer is calculated using the following formula:
[0110]
[0111] Among them, S k represents the current efficiency, m represents the weight gain of the nickel electroplating solution in the nickel plating sample in the MLCC nickel plating layer, I represents the nickel plating current of the nickel electroplating solution in the MLCC nickel plating layer, and k represents the electrochemical equivalent of the nickel electroplating solution in the MLCC nickel plating layer;
[0112] The dispersion of the nickel plating solution in the MLCC nickel plating layer is calculated using the following formula:
[0113]
[0114] Where, T represents the dispersion, S represents the distance ratio between the cathode and the anode of the nickel plating solution in the MLCC nickel plating layer, and M represents the 近 Indicates the weight gain of the nickel plating solution near the cathode in the nickel plating layer of MLCC, M 远 It indicates the weight gain of the nickel plating solution far from the cathode in the nickel plating layer of MLCC;
[0115] The plating performance of the MLCC nickel plating layer is determined according to the deposition speed, the current efficiency and the dispersion.
[0116] It should be noted that in the present application, the preset performance can be divided into four levels: excellent, good, average and poor, that is, when the plating performance of the MLCC nickel plating layer is good or excellent, it means that the plating performance is greater than the preset performance.
[0117] As another embodiment of the present invention, the MLCC nickel-plated layer is subjected to nickel-plating post-treatment to obtain a target MLCC nickel-plated surface, comprising: when the coating performance is greater than a preset performance, removing the chemical reaction factor of the clean MLCC nickel-plated layer to obtain a pure MLCC nickel-plated layer; and drying the pure MLCC nickel-plated layer to obtain a target MLCC nickel-plated surface.
[0118] The chemical reaction factor refers to a pollution factor that can chemically react on the target nickel-plated surface of the MLCC, and the pure MLCC nickel-plated layer refers to the MLCC surface from which irrelevant pollutants have been removed.
[0119] Optionally, when the coating performance is greater than a preset performance, the chemical reaction factors of the clean MLCC nickel-plated layer are removed to obtain a pure MLCC nickel-plated layer, which can be obtained by acid washing followed by water washing.
[0120] S5. Activate the target nickel-plated surface of the MLCC to obtain an active MLCC nickel-plated surface, construct an MLCC electroplated tin layer of the active MLCC nickel-plated surface, analyze the surface attachment elements of the MLCC electroplated tin layer, and optimize the surface attachment elements to obtain the target MLCC electroplated layer.
[0121] The embodiment of the present invention can improve the welding performance of the MLCC workpiece by activating the target nickel-plated surface of the MLCC to obtain an active MLCC nickel-plated surface, and constructing an MLCC electroplated tin layer on the active MLCC nickel-plated surface. The active MLCC nickel-plated surface refers to an active nickel layer formed by treating the MLCC nickel-plated surface with an activator, and the MLCC electroplated tin layer refers to a tin layer deposited on the surface of the MLCC workpiece by an electrochemical method.
[0122] Optionally, the target nickel-plated surface of the MLCC is activated to obtain an active MLCC nickel-plated surface, which can be achieved by using an activator, such as nickel sulfate.
[0123] Furthermore, the construction of the MLCC electroplated tin layer on the active MLCC nickel-plated surface includes: preparing a tin-plating solution for the active MLCC nickel-plated surface, and defining an electroplating equipment for the tin-plating solution; based on the electroplating equipment, determining an electroplating electrode for the active MLCC nickel-plated surface; constructing electroplating parameters for the electroplating electrode, and adjusting a variation factor of the electroplating parameters in real time; based on the variation factor, performing a tin-plating treatment on the active MLCC nickel-plated surface to obtain the MLCC electroplated tin layer.
[0124] Among them, the tin plating solution refers to an electroplating solution containing tin salts and other necessary additives, the electroplating equipment refers to equipment for electroplating the MLCC workpiece, such as an electrolytic cell, the electroplating parameters refer to electroplating indexes that affect the quality of the coating, such as current and time, and the variation factor refers to the factor that changes the electroplating parameters with the quality of the coating.
[0125] Exemplarily, the preparation of the tin plating solution for the nickel-plated surface of the active MLCC includes: weighing the tin sulfate of the nickel-plated surface of the active MLCC into a clean beaker, adding one-third of the measured distilled water, weighing the required amount of sulfonic acid into a clean beaker, adding one-third of boiling water and stirring vigorously until it is dissolved, slowly adding the solution dissolved with sulfonic acid to the tin salt solution, weighing a trace amount of tin sulfate with an electronic balance and pouring it into a beaker, adding a trace amount of water to make it into a paste, and then adding an appropriate amount of boiling water or boiling the solution for a period of time to completely dissolve it, adding an aqueous solution of sodium dodecyl sulfate to the nickel salt solution, and then weighing the required amount of additives in turn, dissolving them with water and then pouring them into the tin salt solution, washing the beaker where the drugs have been dissolved, because some reagents are added in very small amounts, it is necessary to pour the rinsed solution back into the tin salt solution to prevent the reliability of the test data from being affected by the loss of drugs, and after these processes are completed, stirring with a glass rod until each reagent is completely dissolved, and finally adding water to the required content.
[0126] Optionally, the electroplating electrode of the active MLCC nickel-plated surface is determined based on the electroplating equipment, which can be achieved by utilizing the basic principle of electroplating, and the tin plating treatment of the active MLCC nickel-plated surface is performed based on the variation factor to obtain the MLCC electroplated tin layer, which can be obtained through an electrolytic cell.
[0127] Furthermore, the embodiment of the present invention analyzes the surface attachment elements of the MLCC electroplated tin layer and optimizes the surface attachment elements to obtain the MLCC target electroplated layer, which can optimize the performance and appearance of the plating layer, so that the MLCC product can achieve the required heat resistance or solderability, thereby solving the problem of electroplating leakage of MLCC products. The surface attachment elements refer to the contaminant elements remaining on the surface of the MLCC workpiece after tin electroplating, and the MLCC target electroplated layer refers to the expected MLCC electroplated surface achieved by electroplating.
[0128] As an embodiment of the present invention, the analysis of the surface attachment elements of the MLCC electroplated tin layer includes: querying the surface factors of the MLCC electroplated tin layer, and chemically treating the surface factors to obtain chemical reaction results; based on the chemical reaction results, evaluating the degree of influence of the surface attachment elements on the MLCC electroplated tin layer, and determining the surface attachment elements of the MLCC electroplated tin layer according to the degree of influence.
[0129] Among them, the surface factor refers to the residual factor on the surface of the MLCC workpiece after tin electroplating, the chemical reaction result refers to the result obtained after chemical analysis of the surface factor, and the degree of influence refers to the degree of influence of the surface factor on the performance of the MLCC point tin plating layer.
[0130] Optionally, the querying of the surface factor of the MLCC electroplated tin layer can be obtained by means of a scanning electron microscope, the chemical treatment of the surface factor to obtain a chemical reaction result can be obtained by means of volatility analysis, and the evaluation of the influence of the surface-attached elements on the MLCC electroplated tin layer based on the chemical reaction result can be achieved by means of laboratory testing.
[0131] Furthermore, the surface-attached elements are optimized to obtain a target MLCC electroplating layer, including: post-water washing treatment of the surface-attached elements to obtain a clean surface; based on the clean surface, passivation treatment of the MLCC electroplated tin layer to obtain a passivated surface; and liquid removal treatment of the passivated surface to obtain a target MLCC electroplating layer.
[0132] Among them, the clean surface refers to the tin-plated surface of the MLCC after the elements attached to the surface are removed, and the passivated surface refers to the conversion film formed on the surface of the tin-plated layer of the MLCC to improve the corrosion resistance of the metal.
[0133] Optionally, the post-water washing treatment of the surface-attached elements to obtain a clean surface can be achieved using high-frequency vibration cleaning equipment, the passivation treatment of the MLCC electroplated tin layer based on the clean surface to obtain a passivated surface can be obtained by electrochemical passivation, and the liquid removal treatment of the passivated surface to obtain the MLCC target electroplated layer can be achieved using radiation drying.
[0134] The present invention first obtains an MLCC workpiece and analyzes the conductive path of the MLCC workpiece to clarify the electrode structure of the MLCC workpiece, provides a conductive path for MLCC electroplating, and pre-treats the MLCC cut surface to obtain a pre-treated MLCC surface, thereby removing MLCC surface pollutants and improving surface adsorption. The pre-treated MLCC surface is hydrophilically treated to obtain a hydrophilic MLCC surface, thereby enhancing the adhesion of the MLCC surface. Secondly, the present invention performs a hydrophilic post-treatment on the MLCC hydrophilic surface to obtain an MLCC surface to be electroplated, constructs a pre-plating layer on the MLCC surface to be electroplated, and performs a pre-plating post-treatment on the pre-plating layer to obtain an MLCC surface pre-plating layer, thereby providing an intermediate transition layer for nickel electroplating and increasing the adhesion between the nickel layer and the ceramic substrate, thereby solving the problem that during the electroplating liquid injection process, the small-sized MLCC products are not completely hydrophilic after washing, and the small bubbles between the products float up and bring the products to the liquid surface. Furthermore, the present invention defines a nickel plating solution for the MLCC surface pre-plating layer and constructs the electrolysis conditions of the nickel plating solution. Based on the electrolysis conditions, the MLCC surface pre-plating layer is electroplated to obtain an MLCC nickel-plated layer, which can improve the adhesion between the metal and the ceramic substrate, and ensure that the MLCC product can achieve the required heat resistance or weldability. By detecting the plating performance of the MLCC nickel-plated layer, when the plating performance is greater than the preset performance, the MLCC nickel-plated layer is post-processed with nickel plating to obtain an MLCC target nickel-plated surface, which can remove the contamination factor of the MLCC nickel-plated layer, improve the adsorption force between the MLCC nickel-plated layer and other metal layers, and further ensure that the MLCC product can achieve the required heat resistance or weldability. Finally, the embodiment of the present invention activates the MLCC target nickel-plated surface to obtain an active MLCC nickel-plated surface, and constructs an MLCC electroplated tin layer of the active MLCC nickel-plated surface, which can improve the welding performance of the MLCC workpiece. By analyzing the surface attachment elements of the MLCC electroplated tin layer and optimizing the surface attachment elements, the MLCC target electroplated layer is obtained, which can optimize the performance and appearance of the plating and ensure that the MLCC product can achieve the required heat resistance or weldability. Therefore, the method for solving the problem of electroplating omission in small-size MLCCs provided in an embodiment of the present invention can ensure that the MLCC products achieve the required heat resistance or solderability, thereby solving the problem of electroplating omission in MLCC products.
[0135] like Figure 2 1 is a functional module diagram of a system for solving the problem of electroplating leakage in small-sized MLCCs, provided by one embodiment of the present invention.
[0136] The system 100 for solving the problem of electroplating leakage of small-sized MLCCs described in the present invention can be installed in an electronic device. According to the functions implemented, the system 100 for solving the problem of electroplating leakage of small-sized MLCCs can include a hydrophilic treatment module 101, a workpiece pre-plating module 102, an electroplating treatment module 103, a nickel plating treatment module 104, and an electroplating optimization module 105. The module described in the present invention can also be referred to as a unit, which refers to a series of computer program segments that can be executed by an electronic device processor and can complete fixed functions, which are stored in the memory of the electronic device.
[0137] In this embodiment, the functions of each module / unit are as follows:
[0138] The hydrophilic treatment module 101 is used to obtain an MLCC workpiece, analyze the conductive path of the MLCC workpiece, cut the MLCC workpiece based on the conductive path to obtain an MLCC cut surface, pre-treat the MLCC cut surface to obtain a pre-treated MLCC surface, and perform a hydrophilic treatment on the pre-treated MLCC surface to obtain an MLCC hydrophilic surface;
[0139] The workpiece pre-plating module 102 is used to perform a hydrophilic post-treatment on the hydrophilic surface of the MLCC to obtain a surface of the MLCC to be electroplated, construct a pre-plating layer on the surface of the MLCC to be electroplated, and perform a pre-plating post-treatment on the pre-plating layer to obtain a pre-plating layer on the surface of the MLCC;
[0140] The electroplating treatment module 103 is used to define the nickel plating solution of the MLCC surface pre-plating layer and construct the electrolysis conditions of the nickel plating solution, and based on the electrolysis conditions, electroplating the MLCC surface pre-plating layer to obtain the MLCC nickel plating layer;
[0141] The nickel plating processing module 104 is used to detect the plating performance of the MLCC nickel plating layer, and when the plating performance is greater than a preset performance, the MLCC nickel plating layer is subjected to nickel plating post-processing to obtain a target nickel plating surface of the MLCC;
[0142] The electroplating optimization module 105 is used to activate the target nickel-plated surface of the MLCC to obtain an active MLCC nickel-plated surface, and to construct an MLCC electroplated tin layer of the active MLCC nickel-plated surface, analyze the surface attachment elements of the MLCC electroplated tin layer, and optimize the surface attachment elements to obtain the target MLCC electroplated layer.
[0143] In detail, each module described in the system 100 for solving the problem of MLCC small-size electroplating leakage in the embodiment of the present application is used in the same manner as described above. Figure 1The same technical means as described in the method for solving the problem of electroplating leakage in small-size MLCC can produce the same technical effect, so I will not go into details here.
[0144] In the several embodiments provided by the present invention, it should be understood that the provided methods and systems can be implemented in other ways. For example, the method embodiments described above are only illustrative, for example, the division of the modules is only a logical function division, and there may be other division methods in actual implementation.
[0145] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for solving the problem of electroplating leakage in small-size MLCC, characterized in that: The method comprises: Obtaining an MLCC workpiece, analyzing a conductive path of the MLCC workpiece, cutting the MLCC workpiece based on the conductive path to obtain an MLCC cut surface, pre-treating the MLCC cut surface to obtain a pre-treated MLCC surface, and performing a hydrophilic treatment on the pre-treated MLCC surface to obtain an MLCC hydrophilic surface; Performing a hydrophilic post-treatment on the hydrophilic surface of the MLCC to obtain a surface of the MLCC to be electroplated, constructing a pre-plating layer on the surface of the MLCC to be electroplated, and performing a pre-plating post-treatment on the pre-plating layer to obtain a pre-plating layer on the surface of the MLCC; Defining a nickel plating solution for the MLCC surface pre-plating layer, and constructing electrolysis conditions for the nickel plating solution, and electroplating the MLCC surface pre-plating layer based on the electrolysis conditions to obtain an MLCC nickel plating layer; Detecting the plating performance of the MLCC nickel-plated layer, and when the plating performance is greater than a preset performance, performing nickel-plating post-treatment on the MLCC nickel-plated layer to obtain a target nickel-plated surface of the MLCC; The target nickel-plated surface of the MLCC is activated to obtain an active MLCC nickel-plated surface, and an MLCC electroplated tin layer of the active MLCC nickel-plated surface is constructed. The surface attachment elements of the MLCC electroplated tin layer are analyzed, and the surface attachment elements are optimized to obtain the target MLCC electroplated layer.
2. A method for solving the problem of electroplating leakage in small-size MLCC as claimed in claim 1, characterized in that: The pre-processing of the MLCC cut surface to obtain a pre-processed MLCC surface includes: Obtaining a non-destructive surface of the cut surface of the MLCC, and cleaning the non-destructive surface to obtain a pure MLCC surface; The pure MLCC surface is dried to obtain a dry MLCC surface; the dry MLCC surface is activated to obtain a pre-treated MLCC surface.
3. A method for solving the problem of electroplating leakage in small-size MLCC as claimed in claim 2, characterized in that: The step of activating the dried MLCC surface to obtain a pre-treated MLCC surface comprises: Obtaining a plasma treatment device for drying the surface of the MLCC; constructing a plasma on the surface of the dried MLCC based on the plasma treatment device; The plasma is used to perform surface modification treatment on the surface of the dried MLCC to obtain a pretreated MLCC surface.
4. A method for solving the problem of electroplating leakage in small-size MLCC as claimed in claim 3, characterized in that: The step of performing a hydrophilic treatment on the pretreated MLCC surface to obtain a hydrophilic MLCC surface comprises: Preparing a hydrophilic agent for pretreating the surface of the MLCC; Coating the hydrophilic agent on the surface of the pretreated MLCC to obtain a hydrophilic coating surface; The hydrophilic coating surface is subjected to post-coating treatment to obtain a hydrophilic MLCC surface.
5. A method for solving the problem of electroplating leakage in small-size MLCC as claimed in claim 1, characterized in that: The surfactant mixture defining the pre-treatment of the MLCC surface comprises: Analyze the hydrophilicity of the MLCC surface; Based on the hydrophilic purpose, construct the ionic surfactant for pre-treating the MLCC surface, and define the type of solubilizer for the ionic surfactant; Based on the type of the solvent, dissolving the ionic surfactant to obtain a mixed solution; The mixed solution is filtered to obtain the surfactant mixture.
6. A method for solving the problem of electroplating leakage in small-size MLCC as claimed in claim 1, characterized in that: The step of performing a hydrophilic post-treatment on the hydrophilic surface of the MLCC to obtain the surface of the MLCC to be electroplated comprises: constructing a cleaning layer on the hydrophilic surface of the MLCC, and performing oxidation treatment on the cleaning layer to obtain an oxidation layer; Based on the oxide layer, the MLCC workpiece is dried to obtain the MLCC surface to be electroplated.
7. A method for solving the problem of electroplating leakage in small-size MLCC as claimed in claim 1, characterized in that: The step of constructing a pre-plating layer on the surface of the MLCC to be electroplated comprises: Selecting a pre-plated metal on the surface of the MLCC to be electroplated, and analyzing the material properties of the pre-plated metal; Based on the material properties, setting pre-plating parameters of the surface of the MLCC to be electroplated; Based on the pre-plating parameters, the pre-plated metal is placed in a preset electroplating tank for electroplating to obtain the pre-plated layer.
8. A method for solving the problem of electroplating leakage in small-size MLCC as claimed in claim 1, characterized in that: Based on the electrolysis conditions, the pre-plated layer on the surface of the MLCC is electroplated to obtain a nickel-plated layer of the MLCC, comprising: Based on the electrolysis conditions, setting the power supply conditions of the MLCC surface pre-plating layer; Under the power supply condition, setting the electrode properties of the surface pre-plating layer and the preset nickel plating solution; Based on the electrode properties, the surface pre-plating layer and the preset nickel plating solution are electroplated to obtain an MLCC nickel plating layer.
9. A method for solving the problem of electroplating leakage in small-size MLCC as claimed in claim 1, characterized in that: The detecting the plating performance of the MLCC nickel plating layer comprises: The deposition rate of the nickel plating solution in the MLCC nickel plating layer is calculated using the following formula: Wherein, V represents the deposition rate, M1 represents the weight of the sample of the nickel electroplating solution in the MLCC nickel-plated layer before nickel plating, M2 represents the weight of the sample of the nickel electroplating solution in the MLCC nickel-plated layer after nickel plating, and t represents the electroplating time of the nickel electroplating solution in the nickel-plated layer; The current efficiency of the nickel plating solution in the MLCC nickel plating layer is calculated using the following formula: Among them, S k represents the current efficiency, m represents the weight gain of the nickel electroplating solution in the nickel plating sample in the MLCC nickel plating layer, I represents the nickel plating current of the nickel electroplating solution in the MLCC nickel plating layer, and k represents the electrochemical equivalent of the nickel electroplating solution in the MLCC nickel plating layer; The dispersion of the nickel plating solution in the MLCC nickel plating layer is calculated using the following formula: Where, T represents the dispersion, S represents the distance ratio between the cathode and the anode of the nickel plating solution in the MLCC nickel plating layer, and M represents the 近 Indicates the weight gain of the nickel plating solution near the cathode in the nickel plating layer of MLCC, M 远 It indicates the weight gain of the nickel plating solution far from the cathode in the nickel plating layer of MLCC; The plating performance of the MLCC nickel plating layer is determined according to the deposition speed, the current efficiency and the dispersion.
10. A system for solving the problem of electroplating leakage in small-size MLCC, characterized in that: The system comprises: A hydrophilic treatment module is used to obtain an MLCC workpiece, analyze a conductive path of the MLCC workpiece, cut the MLCC workpiece based on the conductive path to obtain an MLCC cut surface, pre-treat the MLCC cut surface to obtain a pre-treated MLCC surface, and perform a hydrophilic treatment on the pre-treated MLCC surface to obtain an MLCC hydrophilic surface; A workpiece pre-plating module is used to perform a hydrophilic post-treatment on the hydrophilic surface of the MLCC to obtain a surface of the MLCC to be electroplated, construct a pre-plating layer on the surface of the MLCC to be electroplated, and perform a pre-plating post-treatment on the pre-plating layer to obtain a pre-plating layer on the surface of the MLCC; An electroplating treatment module, used to define a nickel plating solution for the MLCC surface pre-plating layer, and to construct an electrolysis condition for the nickel plating solution, and to electroplating the MLCC surface pre-plating layer based on the electrolysis condition to obtain an MLCC nickel plating layer; A nickel plating treatment module, used for detecting the plating performance of the MLCC nickel plating layer, and when the plating performance is greater than a preset performance, performing nickel plating post-treatment on the MLCC nickel plating layer to obtain a target nickel plating surface of the MLCC; The electroplating optimization module is used to activate the target nickel-plated surface of the MLCC to obtain an active MLCC nickel-plated surface, and to construct an MLCC electroplated tin layer of the active MLCC nickel-plated surface, analyze the surface attachment elements of the MLCC electroplated tin layer, and optimize the surface attachment elements to obtain the target MLCC electroplated layer.
Citation Information
Patent Citations
Nickel electroplating method of ceramic metalized layer
CN102392279A
Tubular ceramic dielectric capacitor electrode manufacturing method based on chemical nickel plating and tin electroplating
CN111441041A
Metallization process of zirconia ceramic
CN112341250A
Aluminum alloy tin plating electroplating process
CN112853413A
Method for treating ultra-miniature and high-capacity MLCC before electroplating
CN115679400A