EC resin dispersing agent, preparation method thereof and metal conductive paste

By grafting different groups on the EC resin to form high-performance polymer dispersants, the problems of inorganic filler precipitation and insufficient interaction force between resin and silver powder are solved, the dispersion of filler and the adhesion of resin are improved, and the printing is achieved The aspect ratio of the gate line is increased.

CN118978609APending Publication Date: 2024-11-19NANTONG T SUN NEW ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411041024.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Inorganic fillers in existing conductive pastes are prone to precipitation due to changes in temperature and time, resulting in insufficient dispersion, and the effect of the resin and silver powder are poor, so the adhesion of the resin to the silicon wafer needs to be improved.

Method used

Using EC resin dispersant, by grafting different groups such as C7H15OH and phosphate groups on the EC resin, esterification reaction and hydrolysis treatment are carried out to form a high-performance polymer dispersant, which improves the dispersion uniformity of the organic carrier and the resin and The force of silver powder.

Benefits of technology

Improve the dispersion and stability of filler substances, enhance the action force between resin and silver powder and the adhesion force of resin to silicon wafers, reduce the viscosity of slurry, and improve the aspect ratio of the grid line after printing to achieve The purpose of narrowing linearity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978609A_ABST
    Figure CN118978609A_ABST
Patent Text Reader

Abstract

The invention provides an EC resin dispersing agent, a preparation method thereof and metal conductive paste, and belongs to the technical field of conductive metal paste applied to solar cells. The structural formula of the EC resin dispersant is as follows: # imgabs0 #, R is an R1 or R2 group, at least one R is an R2 group, and at least one R is an R1 group; r1 is # imgabs1, R2 is # imgabs2, and R3 is any one of # imgabs3, # imgabs4. The EC resin dispersant disclosed by the invention can improve the dispersion uniformity of an organic carrier in slurry, the acting force between resin and silver powder and the bonding force of the resin to a silicon wafer, and also can improve the viscosity of metal conductive slurry, so that the height-width ratio of a grid line after printing is improved, and the aim of narrowing the linearity is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of conductive metal pastes for solar cells, and in particular relates to an EC resin dispersant and a preparation method thereof, and a metal conductive paste. Background Art

[0002] In the existing conductive paste, the main phosphate and fatty acid dispersants used are inorganic powders and metal powders, which are mutually adsorbed by the polar phosphate or carboxyl groups through anchoring. The other side chains separate the filler particles through steric hindrance or non-polar repulsive groups, maintain a certain spacing distance, achieve dispersion, and reduce the viscosity of the paste. However, when the inorganic filler is dissolved in the solvent, although the filler particles are dispersed, with the change of temperature and time, the inorganic filler is prone to precipitation, and then there are problems such as insufficient dispersion and agglomeration. In addition, the interaction between the resin and the silver powder is poor, and the adhesion of the resin to the silicon wafer needs to be improved.

[0003] Therefore, it is necessary to propose a new dispersant that is conducive to dispersing the filler material, maintaining long-term stability, and avoiding agglomeration between inorganic filler particles. Summary of the invention

[0004] The present disclosure aims to solve at least one of the technical problems existing in the prior art, and provides an EC resin dispersant and a preparation method thereof, and a metal conductive paste.

[0005] In one aspect of the present disclosure, an EC resin dispersant is provided for use in metal conductive paste, wherein the structural formula of the EC resin dispersant is as follows:

[0006]

[0007] wherein R is an R1 or R2 group, and at least one R is an R2 group, and at least one R is an R1 group;

[0008] R1 is

[0009] R2 is R3 is Any one of .

[0010] Optionally, the EC resin dispersant is any one of the following structural formulas:

[0011]

[0012] Optionally, the EC resin dispersant is any one of the following structural formulas:

[0013]

[0014]

[0015] In another aspect of the present disclosure, a method for preparing the EC resin dispersant described above is provided, the method comprising:

[0016] Add C7H 15 OH and phosphoric acid, heat treatment, to obtain grafted C7H 15 O- and phosphate-based EC resin solutions;

[0017] At a preset grafting temperature, materials for grafting R3 groups are added in batches to the grafting compound solution, and subjected to esterification reaction and hydrolysis treatment to obtain a synthetic product.

[0018] Optionally, the material for grafting the R3 group is any one of benzyl alcohol, diethylene glycol butyl ether, and butyl glycolate.

[0019] Optionally, the temperature of the heating treatment is 45-55° C.; and / or,

[0020] The preset grafting temperature is 50-90° C., and the esterification reaction time is 3-5 hours; and / or,

[0021] The time of the hydrolysis treatment is 1-3h.

[0022] Optionally, the solid-to-liquid ratio of the grafted EC resin solution to the material for grafting the R3 group is (9-11): 1 g / mL.

[0023] Optionally, the total amount of the material for grafting the R3 group is 15-25 mL.

[0024] Optionally, the amount of the material for grafting R3 groups added in each batch is 4-6 mL.

[0025] In another aspect of the present disclosure, a metal conductive paste is provided.

[0026] The slurry includes:

[0027] Silver powder;

[0028] Glass powder;

[0029] The organic carrier comprises the EC resin dispersant described above.

[0030] The present invention provides an EC resin dispersant and a preparation method thereof, and a metal conductive paste. The structural formula of the EC resin dispersant is as follows: Wherein, R is an R1 or R2 group, and at least one R is an R2 group, and at least one R is an R1 group; R1 is R2 is R3 is The high-performance polymer dispersant disclosed in the present invention can improve the uniformity of the dispersion of the organic carrier in the slurry, increase the interaction between the resin and the silver powder, and thus enhance the adhesion of the resin to the silicon wafer. It can also increase the viscosity of the metal conductive slurry, further increase the aspect ratio of the gate line after printing, and achieve the purpose of narrowing the linearity. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The flowchart of the method for preparing the EC resin dispersant according to the embodiment of the present disclosure is shown. DETAILED DESCRIPTION

[0032] In order to enable those skilled in the art to better understand the technical solution of the present disclosure, the present disclosure is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be understood that the specific embodiments described herein are only used to explain the present disclosure and are not used to limit the disclosure. The described embodiments are part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the described embodiments of the present disclosure, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present disclosure.

[0033] In one aspect of the present disclosure, an EC resin dispersant is provided for use in metal conductive pastes. The structural formula of the EC resin dispersant is as follows:

[0034]

[0035] wherein R is an R1 or R2 group, and at least one R is an R2 group, and at least one R is an R1 group;

[0036] R1 is

[0037] R2 is In the R2 group, R3 is

[0038] Any one of .

[0039] It should be noted that in the above structural formula, the R group can be an R1 group or an R2 group, but it is necessary to ensure that at least one R group is an R2 group and at least one R group is an R1 group. In other words, one R group is an R1 group and the other R group is an R2 group, and the other R group can be either an R1 group or an R2 group, and the positions of the R1 and R2 groups are not specifically limited.

[0040] In some preferred embodiments, in the above structural formula (1), when two Rs are R1 groups and the other R is R2 group, the corresponding EC resin dispersant is the following structural formula (2) and (3). Of course, it should be understood that the R1 group can also be located at the position of the R2 group, and the R2 group can also be located at the position of any R1 group:

[0041] or

[0042] In other preferred embodiments, in the above structural formula (1), when two Rs are R2 groups and one R is R1 group, the corresponding EC resin dispersant is the following structural formula (4), and similarly, the R1 group therein can also be located at any position of the R2 group, and the R2 group can also be located at the position of the R1 group.

[0043]

[0044] As a further preferred embodiment, the EC resin dispersant is any one of the following structural formulas (5, 6, 7):

[0045]

[0046]

[0047] The EC resin dispersant provided in this embodiment has a viscosity of 5.44-19.07 Pa·s, a molecular weight of 40000-87000, and a hydroxyl value of 7.05-8.01, that is, the grafted EC resin has more hydrogen bonds between molecules and has a greater viscosity, which helps to increase the interaction between the resin and the silver powder.

[0048] In this embodiment, different groups are grafted onto ethyl cellulose ether (EC) to achieve good dispersion of inorganic filler materials. At the same time, molecular cross-linking can be achieved by adjusting its own functional groups to maintain long-term stability, which helps to improve the dispersibility of inorganic fillers in the slurry. At the same time, the interaction between the resin and the silver powder can be enhanced, thereby improving the adhesion of the resin to the silicon wafer.

[0049] In another aspect of the present disclosure, a method S100 for preparing the EC resin dispersant as described above is provided, which specifically comprises the following steps S110 to S120:

[0050] S110, add C7H 15 OH and phosphoric acid, heat treatment, to obtain grafted C7H 15 O- and phosphate-based EC resin solutions.

[0051] Specifically, C7H 15 OH and phosphoric acid, as well as EC resin solution, are placed in a three-necked flask, stirred at 450-550 rpm (be careful to prevent splashing during stirring), and heated to 45-55°C. After dehydration condensation, C7H 15 O- and phosphate esters were grafted onto EC resin.

[0052] In some preferred embodiments, the heating temperature is preferably 45°C, 50°C, 55°C. During the heating process, C7H 15 OH and phosphoric acid undergo dehydration condensation with EC and are grafted onto EC to form C7H 15 O- and phosphate groups.

[0053] In other preferred embodiments, the content of the EC resin solution is preferably 150-250 parts by mass, for example, 150 g, 170 g, 200 g, 250 g, etc.

[0054] It should be understood that EC resin is ethyl cellulose, and its structural formula (8) is as follows: In the structural formula (8), R groups can be grafted onto the three -OH groups of the middle boat-like structure to form a grafted EC resin. In this way, when the formed dispersant is used in a metal conductive paste, the grafted groups are cross-linked to maintain the long-term stability of the paste and avoid agglomeration.

[0055] It should also be understood that the grafted C7H 15 The EC resin solution structure (9) of O- and phosphate groups is as follows:

[0056]

[0057] That is, R1 groups are grafted onto the two lower -OH groups of the middle boat-like structure, and a phosphate group is grafted onto the upper -OH group.

[0058] S120, at a preset grafting temperature, adding a material for grafting R3 groups into the grafting compound solution in batches, and subjecting the mixture to esterification reaction and hydrolysis treatment to obtain a synthetic product.

[0059] Specifically, when the EC resin solution in step S110 is stabilized to the preset grafting temperature, the R3 grafting substance is added in batches, and when the R3 grafting substance is added in each stage, it is necessary to ensure that the R3 grafting substance added in the previous batch is completely dissolved, and the state is slurry, and the color is dark yellow. The esterification reaction time is recorded, and after the esterification reaction is completed, deionized water is added for hydrolysis treatment. During the hydrolysis process, the color of the solution gradually becomes lighter to obtain a product.

[0060] In some preferred embodiments, the material for grafting the R3 group is any one of benzyl alcohol, diethylene glycol butyl ether, and butyl glycolate.

[0061] As a further preferred embodiment, when the material for grafting the R3 group is benzyl alcohol, the R3 group in the corresponding structural formula (1) is

[0062] As a further preferred embodiment, when the material for grafting the R3 group is diethylene glycol butyl ether, the R3 group in the corresponding structural formula (1) is

[0063]

[0064] As a further preferred embodiment, when the material for grafting the R3 group is butyl glycolate, the R3 group in the corresponding structural formula (1) is

[0065] In other preferred embodiments, the amount of the material for grafting R3 groups added in each batch is 4-6 mL, for example, 4 mL, 5 mL, 6 mL, etc.

[0066] In other preferred embodiments, the total amount of the material for grafting the R3 group is 15-25 mL, for example, 15 mL, 20 mL, 25 mL, etc.

[0067] It should be understood that when the amount of each batch of grafted R3 group material added is preferably 4 mL, and the total amount of grafted R3 group material added is 20 mL, the total batch addition is 5 times. When the amount of each batch of grafted R3 group material added is preferably 5 mL, and the total amount of grafted R3 group material added is 20 mL, the total batch addition is 4 times, which is not specifically limited.

[0068] In some other preferred embodiments, the solid-to-liquid ratio of the grafted EC resin solution to the material for grafting the R3 group is (9-11):1 g / mL, for example, 9:1, 10:1, 11:1.

[0069] As a further preferred solution, when the mass of the EC resin solution is 200 g, the material for grafting the R3 group is preferably 20 mL, and the amount added each time is 5 mL, which is added in four times.

[0070] In other preferred embodiments, the grafting temperature is preset to be 50-90°C, and the esterification reaction time is 3-5 hours. For example, the temperature is preferably 50°C, 60°C, 70°C, 90°C, etc., and the time is preferably 3 hours, 4 hours, 5 hours.

[0071] In other preferred embodiments, the hydrolysis treatment time is 1-3 hours. For example, the hydrolysis time is preferably 1 hour, 2 hours, or 3 hours.

[0072] In this embodiment, the preparation process is simple. By controlling the reaction conditions and the amount of material added for grafting the R3 group, the R3 and R1, R2 groups can be grafted onto the EC resin to form a high-performance polymer dispersant, which can effectively improve the dispersion uniformity of the organic carrier in the slurry.

[0073] In another aspect of the present disclosure, a metal conductive paste is provided, which includes: silver powder, glass powder, and an organic carrier, wherein the organic carrier includes the EC resin dispersant described above.

[0074] In some preferred embodiments, the content of silver powder is 80-92 parts by mass, the content of glass powder is 2-6 parts by mass, and the content of organic vehicle is 5-20 parts by mass, wherein the mass proportion of EC resin dispersant in the organic vehicle is 2-15wt%, more preferably 3%-10wt%.

[0075] It should be understood that the organic vehicle may include components such as resin, solvent and thixotropic agent in addition to the dispersant, and this is not specifically limited.

[0076] Specifically, the metal conductive slurry is formed by the following method: placing an organic carrier and glass powder in a ball mill, stirring and centrifuging, then adding an appropriate amount of silver powder to the ball mill, stirring and centrifuging, and using a three-roll mill for rolling and grinding to obtain a slurry.

[0077] In this embodiment, when the EC resin dispersant is added to the metal conductive paste, the viscosity of the paste can be reduced, and the paste will not fall off after being dried after printing, and the linear aspect ratio of the paste after printing is significantly improved.

[0078] The preparation method of EC resin dispersant and metal conductive paste will be further described below in conjunction with specific examples:

[0079] Example 1

[0080] The preparation method of the EC resin dispersant in this example includes the following steps:

[0081] S1. Add C7H2O to 200g EC resin solution. 15 OH and phosphoric acid, stirred at 500 rpm, heated to 50 ° C, and obtained grafted with C7H 15 O- and phosphate-based EC resin solutions.

[0082] S2. When the EC resin solution stabilizes to the preset grafting temperature of 50°C, add a total of 20 mL of diethylene glycol butyl ether in portions, about 5 mL each time. When adding diethylene glycol butyl ether at each stage, ensure that the previous addition is completely dissolved, and the state is slurry, and the color is dark yellow. Record the time. The esterification reaction takes 4 hours. After the esterification reaction is completed, add 2 mL of deionized water and hydrolyze for 2 hours. During the hydrolysis process, the color of the solution gradually becomes lighter, and the reaction is completed. Collect the synthetic product to obtain the EC resin dispersant.

[0083] As shown in Table 1, the viscosity of the grafted EC resin dispersant was 5.44 Pa·s, the molecular weight was 40,000, and the hydroxyl value was 7.05.

[0084] Furthermore, 10 parts by mass of an organic carrier (including the aforementioned EC resin dispersant) and 4 parts by mass of glass powder were placed in a ball mill and centrifuged at 1000 r / s for 300 s → manually stirred → centrifuged at 1000 r / s for 300 s → centrifuged at 1000 r / s for 300 s → added 86 parts by mass of silver powder → centrifuged at 500 r / s for 150 s → manually stirred → centrifuged at 500 r / s for 150 s → centrifuged at 500 r / s for 150 s → three-roll mill → 4-150 (30 / 15) → 4-150 (30 / 15) → 5-150 (15 / 8) → 5-150 (15 / 8).

[0085] As shown in Table 2, when the shear rate is 0.5s-1, the viscosity of the slurry is 338.586Pa·s, when the shear rate is 5s-1, the viscosity of the slurry is 51.5671Pa·s, when the shear rate is 10s-1, the viscosity of the slurry is 32.5127Pa·s, when the shear rate is 50s-1, the viscosity of the slurry is 13.8474Pa·s, and when the shear rate is 95s-1, the stress of the slurry is 1007.86Pa.

[0086] Further, please continue to refer to Table 2. The EC resin dispersant obtained in Example 1 was introduced into the slurry. The average line width of the printed grid lines was 79.23 μm, and the average line height of the printed grid lines was 2.19 μm. It was found that the slurry viscosity was lower than that of the slurry in Comparative Example 1, which indicates that the introduction of R1 increases the solvation effect, effectively reduces the line width, and increases the line height. At the same time, it has no negative effect on the powder loss during drying after printing of the slurry. The powder loss rating is A, which effectively reduces the slurry viscosity.

[0087] Example 2

[0088] The preparation method of the EC resin dispersant in this example includes the following steps:

[0089] S1. Add C7H2O to 200g EC resin solution. 15 OH and phosphoric acid, stirred at 500 rpm, heated to 50 ° C, and obtained grafted with C7H15 O- and phosphate-based EC resin solutions.

[0090] S2. When the EC resin solution stabilizes to the preset grafting temperature of 50°C, add a total of 20 mL of butyl glycolate in portions, about 5 mL each time. When adding butyl glycolate at each stage, ensure that the previous addition is completely dissolved and in a slurry state with a dark yellow color. Record the time. The esterification reaction takes 4 hours. After the esterification reaction is completed, add 2 mL of deionized water and hydrolyze for 2 hours. During the hydrolysis process, the color of the solution gradually becomes lighter, and the reaction is completed. Collect the synthetic product to obtain the EC resin dispersant.

[0091] As shown in Table 1, the viscosity of the grafted EC resin dispersant is 9.15 Pa·s, the molecular weight is 45,000, and the hydroxyl value is 7.23.

[0092] Furthermore, 10 parts by mass of an organic carrier (including the aforementioned EC resin dispersant) and 4 parts by mass of glass powder were placed in a ball mill and centrifuged at 1000 r / s for 300 s → manually stirred → centrifuged at 1000 r / s for 300 s → centrifuged at 1000 r / s for 300 s → added 86 parts by mass of silver powder → centrifuged at 500 r / s for 150 s → manually stirred → centrifuged at 500 r / s for 150 s → centrifuged at 500 r / s for 150 s → three-roll mill → 4-150 (30 / 15) → 4-150 (30 / 15) → 5-150 (15 / 8) → 5-150 (15 / 8).

[0093] As shown in Table 2, when the shear rate is 0.5s-1, the viscosity of the slurry is 375.029Pa·s, when the shear rate is 5s-1, the viscosity of the slurry is 62.2057Pa·s, when the shear rate is 10s-1, the viscosity of the slurry is 37.9748Pa·s, when the shear rate is 50s-1, the viscosity of the slurry is 13.8458Pa·s, and when the shear rate is 95s-1, the stress of the slurry is 904.771Pa.

[0094] Further, please continue to refer to Table 2. The EC resin dispersant obtained in Example 2 is introduced into the slurry, and the average line width of the printed grid line is 76.57 μm, and the average line height of the printed grid line is 2.30 μm. It is found that the slurry viscosity is lower than that of the slurry in Comparative Example 1, which indicates that the introduction of R2 increases the solvation effect and has no negative effect on the drying of the slurry after printing. However, the slurry viscosity increases compared with Example 1, which may be because the planarity of the butyl glycolate structure is larger than that of the diethylene glycol butyl ether structure, and the linear aspect ratio is improved.

[0095] Example 3

[0096] The preparation method of the EC resin dispersant in this example includes the following steps:

[0097] S1. Add C7H2O to 200g EC resin solution. 15 OH and phosphoric acid, stirred at 500 rpm, heated to 50 ° C, and obtained grafted with C7H 15 O- and phosphate-based EC resin solutions.

[0098] S2. When the EC resin solution stabilizes to the preset grafting temperature of 50°C, add a total of 20 mL of benzyl alcohol in portions, about 5 mL each time. When adding benzyl alcohol at each stage, ensure that the previous addition is completely dissolved and in a slurry state with a dark yellow color. Record the time. The esterification reaction takes 4 hours. After the esterification reaction is completed, add 2 mL of deionized water and hydrolyze for 2 hours. During the hydrolysis process, the color of the solution gradually becomes lighter, and the reaction is completed. Collect the synthetic product to obtain the EC resin dispersant.

[0099] As shown in Table 1, the viscosity of the grafted EC resin dispersant is 15.46 Pa·s, the molecular weight is 80,000, and the hydroxyl value is 7.89.

[0100] Furthermore, 10 parts by mass of an organic carrier (including the aforementioned EC resin dispersant) and 4 parts by mass of glass powder were placed in a ball mill and centrifuged at 1000 r / s for 300 s → manually stirred → centrifuged at 1000 r / s for 300 s → centrifuged at 1000 r / s for 300 s → added 86 parts by mass of silver powder → centrifuged at 500 r / s for 150 s → manually stirred → centrifuged at 500 r / s for 150 s → centrifuged at 500 r / s for 150 s → three-roll mill → 4-150 (30 / 15) → 4-150 (30 / 15) → 5-150 (15 / 8) → 5-150 (15 / 8).

[0101] As shown in Table 2, when the shear rate is 0.5s-1, the viscosity of the slurry is 665.205Pa·s, when the shear rate is 5s-1, the viscosity of the slurry is 107.001Pa·s, when the shear rate is 10s-1, the viscosity of the slurry is 66.1031Pa·s, when the shear rate is 50s-1, the viscosity of the slurry is 25.5597Pa·s, and when the shear rate is 95s-1, the stress of the slurry is 1760.79Pa.

[0102] Further, please continue to refer to Table 2. The EC resin dispersant obtained in Example 3 was introduced into the slurry. The average line width of the printed grid lines was 75.82 μm, and the average line height of the printed grid lines was 2.25 μm. It was found that the slurry viscosity was close to that of the comparative slurry. This shows that the introduction of R3 made the EC resin dispersant more planar and increased the viscosity. At the same time, it had no negative effect on the powder loss during drying after printing of the slurry, and the linear aspect ratio of the slurry after printing can be significantly improved.

[0103] Example 4

[0104] The preparation method of the EC resin dispersant in this example includes the following steps:

[0105] S1. Add C7H2O to 200g EC resin solution. 15 OH and phosphoric acid, stirred at 500 rpm, heated to 50 ° C, and obtained grafted with C7H 15 O- and phosphate-based EC resin solutions.

[0106] S2. When the EC resin solution stabilizes to the preset grafting temperature of 70°C, add a total of 20 mL of benzyl alcohol in portions, about 5 mL each time. When adding benzyl alcohol at each stage, ensure that the previous addition is completely dissolved and in a slurry state with a dark yellow color. Record the time. The esterification reaction takes 4 hours. After the esterification reaction is completed, add 2 mL of deionized water and hydrolyze for 2 hours. During the hydrolysis process, the color of the solution gradually becomes lighter, and the reaction is completed. Collect the synthetic product to obtain the EC resin dispersant.

[0107] As shown in Table 1, the viscosity of the grafted EC resin dispersant is 18.49 Pa·s, the molecular weight is 85,000, and the hydroxyl value is 7.95.

[0108] Furthermore, 10 parts by mass of an organic carrier (including the aforementioned EC resin dispersant) and 4 parts by mass of glass powder were placed in a ball mill and centrifuged at 1000 r / s for 300 s → manually stirred → centrifuged at 1000 r / s for 300 s → centrifuged at 1000 r / s for 300 s → added 86 parts by mass of silver powder → centrifuged at 500 r / s for 150 s → manually stirred → centrifuged at 500 r / s for 150 s → centrifuged at 500 r / s for 150 s → three-roll mill → 4-150 (30 / 15) → 4-150 (30 / 15) → 5-150 (15 / 8) → 5-150 (15 / 8).

[0109] As shown in Table 2, when the shear rate is 0.5s-1, the viscosity of the slurry is 666.642Pa·s, when the shear rate is 5s-1, the viscosity of the slurry is 105.118Pa·s, when the shear rate is 10s-1, the viscosity of the slurry is 64.3666Pa·s, when the shear rate is 50s-1, the viscosity of the slurry is 23.1328Pa·s, and when the shear rate is 95s-1, the stress of the slurry is 1465.11Pa.

[0110] Further, please continue to refer to Table 2. The EC resin dispersant obtained in Example 4 was introduced into the slurry. The average line width of the printed grid lines was 65.14 μm, and the average line height of the printed grid lines was 2.56 μm. It was found that the slurry viscosity was close to that of the comparative slurry. This shows that the introduction of R3 made the EC resin dispersant more planar, the grafting temperature increased, and the viscosity slightly increased. At the same time, it had no negative effect on the powder loss after drying of the slurry after printing, and the linear aspect ratio of the slurry after printing can be significantly improved.

[0111] Example 5

[0112] The preparation method of the EC resin dispersant in this example includes the following steps:

[0113] S1. Add C7H2O to 200g EC resin solution. 15 OH and phosphoric acid, stirred at 500 rpm, heated to 50 ° C, and obtained grafted with C7H 15 O- and phosphate-based EC resin solutions.

[0114] S2. When the EC resin solution stabilizes to the preset grafting temperature of 90°C, add a total of 20 mL of benzyl alcohol in portions, about 5 mL each time. When adding benzyl alcohol at each stage, ensure that the previous addition is completely dissolved and in a slurry state with a dark yellow color. Record the time. The esterification reaction takes 4 hours. After the esterification reaction is completed, add 2 mL of deionized water and hydrolyze for 2 hours. During the hydrolysis process, the color of the solution gradually becomes lighter, and the reaction is completed. Collect the synthetic product to obtain the EC resin dispersant.

[0115] As shown in Table 1, the viscosity of the EC resin dispersant after grafting is 19.07 Pa·s, the molecular weight is 87000, and the hydroxyl value is 8.01.

[0116] Furthermore, 10 parts by mass of an organic carrier (including the aforementioned EC resin dispersant) and 4 parts by mass of glass powder were placed in a ball mill and centrifuged at 1000 r / s for 300 s → manually stirred → centrifuged at 1000 r / s for 300 s → centrifuged at 1000 r / s for 300 s → added 86 parts by mass of silver powder → centrifuged at 500 r / s for 150 s → manually stirred → centrifuged at 500 r / s for 150 s → centrifuged at 500 r / s for 150 s → three-roll mill → 4-150 (30 / 15) → 4-150 (30 / 15) → 5-150 (15 / 8) → 5-150 (15 / 8).

[0117] As shown in Table 2, when the shear rate is 0.5s-1, the viscosity of the slurry is 671.461Pa·s, when the shear rate is 5s-1, the viscosity of the slurry is 109.628Pa·s, when the shear rate is 10s-1, the viscosity of the slurry is 67.0961Pa·s, when the shear rate is 50s-1, the viscosity of the slurry is 25.1134Pa·s, and when the shear rate is 95s-1, the stress of the slurry is 1688.59Pa.

[0118] Further, please continue to refer to Table 2. The EC resin dispersant obtained in Example 5 was introduced into the slurry. The average line width of the printed grid lines was 62.28 μm, and the average line height of the printed grid lines was 3.72 μm. It was found that the slurry viscosity was close to that of the comparative slurry. This shows that the introduction of R3 made the EC resin dispersant more planar, the grafting temperature increased, and the viscosity increased. At the same time, it had no negative effect on the powder loss during drying after printing of the slurry, and the linear aspect ratio of the slurry after printing can be significantly improved.

[0119] In summary, according to the results of Examples 1-5, after R1 is introduced into EC resin, the molecular weight of the polymer increases, and after the resin solution is brewed, the intermolecular interaction force is enhanced, and the viscosity increases. Secondly, after R2 is introduced into EC resin, the planarity of butyl glycolate structure is stronger than that of diethylene glycol butyl ether, and after it is grafted onto ethyl cellulose, the intermolecular interaction force is greatly enhanced, and the viscosity increases. Furthermore, after R3 is introduced into EC resin, the planarity of benzyl alcohol structure is stronger than that of diethylene glycol butyl ether and butyl glycolate, and after it is grafted onto ethyl cellulose, the steric hindrance increases, and after it is brewed into a resin solution, the degree of mutual entanglement between molecules is higher, and the viscosity increases; and as the grafting temperature increases, the molecules are more closely entangled, more intermolecular hydrogen bonds are formed, and the viscosity increases.

[0120] Comparative Example 1

[0121] The preparation method of the EC resin dispersant in this example includes the following steps:

[0122] Add C7H to 200g EC resin solution. 15 OH and phosphoric acid, stirred at 500 rpm, heated to 50 ° C, and obtained grafted with C7H 15 O- and phosphate-based EC resin solutions.

[0123] As shown in Table 1, the viscosity of the grafted EC resin was 4.91 Pa·s, the molecular weight was 38,000, and the hydroxyl value was 6.42.

[0124] Furthermore, 10 parts by mass of an organic carrier (including the aforementioned grafted EC resin) and 4 parts by mass of glass powder were placed in a ball mill and centrifuged at 1000 r / s for 300 s → manually stirred → centrifuged at 1000 r / s for 300 s → centrifuged at 1000 r / s for 300 s → added 86 parts by mass of silver powder → centrifuged at 500 r / s for 150 s → manually stirred → centrifuged at 500 r / s for 150 s → centrifuged at 500 r / s for 150 s → three-roll mill → 4-150 (30 / 15) → 4-150 (30 / 15) → 5-150 (15 / 8) → 5-150 (15 / 8).

[0125] As shown in Table 2, when the shear rate is 0.5s-1, the viscosity of the slurry is 527.248Pa·s, when the shear rate is 5s-1, the viscosity of the slurry is 107.511Pa·s, when the shear rate is 10s-1, the viscosity of the slurry is 70.2561Pa·s, when the shear rate is 50s-1, the viscosity of the slurry is 27.9979Pa·s, and when the shear rate is 95s-1, the stress of the slurry is 1842.97Pa.

[0126] Further, please continue to refer to Table 2. The EC resin dispersant obtained in this comparative example 1 was introduced into the slurry. The average line width of the printed grid lines was 78.25 μm, and the average line height of the printed grid lines was 1.43 μm. It was found that powder falling occurred after the slurry was printed.

[0127] Table 1 EC resin dispersant grafting R3 materials, grafting temperature and performance results

[0128]

[0129] Table 2 Performance results of metal conductive paste

[0130]

[0131]

[0132] In summary, the molar fraction of EC resin dispersant in Examples 1-5 and Comparative Example 1 is the same. Except for the EC resin dispersant, the composition and mass fraction of other components in the slurry of Examples 1-5 and Comparative Example 1 are the same, and the powder loss rating of Examples 1-5 is A, and there is no powder loss phenomenon.

[0133] The present disclosure provides an EC resin dispersant and a preparation method thereof, and a metal conductive paste, which have the following beneficial effects compared to the prior art: the EC resin dispersant of the present disclosure has a good dispersing effect on fillers, can achieve intermolecular cross-linking through the adjustment of its own functional groups, maintain long-term stability, avoid filler particle agglomeration, and also increase the interaction between the resin and the silver powder, the adhesion between the resin and the silicon wafer, etc. In addition, the preparation method of the present disclosure is simple, and by adjusting the process parameters, the R1, R2, and R3 groups are grafted onto the EC resin to form a high molecular polymer dispersant.

[0134] It is to be understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present disclosure, but the present disclosure is not limited thereto. For those of ordinary skill in the art, various modifications and improvements can be made without departing from the spirit and substance of the present disclosure, and these modifications and improvements are also considered to be within the scope of protection of the present disclosure.

Claims

1. An EC resin dispersant for metal conductive paste, characterized in that: The structural formula of the EC resin dispersant is as follows: wherein R is an R1 or R2 group, and at least one R is an R2 group, and at least one R is an R1 group; R1 is R2 is R3 is Any one of .

2. The EC resin dispersant according to claim 1, characterized in that The EC resin dispersant is any one of the following structural formulas:

3. The EC resin dispersant according to claim 2, characterized in that The EC resin dispersant is any one of the following structural formulas:

4. A method for preparing the EC resin dispersant according to any one of claims 1 to 3, characterized in that: The method comprises: Add C7H 15 OH and phosphoric acid, heat treatment, to obtain grafted C7H 15 O- and phosphate-based EC resin solutions; At a preset grafting temperature, materials for grafting R3 groups are added in batches to the grafting compound solution, and subjected to esterification reaction and hydrolysis treatment to obtain a synthetic product.

5. The method according to claim 4, characterized in that The material for grafting the R3 group is any one of benzyl alcohol, diethylene glycol butyl ether and butyl glycolate.

6. The method according to claim 4, characterized in that The temperature of the heating treatment is 45-55°C; and / or, The preset grafting temperature is 50-90° C., and the esterification reaction time is 3-5 hours; and / or, The time of the hydrolysis treatment is 1-3h.

7. The method according to claim 4, characterized in that The solid-to-liquid ratio of the grafted EC resin solution to the material for grafting the R3 group is (9-11): 1 g / mL.

8. The method according to claim 7, characterized in that The total amount of material added for grafting R3 groups is 15-25 mL.

9. The method according to claim 8, characterized in that The amount of the material for grafting the R3 group added in each batch is 4-6 mL.

10. A metal conductive paste, characterized in that: The metal conductive paste comprises: Silver powder; Glass powder; An organic carrier, comprising the EC resin dispersant according to any one of claims 1 to 3.