Preparation method, product and application of polydentate organic ligand and transition metal coordination polymer thereof

By introducing triphenylamine groups and benzotriazole structures into organic ligands, the coordination of multi-dentate organic ligands with metal ions is solved, and the problem of poor solubility of transition metal coordination polymers is achieved, and high solubility and Excellent electrochromic properties improve the stability and response speed of the material.

CN118978510AActive Publication Date: 2024-11-19JILIN UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411039851.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The existing transition metal coordination polymers have poor solubility, which affects their processing operations and electrochromic properties.

Method used

By introducing triphenylamine groups and benzotriazole structures, the helical flexibility and electron acceptor properties of the organic ligand are improved, and the coordination between multi-dentate organic ligands and metal ions is synthesized to prepare high solubility and excellent electrochromicity. Performance of transition metal coordination polymer.

Benefits of technology

The solubility and electrochromic properties of transition metal coordination polymers are improved, stable electroactivity, low starting voltage and fast color conversion are achieved, and the cyclic stability of electrochromic materials is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978510A_ABST
    Figure CN118978510A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of functional molecular materials, in particular to a polydentate organic ligand, a preparation method of a transition metal coordination polymer of the polydentate organic ligand, a product and application. The structural formula of the polydentate organic ligand is as shown in formula I; the transition metal coordination polymer is obtained through a complex reaction of a polydentate organic ligand and a metal salt in the # imgabs0 #. The invention provides a polydentate (tridentate) organic ligand containing a triphenylamine-pyridine-benzotriazole structure, and a novel transition metal coordination polymer containing the triphenylamine-pyridine-benzotriazole structure is synthesized by using the polydentate organic ligand. The electron donating group is introduced to the benzene ring para-position of triphenylamine, so that the redox potential can be effectively reduced, and the solubility of the organic ligand is further improved. Compared with monodentate and bidentate ligands in the prior art, the tridentate ligand prepared by the preparation method disclosed by the invention has the advantages that the combination with metal is firmer, the stability of the complex is higher, and the corresponding electrochromic cycle stability is more excellent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of functional molecular materials, and in particular to a preparation method, product and application of a multidentate organic ligand and a transition metal coordination polymer thereof. Background Art

[0002] As a branch of metal supramolecular polymers, transition metal coordination polymers have the advantages of both inorganic and organic materials. It is easy to control the photoelectric properties of materials by molecular tailoring of ligands, changes in metal ions and coordination modes. At the same time, coordination polymers based on variable valence transition metals have good redox properties and rich electronic transition behaviors. They are a type of electrochromic material with excellent performance, high optical contrast, fast response time, multiple color changes, etc.

[0003] Pyridine, polypyridine and other nitrogen-containing heterocyclic molecules contain lone pairs of electrons on the N in the structure, which are easy to coordinate with metal ions and contain large π electron conjugated structures. The complexes formed usually have strong electrochromic properties. In particular, when transition metal ions form an alternating structure with organic molecules containing polypyridine and multiple nitrogen-containing heterocyclic structures, polyorganometallic complexes with polymer-like structures can be obtained, thereby showing more outstanding electrochromic properties. However, this type of structure containing multiple heterocyclic rings often has poor solubility, which is not conducive to further processing operations.

[0004] Therefore, how to improve the solubility of transition metal coordination polymers while ensuring electrochromic performance is a technical problem that urgently needs to be solved in the field of functional molecular materials technology. Summary of the invention

[0005] Based on the above content, the present invention provides a preparation method, product and application of a multidentate organic ligand and a transition metal coordination polymer thereof.

[0006] To achieve the above object, the present invention provides the following solutions:

[0007] One of the technical solutions of the present invention is a multidentate organic ligand, the structural formula of which is shown in Formula I;

[0008]

[0009] In Formula I, R is one of the following structural formulas:

[0010]

[0011] A second technical solution of the present invention is a method for preparing the above-mentioned multidentate organic ligand, comprising the following steps:

[0012] Bis(4-bromophenyl)amine and iodide undergo Ullmann reaction to prepare dibromo-containing diphenylamine substituted compounds;

[0013] The dibromo-containing diphenylamine substituted compound is subjected to a Suzuki reaction with bis(pinacol)diboron to obtain a 4,4'-diboric acid pinesyl ester triphenylamine compound;

[0014] The 4,4'-diboronic acid pinesyl ester triphenylamine compound and 2,6-dibromo-4-iodopyridine undergo a Suzuki reaction to obtain a 2,6-dibromopyridine-substituted triphenylamine compound;

[0015] The triphenylamine compound substituted by 2,6-dibromopyridine and benzotriazole undergo Ullmann reaction to obtain the multidentate organic ligand.

[0016] The structural formula of the dibromo-containing diphenylamine substituted compound is

[0017] The structural formula of the 4,4'-diboric acid pinesyl ester triphenylamine compound is

[0018]

[0019] The structural formula of the triphenylamine compound substituted with 2,6-dibromopyridine is

[0020]

[0021] The R in the structural formula of the dibromo-containing diphenylamine substituted compound, 4,4'-diboric acid pinesol ester triphenylamine compound, and 2,6-dibromopyridine substituted triphenylamine compound is independently one of the following structural formulas:

[0022]

[0023] In some embodiments of the present invention, the molar ratio of the bis(4-bromophenyl)amine to the iodide is 1:(1-3);

[0024] The molar ratio of the dibromo-containing diphenylamine substituted compound to the bis(pinacol)diboron is 1:(1.5-4);

[0025] The molar ratio of the 4,4'-diboronic acid pinesyl ester triphenylamine compound to the 2,6-dibromo-4-iodopyridine is 1:(1.5-4);

[0026] The molar ratio of the triphenylamine compound substituted by 2,6-dibromopyridine to the benzotriazole is 1:(3-7).

[0027] In some embodiments of the present invention, the iodide is 4-iodotoluene, 4-iodoanisole, 9-iodophenanthrene, iodobenzene, 4-iodoisopropylbenzene, 4-iodobiphenyl, 4-iodocyanobenzene, 1-iodo-4-(1-methylpropyl)benzene, 1-iodonaphthalene or 4-iodo-tert-butylbenzene.

[0028] The third technical solution of the present invention is the use of the above-mentioned multidentate organic ligand in the preparation of transition metal coordination polymers or electrochromic materials.

[0029] A fourth technical solution of the present invention is a method for preparing a transition metal coordination polymer, comprising the following steps:

[0030] The multidentate organic ligand is subjected to a complexation reaction with a metal salt to obtain the transition metal coordination polymer.

[0031] In some embodiments of the present invention, the molar ratio of the multidentate organic ligand to the metal salt is (2-3):1; the metal salt is an iron salt, a cobalt salt, a nickel salt or a zinc salt; the temperature of the complex reaction is 60-100°C and the time is 10h-20h.

[0032] A fifth technical solution of the present invention is a transition metal coordination polymer prepared by the above-mentioned method for preparing a transition metal coordination polymer.

[0033] The sixth technical solution of the present invention is the use of the above-mentioned transition metal coordination polymer in the preparation of electrochromic materials.

[0034] The seventh technical solution of the present invention is an electrochromic material, the raw materials of which include the above-mentioned multidentate organic ligand or transition metal coordination polymer.

[0035] The present invention discloses the following technical effects:

[0036] The invention provides a multidentate (tridentate) organic ligand containing a "triphenylamine-pyridine-benzotriazole" structure, and utilizes the multidentate organic ligand to synthesize a novel transition metal coordination polymer containing a "triphenylamine-pyridine-benzotriazole" structure.

[0037] The invention introduces an electron-donating group at the para position of the benzene ring of triphenylamine, which can not only effectively reduce the redox potential but also further improve the solubility of the organic ligand.

[0038] Compared with the monodentate and bidentate ligands in the prior art, the tridentate ligand prepared by the present invention has a stronger bond with the metal, a higher stability of the complex, and a better corresponding electrochromic cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0040] Figure 1 This is the hydrogen nuclear magnetic spectrum of the multidentate organic ligand prepared in Example 1 of the present invention.

[0041] Figure 2 This is the hydrogen nuclear magnetic spectrum of the multidentate organic ligand prepared in Example 4 of the present invention.

[0042] Figure 3 This is the X-ray photoelectron spectrum of the transition metal coordination polymer prepared in Example 11 of the present invention.

[0043] Figure 4 This is the electrochromatogram of the transition metal coordination polymer film (film 1) prepared in Example 11 of the present invention.

[0044] Figure 5 This is the cyclic voltammogram of the transition metal coordination polymer film (film 1) prepared in Example 11 of the present invention.

[0045] Figure 6 This is the electrochromic response time spectrum of the transition metal coordination polymer film (film 1) prepared in Example 11 of the present invention.

[0046] Figure 7 This is the hydrogen nuclear magnetic spectrum of the multidentate organic ligand prepared in Example 8 of the present invention. DETAILED DESCRIPTION

[0047] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0048] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0049] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0050] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0051] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0052] In order to overcome the problem of poor solubility of transition metal coordination polymers, the present invention introduces triphenylamine groups, which also have excellent electrochromic properties, into the organic ligand framework to improve the solubility of transition metal coordination polymers with its unique helical flexible structure. At the same time, the excellent electron acceptor benzotriazole introduced into the multidentate ligand also further improves the solubility of the material.

[0053] The present invention aims to synthesize a type of multidentate ligand based on the "triphenylamine-pyridine-benzotriazole" structure, and synthesize a series of transition metal coordination polymers by coordination with metal ions. The transition metal coordination polymer prepared by the present invention has stable electroactivity, low starting voltage, fast color conversion speed and excellent electrochromic performance.

[0054] The first aspect of the present invention provides a multidentate organic ligand, the structural formula of which is shown in Formula I;

[0055]

[0056] In Formula I, R is one of the following structural formulas:

[0057]

[0058] The second aspect of the present invention provides a method for preparing the above-mentioned multidentate organic ligand, comprising the following steps:

[0059] Bis(4-bromophenyl)amine and iodide undergo Ullmann reaction to prepare dibromo-containing diphenylamine substituted compounds;

[0060] The dibromo-containing diphenylamine substituted compound is subjected to a Suzuki reaction with bis(pinacol)diboron to obtain a 4,4'-diboric acid pinesyl ester triphenylamine compound;

[0061] The 4,4'-diboronic acid pinesyl ester triphenylamine compound and 2,6-dibromo-4-iodopyridine undergo a Suzuki reaction to obtain a 2,6-dibromopyridine-substituted triphenylamine compound;

[0062] The triphenylamine compound substituted by 2,6-dibromopyridine and benzotriazole undergo Ullmann reaction to obtain the multidentate organic ligand.

[0063] In some embodiments of the present invention, the method for preparing the multidentate organic ligand comprises the following steps:

[0064] (1) Ullmann reaction

[0065] Add bis(4-bromophenyl)amine: iodide: cuprous iodide: o-phenanthroline: potassium hydroxide in a molar ratio of 1:(1-3):(0.04-0.06):(0.04-0.06):(6-10) to the Schlenk flask. Then use a double row of tubes to apply three vacuum-nitrogen cycles to the reaction system. After the solid reactant is fully soaked in the nitrogen atmosphere, add the solvent anhydrous toluene (5 ml solvent / mmol diamine monomer) with a syringe, and apply three vacuum-nitrogen cycles to the system again. Allow the system to react in a nitrogen atmosphere at 100-130°C for 10-40 hours. After the reaction is completed, filter out the catalyst, wash the product attached to the catalyst with dichloromethane (3*10 ml), collect the filtrate, add deionized water (V 二氯甲烷 :V 去离子水 =2:2~1) to extract the obtained product several times. Combine the organic phases and dry them with anhydrous sodium sulfate. Filter by suction and remove the organic solvent in the filtrate by vacuum distillation. Use dichloromethane / petroleum ether as eluent (V 二氯甲烷 :V 石油醚 =2~10:1), and purify the crude product by silica gel column chromatography to obtain N-aryl-4,4'-dibromodiphenylamine (dibromo-containing diphenylamine substituted compound).

[0066] The reaction route is as follows:

[0067]

[0068] (2) Suzuki reaction

[0069] N-aryl-4,4'-dibromodiphenylamine substituted compound, bis(pinacolato)diboron, potassium acetate and [1,1'-bis(diphenylphosphino)ferrocene]dichloropalladium (catalyst) were added to a Schlenk flask in a molar ratio of 1:(1.5-4):(5-8):(0.04-0.06). After applying three cycles of vacuum-nitrogen cycle to the system, 1,4-dioxane was added as a solvent (10ml 1,4-dioxane / mmol 4,4'-dibromotriphenylamine compound) using a syringe, and then three cycles of nitrogen-vacuum cycle were applied. The reaction was carried out at 80-110°C under a nitrogen atmosphere for 10-40h. After the reaction was completed, the catalyst was filtered off, the filtrate was collected, and dichloromethane and deionized water (V dichloromethane: V deionized water = 2:2-1) were added to extract the obtained product multiple times. The organic phases were combined and dried with anhydrous sodium sulfate. The mixture was filtered and the solvent was removed by rotary evaporation to obtain 4,4'-diboronic acid pinesyl ester triphenylamine compound (boric acid ester).

[0070] The reaction route is as follows:

[0071]

[0072] The prepared 4,4'-diboronic acid pinesyl ester triphenylamine compound, 2,6-dibromo-4-iodopyridine, potassium carbonate and tetrakis(triphenylphosphine)palladium were added to a Schlenk flask in a molar ratio of 1:(1.5-4):(5-8):(0.04-0.06), and after three cycles of vacuum-nitrogen circulation, 1,4-dioxane (10 ml 1,4-dioxane / mmol 2,6-dibromo-4-iodopyridine) and water were added as solvents (V 1,4-二氧六环 :V 水 =2-4:1), and continue to apply three nitrogen-vacuum cycles. After the cycle is completed, react for 10h-40h at 80-110°C in a nitrogen atmosphere. After the reaction is complete, discharge the material into deionized water, filter, dry, and then wash with methanol. 2,6-dibromopyridine-substituted triphenylamine compounds (dibromopyridine-substituted triphenylamine compounds) are obtained.

[0073] The reaction route is as follows:

[0074]

[0075] (3) Ullmann reaction

[0076] Dibromopyridine-substituted triphenylamine compounds, benzotriazole, cuprous iodide, N,N'-dimethylethylenediamine and potassium carbonate were added to a Schlenk flask in a molar ratio of 1:(3-7):(0.1-0.3):(0.2-0.6):(1-3). After applying three cycles of vacuum-nitrogen cycles to the system, dimethyl sulfoxide was added as a solvent (10 ml dimethyl sulfoxide / mmol 4,4'-dibromotriphenylamine compounds) using a syringe, and then three cycles of nitrogen-vacuum cycles were applied. The reaction was carried out at 80-120°C for 36-72 hours under a nitrogen atmosphere. After the reaction was completed, 20 ml of deionized water was slowly added to the reaction mixture, and extracted with ethyl acetate (3*20 ml). The organic phase was collected and dried with anhydrous sodium sulfate, filtered, and the organic solvent in the filtrate was removed by vacuum distillation. Ethyl acetate / petroleum ether was used as the eluent (V 乙酸乙酯 :V 石油醚 =10-20:1) and the crude product was purified by column chromatography to obtain the target product (multidentate organic ligand) containing the structure of "triphenylamine-pyridine-benzotriazole".

[0077] The reaction route is as follows:

[0078]

[0079] In some embodiments of the present invention, the iodide is 4-iodotoluene, 4-iodoanisole, 9-iodophenanthrene, iodobenzene, 4-iodoisopropylbenzene, 4-iodobiphenyl, 4-iodocyanobenzene, 1-iodo-4-(1-methylpropyl)benzene, 1-iodonaphthalene or 4-iodo-tert-butylbenzene.

[0080] The third aspect of the present invention provides the use of the above-mentioned multidentate organic ligand in the preparation of transition metal coordination polymers or electrochromic materials.

[0081] A fourth aspect of the present invention provides a method for preparing a transition metal coordination polymer, comprising the following steps:

[0082] The multidentate organic ligand is subjected to a complexation reaction with a metal salt to obtain the transition metal coordination polymer.

[0083] In some embodiments of the present invention, the molar ratio of the multidentate organic ligand to the metal salt is (2-3):1.

[0084] In some embodiments of the present invention, the metal salt is a transition metal salt, such as an iron salt, a cobalt salt, a nickel salt or a zinc salt, etc.; more specifically, it can be a bromide, iodide, nitrate, sulfate, phosphate, acetate, etc. of iron, cobalt, nickel or zinc.

[0085] In some embodiments of the present invention, the temperature of the complexation reaction is 60-100° C. and the time is 10 h-20 h.

[0086] A fifth aspect of the present invention provides a transition metal coordination polymer prepared by the above-mentioned method for preparing a transition metal coordination polymer.

[0087] A sixth aspect of the present invention provides the use of the above transition metal coordination polymer in the preparation of electrochromic materials.

[0088] A seventh aspect of the present invention provides an electrochromic material, the raw materials of which include the above-mentioned multidentate organic ligand or transition metal coordination polymer.

[0089] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0090] Example 1

[0091] The structure of a multidentate organic ligand is shown below:

[0092]

[0093] (1) Add 16.35 g (50.0 mmol) of bis(4-bromophenyl)amine, 10.9 g (50.0 mmol) of 4-iodotoluene, 0.38 g (2.0 mmol) of cuprous iodide, 0.36 g (2.0 mmol) of o-phenanthroline and 16.83 g (0.3 mol) of potassium hydroxide into a Schlenk bottle and apply three nitrogen-vacuum cycles. Finally, add 250 ml of anhydrous toluene as solvent and perform three vacuum-nitrogen cycles. Heat to 110°C under nitrogen atmosphere and react for 10 h. After the reaction is completed, filter, wash the catalyst (cuprous iodide) with dichloromethane (3×10 ml), collect the filtrate, and wash it with dichloromethane (3×10 ml) and deionized water (3×10 ml). Combine the organic phases and dry them with anhydrous sodium sulfate. Filter by suction and remove the organic solvent in the filtrate by distillation under reduced pressure. Use dichloromethane / petroleum ether as eluent (V 二氯甲烷 :V 石油醚 =3:1), and the crude product was purified by silica gel column chromatography to obtain 5.84 g of a dibromo-containing diphenylamine substituted compound (dibromo compound) with a yield of 28%.

[0094] (2) 5.84 g (14 mmol) of dibromo compound, 5.33 g (21 mmol) of bis(pinacolato)diboron, 6.87 g (70 mmol) of potassium acetate and 0.41 g (0.56 mmol) of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride were placed in a Schlenk flask and subjected to three vacuum-nitrogen cycles. Subsequently, 140 ml of 1,4-dioxane was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 80° C. under a nitrogen atmosphere for 10 h. After the reaction was completed, the mixture was extracted with dichloromethane (3×10 ml) and deionized water (3×10 ml). The organic phases were combined and dried over anhydrous sodium sulfate. After the organic solvent was dried by spin drying, 2.86 g of borate was obtained with a yield of 40%.

[0095] 2.86 g (5.6 mmol) of the boric acid ester prepared above, 3.05 g (8.4 mmol) of 2,6-dibromo-4-iodopyridine, 3.87 g (28 mmol) of potassium carbonate and 0.26 g (0.22 mmol) of tetrakis(triphenylphosphine)palladium were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 56 ml of 1,4-dioxane and 18 ml of water were added as solvents using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 80 ° C for 10 h under a nitrogen atmosphere. After the reaction was complete, the material was discharged into deionized water, filtered, dried, and then washed with methanol. 1.76 g of dibromopyridine-substituted triphenylamine compounds were obtained with a yield of 43%.

[0096] (3) 1.76 g (2.41 mmol) of dibromopyridine-substituted triphenylamine compounds, 0.86 g (7.23 mmol) of benzotriazole, 45 mg (0.24 mmol) of cuprous iodide, 42 mg (0.48 mmol) of N,N'-dimethylethylenediamine and 0.33 g (2.41 mmol) of potassium carbonate were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 24 ml of dimethyl sulfoxide was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 80°C under a nitrogen atmosphere for 36 h. After the reaction was completed, 20 ml of deionized water was slowly added to the reaction mixture, and extraction was carried out with ethyl acetate (3×20 ml). The organic phase was collected and dried with anhydrous sodium sulfate, filtered, and the organic solvent in the filtrate was removed by vacuum distillation. Ethyl acetate / petroleum ether was used as the eluent (V 乙酸乙酯 :V 石油醚 =12:1) the crude product was purified by column chromatography to obtain 0.78 g of the target product (multidentate organic ligand) containing the structure of "triphenylamine-pyridine-benzotriazole" with a yield of 37%.

[0097] Example 2

[0098] The structure of a multidentate organic ligand is shown below:

[0099]

[0100] (1) Add 16.35 g (50.0 mmol) of bis(4-bromophenyl)amine, 11.7 g (50.0 mmol) of 4-iodoanisole, 0.38 g (2.0 mmol) of cuprous iodide, 0.36 g (2.0 mmol) of o-phenanthroline and 16.83 g (0.3 mol) of potassium hydroxide into a Schlenk bottle and apply three vacuum-nitrogen cycles. Finally, add 250 ml of anhydrous toluene as a solvent and perform three vacuum-nitrogen cycles. Heat to 110°C under a nitrogen atmosphere and react for 10 h. After the reaction is completed, filter, wash the catalyst with dichloromethane (3×10 ml), collect the filtrate, and wash it with dichloromethane (3×10 ml) and deionized water (3×10 ml). Combine the organic phases and dry them with anhydrous sodium sulfate. Filter by suction and remove the organic solvent in the filtrate by vacuum distillation. Use dichloromethane / petroleum ether as eluent (V 二氯甲烷 :V 石油醚 =2:1), and the crude product was purified by silica gel column chromatography to obtain 6.71 g of a dibromo-containing diphenylamine substituted compound (dibromo compound) with a yield of 31%.

[0101] (2) 6.71 g (15.5 mmol) of the dibromo compound, 5.90 g (23.25 mmol) of bis(pinacolato)diboron, 7.61 g (77.5 mmol) of potassium acetate and 0.45 g (0.62 mmol) of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride were placed in a Schlenk flask and subjected to three vacuum-nitrogen cycles. Subsequently, 155 ml of 1,4-dioxane was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 80° C. under a nitrogen atmosphere for 10 h. After the reaction was completed, the mixture was extracted with dichloromethane (3×10 ml) and deionized water (3×10 ml). The organic phases were combined and dried over anhydrous sodium sulfate. After the organic solvent was dried by spin drying, 3.60 g of borate was obtained with a yield of 44%.

[0102] 3.60 g (6.82 mmol) of the boric acid ester prepared above, 3.71 g (10.23 mmol) of 2,6-dibromo-4-iodopyridine, 4.71 g (34.10 mmol) of potassium carbonate and 0.31 g (0.27 mmol) of tetrakis(triphenylphosphine)palladium were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 68 ml of 1,4-dioxane and 23 ml of water were added as solvents using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 80 ° C for 10 h under a nitrogen atmosphere. After the reaction was complete, the material was discharged into deionized water, filtered, dried, and then washed with methanol. 1.94 g of dibromopyridine-substituted triphenylamine compounds were obtained with a yield of 38%.

[0103] (3) 1.94 g (2.6 mmol) of dibromopyridine-substituted triphenylamine compounds, 0.93 g (7.8 mmol) of benzotriazole, 50 mg (0.26 mmol) of cuprous iodide, 46 mg (0.52 mmol) of N,N'-dimethylethylenediamine and 0.36 g (2.6 mmol) of potassium carbonate were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 26 ml of dimethyl sulfoxide was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 80°C under a nitrogen atmosphere for 36 h. After the reaction was completed, 20 ml of deionized water was slowly added to the reaction mixture, and extraction was carried out with ethyl acetate (3×20 ml). The organic phase was collected and dried with anhydrous sodium sulfate, filtered, and the organic solvent in the filtrate was removed by vacuum distillation. Ethyl acetate / petroleum ether was used as the eluent (V 乙酸乙酯 :V 石油醚 =10:1) and the crude product was purified by column chromatography to obtain 0.79 g of the target product (multidentate organic ligand) containing the structure of "triphenylamine-pyridine-benzotriazole" with a yield of 34%.

[0104] Example 3

[0105] The structure of a multidentate organic ligand is shown below:

[0106]

[0107] (1) Add 16.35 g (50.0 mmol) of bis(4-bromophenyl)amine, 15.20 g (50.0 mmol) of 9-iodophenanthrene, 0.38 g (2.0 mmol) of cuprous iodide, 0.36 g (2.0 mmol) of o-phenanthroline and 16.83 g (0.3 mol) of potassium hydroxide into a Schlenk bottle and apply three vacuum-nitrogen cycles. Finally, add 250 ml of anhydrous toluene as a solvent and perform three more vacuum-nitrogen cycles. Heat to 110°C under a nitrogen atmosphere and react for 10 h. After the reaction is completed, filter, wash the catalyst with dichloromethane (3×10 ml), collect the filtrate, and wash it with dichloromethane (3×10 ml) and deionized water (3×10 ml). Combine the organic phases and dry them with anhydrous sodium sulfate. Filter by suction and remove the organic solvent in the filtrate by vacuum distillation. Use dichloromethane / petroleum ether as the eluent (V 二氯甲烷 :V 石油醚 =5:1), and the crude product was purified by silica gel column chromatography to obtain 6.01 g of a dibromo-containing diphenylamine substituted compound (dibromo compound) with a yield of 24%.

[0108] (2) 6.01 g (12 mmol) of dibromo compound, 4.57 g (18 mmol) of bis(pinacolato)diboron, 5.89 g (60 mmol) of potassium acetate and 0.35 g (0.48 mmol) of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride were placed in a Schlenk flask and subjected to three vacuum-nitrogen cycles. Subsequently, 120 ml of 1,4-dioxane was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 80° C. under a nitrogen atmosphere for 10 h. After the reaction was completed, the mixture was extracted with dichloromethane (3×10 ml) and deionized water (3×10 ml). The organic phases were combined and dried over anhydrous sodium sulfate. After the organic solvent was dried, 2.80 g of borate was obtained with a yield of 39%.

[0109] 2.80 g (4.68 mmol) of the boric acid ester prepared above, 2.55 g (7.02 mmol) of 2,6-dibromo-4-iodopyridine, 3.23 g (23.4 mmol) of potassium carbonate and 0.22 g (0.19 mmol) of tetrakis(triphenylphosphine)palladium were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 46 ml of 1,4-dioxane and 15 ml of water were added as solvents using a syringe, and three vacuum-nitrogen cycles were applied. The reaction was carried out at 80 ° C for 10 h under a nitrogen atmosphere. After the reaction was complete, the material was discharged into deionized water, filtered, dried, and then washed with methanol. 1.63 g of dibromopyridine-substituted triphenylamine compounds were obtained with a yield of 43%.

[0110] (3) 1.63 g (2.01 mmol) of dibromopyridine-substituted triphenylamine compounds, 0.72 g (6.03 mmol) of benzotriazole, 38 mg (0.20 mmol) of cuprous iodide, 35 mg (0.40 mmol) of N,N'-dimethylethylenediamine and 0.28 g (2.01 mmol) of potassium carbonate were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 20 ml of dimethyl sulfoxide was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 80°C under a nitrogen atmosphere for 36 h. After the reaction was completed, 20 ml of deionized water was slowly added to the reaction mixture, and extraction was carried out with ethyl acetate (3×20 ml). The organic phase was collected and dried with anhydrous sodium sulfate, filtered, and the organic solvent in the filtrate was removed by vacuum distillation. Ethyl acetate / petroleum ether was used as the eluent (V 乙酸乙酯 :V 石油醚 =15:1) and the crude product was purified by column chromatography to obtain 0.87 g of the target product (multidentate organic ligand) containing the structure of "triphenylamine-pyridine-benzotriazole" with a yield of 45%.

[0111] Example 4

[0112] The structure of a multidentate organic ligand is shown below:

[0113]

[0114] (1) Add 16.35 g (50.0 mmol) of bis(4-bromophenyl)amine, 20.40 g (100.0 mmol) of iodobenzene, 0.48 g (2.5 mmol) of cuprous iodide, 0.45 g (2.5 mmol) of o-phenanthroline and 22.45 g (0.4 mol) of potassium hydroxide into a Schlenk bottle and apply three vacuum-nitrogen cycles. Finally, add 250 ml of anhydrous toluene as a solvent and perform three vacuum-nitrogen cycles. Heat to 120°C under a nitrogen atmosphere and react for 25 h. After the reaction is completed, filter, wash the catalyst with dichloromethane (3×10 ml), collect the filtrate, and wash it with dichloromethane (3×10 ml) and deionized water (3×7.5 ml). Combine the organic phases and dry them with anhydrous sodium sulfate. Filter by suction and remove the organic solvent in the filtrate by distillation under reduced pressure. Use dichloromethane / petroleum ether as the eluent (V 二氯甲烷 :V 石油醚 =4:1), and the crude product was purified by silica gel column chromatography to obtain 10.48 g of a dibromo-containing diphenylamine substituted compound (dibromo compound) with a yield of 52%.

[0115] (2) 10.28 g (26 mmol) of the dibromo compound, 19.81 g (78 mmol) of bis(pinacolato)diboron, 15.31 g (156 mmol) of potassium acetate and 0.95 g (1.3 mmol) of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride were placed in a Schlenk flask and subjected to three vacuum-nitrogen cycles. Subsequently, 260 ml of 1,4-dioxane was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 100 °C under a nitrogen atmosphere for 25 h. After the reaction was completed, the mixture was extracted with dichloromethane (3 × 10 ml) and deionized water (3 × 7.5 ml). The organic phases were combined and dried over anhydrous sodium sulfate. After the organic solvent was dried, 6.21 g of borate was obtained with a yield of 48%.

[0116] 6.21 g (12.48 mmol) of the boric acid ester prepared above, 13.58 g (37.44 mmol) of 2,6-dibromo-4-iodopyridine, 10.35 g (74.88 mmol) of potassium carbonate and 0.72 g (0.62 mmol) of tetrakis(triphenylphosphine)palladium were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 125 ml of 1,4-dioxane and 42 ml of water were added as solvents using a syringe, and three vacuum-nitrogen cycles were applied. The reaction was carried out at 100 ° C for 25 h under a nitrogen atmosphere. After the reaction was complete, the material was discharged into deionized water, filtered, dried, and then washed with methanol. 3.84 g of dibromopyridine-substituted triphenylamine compounds were obtained with a yield of 43%.

[0117] (3) 3.84 g (5.4 mmol) of dibromopyridine-substituted triphenylamine compounds, 3.21 g (27 mmol) of benzotriazole, 0.21 g (1.08 mmol) of cuprous iodide, 0.19 g (2.16 mmol) of N,N'-dimethylethylenediamine and 1.49 g (10.8 mmol) of potassium carbonate were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 54 ml of dimethyl sulfoxide was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 100 °C under a nitrogen atmosphere for 48 h. After the reaction was completed, 20 ml of deionized water was slowly added to the reaction mixture, and extraction was carried out with ethyl acetate (3×20 ml). The organic phase was collected and dried with anhydrous sodium sulfate, filtered, and the organic solvent in the filtrate was removed by vacuum distillation. Ethyl acetate / petroleum ether was used as the eluent (V 乙酸乙酯 :V 石油醚 =10:1) and the crude product was purified by column chromatography to obtain 2.53 g of the target product (multidentate organic ligand) containing the structure of "triphenylamine-pyridine-benzotriazole" with a yield of 54%.

[0118] Example 5

[0119] The structure of a multidentate organic ligand is shown below:

[0120]

[0121] (1) Add 16.35 g (50.0 mmol) of bis(4-bromophenyl)amine, 24.60 g (100.0 mmol) of 4-iodoisopropylbenzene, 0.48 g (2.5 mmol) of cuprous iodide, 0.45 g (2.5 mmol) of o-phenanthroline and 22.45 g (0.4 mol) of potassium hydroxide into a Schlenk bottle and apply three vacuum-nitrogen cycles. Finally, add 250 ml of anhydrous toluene as a solvent and perform three vacuum-nitrogen cycles. Heat to 120 °C under a nitrogen atmosphere and react for 25 h. After the reaction is completed, filter, wash the catalyst with dichloromethane (3 × 10 ml), collect the filtrate, and wash it with dichloromethane (3 × 10 ml) and deionized water (3 × 7.5 ml). Combine the organic phases and dry them with anhydrous sodium sulfate. Filter by suction and remove the organic solvent in the filtrate by vacuum distillation. Use dichloromethane / petroleum ether as eluent (V 二氯甲烷 :V 石油醚 =3:1), and the crude product was purified by silica gel column chromatography to obtain 10.85 g of a dibromo-containing diphenylamine substituted compound (dibromo compound) with a yield of 49%.

[0122] (2) 10.85 g (24.5 mmol) of the dibromo compound, 18.66 g (73.5 mmol) of bis(pinacolato)diboron, 14.43 g (147 mmol) of potassium acetate and 0.90 g (1.225 mmol) of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride were placed in a Schlenk flask and subjected to three vacuum-nitrogen cycles. Subsequently, 245 ml of 1,4-dioxane was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 100° C. under a nitrogen atmosphere for 25 h. After the reaction was completed, the mixture was extracted with dichloromethane (3×10 ml) and deionized water (3×7.5 ml). The organic phases were combined and dried over anhydrous sodium sulfate. After the organic solvent was dried by spin drying, 6.74 g of borate was obtained with a yield of 51%.

[0123] 6.74 g (12.5 mmol) of the boric acid ester prepared above, 13.60 g (37.5 mmol) of 2,6-dibromo-4-iodopyridine, 10.37 g (75 mmol) of potassium carbonate and 0.72 g (0.625 mmol) of tetrakis(triphenylphosphine)palladium were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 125 ml of 1,4-dioxane and 42 ml of water were added as solvents using a syringe, and three vacuum-nitrogen cycles were applied. The reaction was carried out at 100 ° C for 25 h under a nitrogen atmosphere. After the reaction was complete, the material was discharged into deionized water, filtered, dried, and then washed with methanol. 4.32 g of dibromopyridine-substituted triphenylamine compounds were obtained with a yield of 46%.

[0124] (3) 4.32 g (5.75 mmol) of dibromopyridine-substituted triphenylamine compounds, 3.42 g (28.75 mmol) of benzotriazole, 0.22 g (1.15 mmol) of cuprous iodide, 0.20 g (2.3 mmol) of N,N'-dimethylethylenediamine and 1.59 g (11.5 mmol) of potassium carbonate were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 58 ml of dimethyl sulfoxide was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 100 °C under a nitrogen atmosphere for 48 h. After the reaction was completed, 20 ml of deionized water was slowly added to the reaction mixture, and extraction was carried out with ethyl acetate (3×20 ml). The organic phase was collected and dried with anhydrous sodium sulfate, filtered, and the organic solvent in the filtrate was removed by vacuum distillation. Ethyl acetate / petroleum ether was used as the eluent (V 乙酸乙酯 :V 石油醚 =12:1) the crude product was purified by column chromatography to obtain 2.51 g of the target product (multidentate organic ligand) containing the structure of "triphenylamine-pyridine-benzotriazole" with a yield of 48%.

[0125] Example 6

[0126] The structure of a multidentate organic ligand is shown below:

[0127]

[0128] (1) Add 16.35 g (50.0 mmol) of bis(4-bromophenyl)amine, 28.00 g (100.0 mmol) of 4-iodobiphenyl, 0.48 g (2.5 mmol) of cuprous iodide, 0.45 g (2.5 mmol) of o-phenanthroline and 22.45 g (0.4 mol) of potassium hydroxide into a Schlenk bottle and apply three vacuum-nitrogen cycles. Finally, add 250 ml of anhydrous toluene as a solvent and perform three vacuum-nitrogen cycles. Heat to 120 °C under a nitrogen atmosphere and react for 25 h. After the reaction is completed, filter, wash the catalyst with dichloromethane (3 × 10 ml), collect the filtrate, and wash it with dichloromethane (3 × 10 ml) and deionized water (3 × 7.5 ml). Combine the organic phases and dry them with anhydrous sodium sulfate. Filter and remove the organic solvent in the filtrate by vacuum distillation. Use dichloromethane / petroleum ether as eluent (V 二氯甲烷 :V 石油醚 =5:1), and the crude product was purified by silica gel column chromatography to obtain 12.45 g of a dibrominated diphenylamine substituted compound (dibromo compound) with a yield of 52%.

[0129] (2) 12.45 g (26 mmol) of the dibromo compound, 19.81 g (78 mmol) of bis(pinacolato)diboron, 15.31 g (156 mmol) of potassium acetate and 0.95 g (1.3 mmol) of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride were placed in a Schlenk flask and subjected to three vacuum-nitrogen cycles. Subsequently, 260 ml of 1,4-dioxane was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 100 °C under a nitrogen atmosphere for 25 h. After the reaction was completed, the mixture was extracted with dichloromethane (3 × 10 ml) and deionized water (3 × 7.5 ml). The organic phases were combined and dried over anhydrous sodium sulfate. After the organic solvent was dried, 6.41 g of borate was obtained with a yield of 43%.

[0130] 6.41 g (11.18 mmol) of the boric acid ester prepared above, 12.17 g (33.54 mmol) of 2,6-dibromo-4-iodopyridine, 9.27 g (67.08 mmol) of potassium carbonate and 0.65 g (0.56 mmol) of tetrakis(triphenylphosphine)palladium were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 112 ml of 1,4-dioxane and 37 ml of water were added as solvents using a syringe, and three vacuum-nitrogen cycles were applied. The reaction was carried out at 100 ° C for 25 h under a nitrogen atmosphere. After the reaction was complete, the material was discharged into deionized water, filtered, dried, and then washed with methanol. 4.15 g of dibromopyridine-substituted triphenylamine compounds were obtained with a yield of 47%.

[0131] (3) 4.15 g (5.25 mmol) of dibromopyridine-substituted triphenylamine compounds, 3.13 g (26.25 mmol) of benzotriazole, 0.20 g (1.05 mmol) of cuprous iodide, 0.19 g (2.10 mmol) of N,N'-dimethylethylenediamine and 1.45 g (10.5 mmol) of potassium carbonate were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 53 ml of dimethyl sulfoxide was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 100 °C under a nitrogen atmosphere for 48 h. After the reaction was completed, 20 ml of deionized water was slowly added to the reaction mixture, and extraction was carried out with ethyl acetate (3×20 ml). The organic phase was collected and dried with anhydrous sodium sulfate, filtered, and the organic solvent in the filtrate was removed by vacuum distillation. Ethyl acetate / petroleum ether was used as the eluent (V 乙酸乙酯 :V 石油醚 =15:1) and the crude product was purified by column chromatography to obtain 2.03 g of the target product (multidentate organic ligand) containing the structure of "triphenylamine-pyridine-benzotriazole" with a yield of 41%.

[0132] Example 7

[0133] The structure of a multidentate organic ligand is shown below:

[0134]

[0135] (1) Add 16.35 g (50.0 mmol) of bis(4-bromophenyl)amine, 22.90 g (100.0 mmol) of 4-iodocyanobenzene, 0.48 g (2.5 mmol) of cuprous iodide, 0.45 g (2.5 mmol) of o-phenanthroline and 22.45 g (0.4 mol) of potassium hydroxide into a Schlenk bottle and apply three vacuum-nitrogen cycles. Finally, add 250 ml of anhydrous toluene as a solvent and perform three vacuum-nitrogen cycles. Heat to 120°C under a nitrogen atmosphere and react for 25 h. After the reaction is completed, filter, wash the catalyst with dichloromethane (3×10 ml), collect the filtrate, and wash it with dichloromethane (3×10 ml) and deionized water (3×7.5 ml). Combine the organic phases and dry them with anhydrous sodium sulfate. Filter by suction and remove the organic solvent in the filtrate by distillation under reduced pressure. Use dichloromethane / petroleum ether as the eluent (V 二氯甲烷 :V 石油醚 =10:1), and the crude product was purified by silica gel column chromatography to obtain 7.92 g of a dibromo-containing diphenylamine substituted compound (dibromo compound) with a yield of 37%.

[0136] (2) 7.92 g (18.5 mmol) of the dibromo compound, 14.09 g (55.5 mmol) of bis(pinacolato)diboron, 10.89 g (111 mmol) of potassium acetate and 0.68 g (0.925 mmol) of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride were placed in a Schlenk flask and subjected to three vacuum-nitrogen cycles. Subsequently, 185 ml of 1,4-dioxane was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 100 °C under a nitrogen atmosphere for 25 h. After the reaction was completed, the mixture was extracted with dichloromethane (3 × 10 ml) and deionized water (3 × 7.5 ml). The organic phases were combined and dried over anhydrous sodium sulfate. After the organic solvent was dried, 4.05 g of borate was obtained with a yield of 42%.

[0137] 4.05 g (7.77 mmol) of the boric acid ester prepared above, 8.46 g (23.31 mmol) of 2,6-dibromo-4-iodopyridine, 6.44 g (46.62 mmol) of potassium carbonate and 0.45 g (0.39 mmol) of tetrakis(triphenylphosphine)palladium were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 78 ml of 1,4-dioxane and 26 ml of water were added as solvents using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 100 ° C for 25 h under a nitrogen atmosphere. After the reaction was complete, the material was discharged into deionized water, filtered, dried, and then washed with methanol. 2.53 g of dibromopyridine-substituted triphenylamine compounds were obtained with a yield of 44%.

[0138] (3) 2.53 g (3.42 mmol) of dibromopyridine-substituted triphenylamine compounds, 2.04 g (17.10 mmol) of benzotriazole, 0.13 g (0.68 mmol) of cuprous iodide, 0.12 g (1.36 mmol) of N,N'-dimethylethylenediamine and 0.95 g (6.84 mmol) of potassium carbonate were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 34 ml of dimethyl sulfoxide was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 100°C under a nitrogen atmosphere for 48 h. After the reaction was completed, 20 ml of deionized water was slowly added to the reaction mixture, and extraction was carried out with ethyl acetate (3×20 ml). The organic phase was collected and dried with anhydrous sodium sulfate, filtered, and the organic solvent in the filtrate was removed by vacuum distillation. Ethyl acetate / petroleum ether was used as the eluent (V 乙酸乙酯 :V 石油醚 =12:1) the crude product was purified by column chromatography to obtain 1.19 g of the target product (multidentate organic ligand) containing the structure of "triphenylamine-pyridine-benzotriazole" with a yield of 39%.

[0139] Example 8

[0140] The structure of a multidentate organic ligand is shown below:

[0141]

[0142] (1) Add 16.35 g (50.0 mmol) of bis(4-bromophenyl)amine, 39.00 g (150.0 mmol) of 1-iodo-4-(1-methylpropyl)benzene, 0.57 g (3 mmol) of cuprous iodide, 0.54 g (3 mmol) of o-phenanthroline and 28.06 g (0.5 mol) of potassium hydroxide into a Schlenk bottle and apply three vacuum-nitrogen cycles. Finally, add 250 ml of anhydrous toluene as a solvent and perform three vacuum-nitrogen cycles. Heat to 130°C under a nitrogen atmosphere and react for 40 h. After the reaction is completed, filter, wash the catalyst with dichloromethane (3×10 ml), collect the filtrate, and wash it with dichloromethane (3×10 ml) and deionized water (3×5 ml). Combine the organic phases and dry them with anhydrous sodium sulfate. Filter by suction and remove the organic solvent in the filtrate by vacuum distillation. Use dichloromethane / petroleum ether as eluent (V 二氯甲烷 :V 石油醚 =8:1), and the crude product was purified by silica gel column chromatography to obtain 7.08 g of a dibromo-containing diphenylamine substituted compound (dibromo compound) with a yield of 31%.

[0143] (2) 7.08 g (15.5 mmol) of the dibromo compound, 15.74 g (62 mmol) of bis(pinacolato)diboron, 12.17 g (124 mmol) of potassium acetate and 0.68 g (0.93 mmol) of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride were placed in a Schlenk flask and subjected to three vacuum-nitrogen cycles. Subsequently, 155 ml of 1,4-dioxane was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 110° C. under a nitrogen atmosphere for 40 h. After the reaction was completed, the mixture was extracted with dichloromethane (3×10 ml) and deionized water (3×5 ml). The organic phases were combined and dried over anhydrous sodium sulfate. After the organic solvent was dried, 3.25 g of boric ester was obtained with a yield of 38%.

[0144] 3.25 g (5.9 mmol) of the boric acid ester prepared above, 8.56 g (23.6 mmol) of 2,6-dibromo-4-iodopyridine, 6.52 g (47.2 mmol) of potassium carbonate and 0.40 g (0.35 mmol) of tetrakis(triphenylphosphine)palladium were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 59 ml of 1,4-dioxane and 20 ml of water were added as solvents using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 110 ° C for 40 h under a nitrogen atmosphere. After the reaction was complete, the material was discharged into deionized water, filtered, dried, and then washed with methanol. 1.80 g of dibromopyridine-substituted triphenylamine compounds were obtained with a yield of 40%.

[0145] (3) 1.80 g (2.36 mmol) of dibromopyridine-substituted triphenylamine compounds, 1.97 g (16.52 mmol) of benzotriazole, 0.14 g (0.71 mmol) of cuprous iodide, 0.13 g (1.42 mmol) of N,N'-dimethylethylenediamine and 0.98 g (7.08 mmol) of potassium carbonate were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 24 ml of dimethyl sulfoxide was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 120°C under a nitrogen atmosphere for 72 h. After the reaction was completed, 20 ml of deionized water was slowly added to the reaction mixture, and extraction was carried out with ethyl acetate (3×20 ml). The organic phase was collected and dried with anhydrous sodium sulfate, filtered, and the organic solvent in the filtrate was removed by vacuum distillation. Ethyl acetate / petroleum ether was used as the eluent (V 乙酸乙酯 :V 石油醚 =15:1) and the crude product was purified by column chromatography to obtain 0.59 g of the target product (multidentate organic ligand) containing the structure of "triphenylamine-pyridine-benzotriazole" with a yield of 27%.

[0146] Example 9

[0147] The structure of a multidentate organic ligand is shown below:

[0148]

[0149] (1) Add 16.35 g (50.0 mmol) of bis(4-bromophenyl)amine, 38.09 g (150.0 mmol) of 1-iodonaphthalene, 0.57 g (3 mmol) of cuprous iodide, 0.54 g (3 mmol) of o-phenanthroline and 28.06 g (0.5 mol) of potassium hydroxide into a Schlenk bottle and apply three vacuum-nitrogen cycles. Finally, add 250 ml of anhydrous toluene as a solvent and perform three more vacuum-nitrogen cycles. Heat to 130 °C under a nitrogen atmosphere and react for 40 h. After the reaction is completed, filter, wash the catalyst with dichloromethane (3 × 10 ml), collect the filtrate, and wash it with dichloromethane (3 × 10 ml) and deionized water (3 × 5 ml). Combine the organic phases and dry them with anhydrous sodium sulfate. Filter and remove the organic solvent in the filtrate by vacuum distillation. Use dichloromethane / petroleum ether as the eluent (V 二氯甲烷 :V 石油醚 =10:1), and the crude product was purified by silica gel column chromatography to obtain 7.89 g of a dibromo-containing diphenylamine substituted compound (dibromo compound) with a yield of 35%.

[0150] (2) 7.89 g (17.5 mmol) of the dibromo compound, 17.78 g (75 mmol) of bis(pinacolato)diboron, 13.74 g (140 mmol) of potassium acetate and 0.77 g (1.05 mmol) of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride were placed in a Schlenk flask and subjected to three vacuum-nitrogen cycles. Subsequently, 175 ml of 1,4-dioxane was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 110° C. under a nitrogen atmosphere for 40 h. After the reaction was completed, the mixture was extracted with dichloromethane (3×10 ml) and deionized water (3×5 ml). The organic phases were combined and dried over anhydrous sodium sulfate. After the organic solvent was dried, 3.93 g of borate was obtained with a yield of 41%.

[0151] 3.93 g (7.1 mmol) of the boric acid ester prepared above, 10.30 g (28.4 mmol) of 2,6-dibromo-4-iodopyridine, 7.85 g (56.8 mmol) of potassium carbonate and 0.50 g (0.43 mmol) of tetrakis(triphenylphosphine)palladium were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 71 ml of 1,4-dioxane and 24 ml of water were added as solvents using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 110 ° C for 40 h under a nitrogen atmosphere. After the reaction was complete, the material was discharged into deionized water, filtered, dried, and then washed with methanol. 2.43 g of dibromopyridine-substituted triphenylamine compounds were obtained with a yield of 45%.

[0152] (3) 2.43 g (3.1 mmol) of dibromopyridine-substituted triphenylamine compounds, 2.58 g (21.7 mmol) of benzotriazole, 0.18 g (0.93 mmol) of cuprous iodide, 0.16 g (1.86 mmol) of N,N'-dimethylethylenediamine and 1.29 g (9.3 mmol) of potassium carbonate were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 31 ml of dimethyl sulfoxide was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 120°C under a nitrogen atmosphere for 72 h. After the reaction was completed, 20 ml of deionized water was slowly added to the reaction mixture, and extraction was carried out with ethyl acetate (3×20 ml). The organic phase was collected and dried with anhydrous sodium sulfate, filtered, and the organic solvent in the filtrate was removed by vacuum distillation. Ethyl acetate / petroleum ether was used as the eluent (V 乙酸乙酯 :V 石油醚 =20:1) the crude product was purified by column chromatography to obtain 1.05 g of the target product (multidentate organic ligand) containing the structure of "triphenylamine-pyridine-benzotriazole" with a yield of 37%.

[0153] Example 10

[0154] The structure of a multidentate organic ligand is shown below:

[0155]

[0156] (1) Add 16.35 g (50.0 mmol) of bis(4-bromophenyl)amine, 39.00 g (150.0 mmol) of 4-iodo-tert-butylbenzene, 0.57 g (3 mmol) of cuprous iodide, 0.54 g (3 mmol) of o-phenanthroline and 28.06 g (0.5 mol) of potassium hydroxide into a Schlenk bottle and apply three vacuum-nitrogen cycles. Finally, add 250 ml of anhydrous toluene as a solvent and perform three more vacuum-nitrogen cycles. Heat to 130 °C under a nitrogen atmosphere and react for 40 h. After the reaction is completed, filter, wash the catalyst with dichloromethane (3 × 10 ml), collect the filtrate, and wash it with dichloromethane (3 × 10 ml) and deionized water (3 × 5 ml). Combine the organic phases and dry them with anhydrous sodium sulfate. Filter and remove the organic solvent in the filtrate by vacuum distillation. Use dichloromethane / petroleum ether as eluent (V 二氯甲烷 :V 石油醚 =8:1), and the crude product was purified by silica gel column chromatography to obtain 7.54 g of a dibrominated diphenylamine substituted compound (dibromo compound) with a yield of 33%.

[0157] (2) 7.54 g (16.5 mmol) of the dibromo compound, 16.76 g (66 mmol) of bis(pinacolato)diboron, 12.95 g (132 mmol) of potassium acetate and 0.72 g (0.99 mmol) of [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride were placed in a Schlenk flask and subjected to three vacuum-nitrogen cycles. Subsequently, 155 ml of 1,4-dioxane was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 110° C. under a nitrogen atmosphere for 40 h. After the reaction was completed, the mixture was extracted with dichloromethane (3×10 ml) and deionized water (3×5 ml). The organic phases were combined and dried over anhydrous sodium sulfate. After the organic solvent was dried, 3.56 g of borate was obtained with a yield of 39%.

[0158] 3.56 g (6.4 mmol) of the boric acid ester prepared above, 9.29 g (25.6 mmol) of 2,6-dibromo-4-iodopyridine, 7.08 g (51.2 mmol) of potassium carbonate and 0.44 g (0.38 mmol) of tetrakis(triphenylphosphine)palladium were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 64 ml of 1,4-dioxane and 21 ml of water were added as solvents using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 110 ° C for 40 h under a nitrogen atmosphere. After the reaction was complete, the material was discharged into deionized water, filtered, dried, and then washed with methanol. 2.06 g of dibromopyridine-substituted triphenylamine compounds were obtained with a yield of 42%.

[0159] (3) 2.06 g (2.7 mmol) of dibromopyridine-substituted triphenylamine compounds, 2.25 g (18.9 mmol) of benzotriazole, 0.15 g (0.81 mmol) of cuprous iodide, 0.14 g (1.62 mmol) of N,N'-dimethylethylenediamine and 1.12 g (8.1 mmol) of potassium carbonate were placed in a Schlenk flask, and then three vacuum-nitrogen cycles were applied. 27 ml of dimethyl sulfoxide was added as a solvent using a syringe, and three vacuum-nitrogen cycles were applied again. The reaction was carried out at 120°C under a nitrogen atmosphere for 72 h. After the reaction was completed, 20 ml of deionized water was slowly added to the reaction mixture, and extraction was carried out with ethyl acetate (3×20 ml). The organic phase was collected and dried with anhydrous sodium sulfate, filtered, and the organic solvent in the filtrate was removed by vacuum distillation. Ethyl acetate / petroleum ether was used as the eluent (V 乙酸乙酯 :V 石油醚 =15:1) and the crude product was purified by column chromatography to obtain 0.77 g of the target product (multidentate organic ligand) containing the structure of "triphenylamine-pyridine-benzotriazole" with a yield of 31%.

[0160] Embodiment 11

[0161] The target ligand is polymerized with Fe(BF4)2·6H2O to obtain transition metal coordination polymer film 1:

[0162] 176.3 mg (0.2 mmol) of the multidentate organic ligand prepared in Example 1 and 33.8 mg (0.1 mmol) of Fe(BF4)2·6H2O were weighed and dissolved in 100 ml of ethanol. The mixture was refluxed at 60°C for 10 h to allow the ligand to completely complex with the metal ions. The insoluble matter was filtered out while hot, distilled under reduced pressure, washed with ethanol several times, and dried in vacuo to obtain 125 mg of a solid transition metal coordination polymer.

[0163] Take 50 mg of the above solid and dissolve it in 100 ml of methanol. Filter out the insoluble matter, take 5 ml of the solution and add it to the spray bottle of the pneumatic spray pen, then spray it on the surface of the ITO conductive glass, put it in an oven, and dry it at 30°C for 10 hours. After the methanol evaporates on the surface of the ITO glass, a uniform transition metal coordination polymer film is obtained, which is marked as Film 1.

[0164] Example 12

[0165] The target ligand was polymerized with CoCl2·6H2O to obtain transition metal coordination polymer film 2:

[0166] 190.8 mg (0.22 mmol) of the multidentate organic ligand prepared in Example 4 and 23.8 mg (0.10 mmol) of CoCl2·6H2O were weighed and dissolved in 100 ml of ethanol. The mixture was refluxed at 70°C for 13 h to allow the ligand to completely complex with the metal ions. The insoluble matter was filtered out while hot, distilled under reduced pressure, washed with ethanol several times, and dried in vacuo to obtain 154 mg of a solid transition metal coordination polymer.

[0167] Take 50 mg of the above solid and dissolve it in 100 ml of methanol, filter out the insoluble matter, take 7 ml of the solution and add it to the spray bottle of the pneumatic spray pen, then spray it on the surface of the ITO conductive glass, put it in an oven, and dry it at 40°C for 13 hours. After the methanol evaporates on the surface of the ITO glass, a uniform transition metal coordination polymer film is obtained, which is marked as Film 1.

[0168] Example 13

[0169] The target ligand was polymerized with ZnSO4·7H2O to obtain transition metal coordination polymer film 3:

[0170] 216.8 mg (0.25 mmol) of the multidentate organic ligand prepared in Example 4 and 28.8 mg (0.10 mmol) of ZnSO4·7H2O were weighed and dissolved in 100 ml of ethanol. The mixture was refluxed at 80°C for 16 h to allow the ligand to completely complex with the metal ions. The insoluble matter was filtered out while hot, distilled under reduced pressure, washed with ethanol several times, and dried in vacuo to obtain 158 mg of a solid transition metal coordination polymer.

[0171] Take 50 mg of the above solid and dissolve it in 100 ml of methanol. Filter out the insoluble matter, take 9 ml of the solution and add it to the spray bottle of the pneumatic spray pen, then spray it on the surface of the ITO conductive glass, put it in an oven, and dry it at 50°C for 16 hours. After the methanol evaporates on the surface of the ITO glass, a uniform transition metal coordination polymer film is obtained, which is marked as Film 3.

[0172] Embodiment 14

[0173] The target ligand is polymerized with Ni(OCOCH3)2·4H2O to obtain transition metal coordination polymer film 4:

[0174] Weigh 275.2 mg (0.3 mmol) of the multidentate organic ligand prepared in Example 9 and 25.9 mg (0.10 mmol) of Ni(OCOCH3)2·4H2O, dissolve them in 100 ml of ethanol, and reflux at 100°C for 20 h to completely complex the ligand with the metal ion. Filter out the insoluble matter while hot, distill under reduced pressure, wash with ethanol several times, and dry in vacuo to obtain 154 mg of a solid transition metal coordination polymer.

[0175] Take 50 mg of the above solid and dissolve it in 100 ml of methanol. Filter out the insoluble matter, take 10 ml of the solution and add it to the spray bottle of the pneumatic spray pen, then spray it on the surface of the ITO conductive glass, put it in an oven, and dry it at 60°C for 20 hours. After the methanol evaporates on the surface of the ITO glass, a uniform transition metal coordination polymer film is obtained, which is marked as Film 4.

[0176] Characterization and performance testing

[0177] 1) Figure 1 This is the hydrogen nuclear magnetic spectrum of the multidentate organic ligand prepared in Example 1; 1HNMR (500 MHz, Chloroform) δ8.07 (s, 2H), 7.97 (d, J = 4.1 Hz, 1H), 7.96 (s, 2H), 7.95 (d, J = 4.0 Hz, 1H), 7.56 (s, 1H), 7.54 (s, 1H), 7.41 (d, J = 4.1 Hz, 1H), 7.40 (s, 2H), 7.37 (s, 2H), 7.36 (s, 1H), 7.16 (s, 1H), 7.13 (s, 1H), 7.12 (s, 1H), 2.32 (s, 1H). The peak positions and integrated peak areas are consistent with the structure, indicating that the target organic ligand was successfully prepared.

[0178] 2) Figure 2The hydrogen nuclear magnetic spectrum of the multidentate organic ligand prepared in Example 4; 1HNMR (500 MHz, Chloroform) δ8.04 (s, 1H), 7.97 (d, J = 4.1 Hz, 1H), 7.96 (s, 1H), 7.95 (d, J = 4.0 Hz, 1H), 7.56 (s, 1H), 7.54 (s, 1H), 7.42-7.40 (m, 1H), 7.40 (s, 1H), 7.39 (s, 1H), 7.38 (d, The peak positions and integrated peak areas were consistent with the structure, indicating the successful preparation of the target organic ligand.

[0179] 3) Figure 7 This is the hydrogen nuclear magnetic spectrum of the multidentate organic ligand prepared in Example 8 of the present invention; 1 H NMR (500 MHz, Chloroform) δ8.10 (s, 1H), 7.96 (s, 2H), 7.55 (s, 1H), 7.55–7.52 (m, 1H), 7.42 (t, J = 7.5 Hz, 1H), 7.38 (d, J = 15.0 Hz, 2H), 7.37 (s, 1H), 7.18 (s, 1H), 7.18 (s, 1H), 7.06 (s, 1H), 7.06 (s, 1H), 2.55 (s, 1H), 1.52 (s, 1H), 1.16 (s, 1H), 0.76 (s, 1H). The peak positions and integrated peak areas were consistent with the structure, indicating the successful preparation of the target organic ligand.

[0180] 4) Figure 3 is the X-ray photoelectron spectrum of the transition metal coordination polymer prepared in Example 11; Figure 3 As shown, XPS elements detected C and N in the organic ligands, as well as Fe, B and F in the metal salts, proving the successful synthesis of transition metal coordination polymers.

[0181] 5) Figure 4 The electrochromatogram of the film 1 prepared in Example 11 is as follows: by using an electrochemical workstation, in the Amperometric it Curve mode, voltages of 0V, 1.2V and 1.3V are applied to the working electrode, and the changes in absorbance at different wavelengths are monitored by a UV-visible near-infrared spectrophotometer. Figure 4As shown, film 1 shows absorption in both visible light and near-infrared regions. When the voltage increases from 0V to 1.3V, the maximum absorption wavelength of the film also changes.

[0182] 6) The cyclic voltammetry performance of the film 1 prepared in Example 11 was tested as follows: the ITO containing the transition metal coordination polymer film in Example 11 was used as the working electrode, the platinum wire was used as the counter electrode, the Ag / AgCl was used as the reference electrode, and the 0.1M tetrabutylammonium perchlorate (TBAP) acetonitrile solution was used as the electrolyte; based on the three-electrode system, the cyclic voltammetry performance was tested by an electrochemical workstation at a scan rate of 100 mV / s. The results are shown in FIG. Figure 5 , Figure 5 is the cyclic voltammogram of the film 1 in Example 11; Figure 5 It can be seen that film 1 has a pair of reversible redox potentials.

[0183] 7) Figure 6 The electrochromic response time spectrum of the film 1 prepared in Example 11 is as follows: a square wave voltage of 1.10 to 1.40 V is applied to the working electrode in the Chronoamperometry mode by an electrochemical workstation, and the change of the absorption spectrum at 600 nm is monitored by a UV-visible near-infrared spectrophotometer. Figure 6 It can be seen that the transition metal coordination polymer marked as film 1 has a faster response speed and excellent cycle stability.

[0184] 8) The solubility test was conducted on the transition metal coordination polymers prepared in Examples 11 to 14. The concentration of the solutions formed by different transition metal coordination polymers in different solvents was 2 mg / mL. The results are shown in Table 1.

[0185] Table 1 Solubility of transition metal coordination polymers prepared in Examples 11 to 14 in 6 common solvents

[0186]

[0187] Note: ++: soluble at room temperature; +: soluble upon heating; -: insoluble upon heating.

[0188] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A multidentate organic ligand, It is characterized in that The structural formula is shown in Formula Ⅰ; In Formula I, R is one of the following structural formulas:

2. A method for preparing the multidentate organic ligand according to claim 1, It is characterized in that The following steps are involved: Bis(4-bromophenyl)amine and iodide undergo Ullmann reaction to prepare dibromo-containing diphenylamine substituted compounds; The dibromo-containing diphenylamine substituted compound is subjected to a Suzuki reaction with bis(pinacol)diboron to obtain a 4,4'-diboric acid pinesyl ester triphenylamine compound; The 4,4'-diboronic acid pinesyl ester triphenylamine compound and 2,6-dibromo-4-iodopyridine undergo a Suzuki reaction to obtain a 2,6-dibromopyridine-substituted triphenylamine compound; The triphenylamine compound substituted by 2,6-dibromopyridine and benzotriazole undergo Ullmann reaction to obtain the multidentate organic ligand.

3. The method for preparing the multidentate organic ligand according to claim 2, It is characterized in that The molar ratio of the bis(4-bromophenyl)amine to the iodide is 1:(1-3); The molar ratio of the dibromo-containing diphenylamine substituted compound to the bis(pinacol)diboron is 1:(1.5-4); The molar ratio of the 4,4'-diboronic acid pinesyl ester triphenylamine compound to the 2,6-dibromo-4-iodopyridine is 1:(1.5-4); The molar ratio of the triphenylamine compound substituted by 2,6-dibromopyridine to the benzotriazole is 1:(3-7).

4. The method for preparing a multidentate organic ligand according to claim 2, It is characterized in that The iodide is 4-iodotoluene, 4-iodoanisole, 9-iodophenanthrene, iodobenzene, 4-iodoisopropylbenzene, 4-iodobiphenyl, 4-iodocyanobenzene, 1-iodo-4-(1-methylpropyl)benzene, 1-iodonaphthalene or 4-iodo-tert-butylbenzene.

5. Use of the multidentate organic ligand according to claim 1 in the preparation of transition metal coordination polymers or electrochromic materials.

6. A method for preparing a transition metal coordination polymer, It is characterized in that The following steps are involved: The multidentate organic ligand according to claim 1 is subjected to a complexation reaction with a metal salt to obtain the transition metal coordination polymer.

7. The method for preparing the transition metal coordination polymer according to claim 6, It is characterized in that The molar ratio of the multidentate organic ligand to the metal salt is (2-3):1; the metal salt is a transition metal salt; the temperature of the complex reaction is 60-100°C, and the time is 10h-20h.

8. A transition metal coordination polymer prepared according to the method for preparing a transition metal coordination polymer according to claim 6 or 7.

9. Use of the transition metal coordination polymer as claimed in claim 8 in the preparation of electrochromic materials.

10. An electrochromic material, It is characterized in that The raw material comprises the multidentate organic ligand according to claim 1 or the transition metal coordination polymer according to claim 8.

Citation Information

Patent Citations

  • Terpyridyl derivative with electroluminescent and electrochromic characteristics and complex thereof

    CN102532003A

  • TPA-TPY-Fe<2+> metal complex nanosheet as well as preparation method and application thereof

    CN109143713A

  • Polydentate organic ligand, metal supramolecular polymer, polymer film and preparation method