Preparation method of dendronized spiral polydiphenylacetylene and chiral fluorescent nano particles of dendronized spiral polydiphenylacetylene

Through the design and halogenization reaction of branched spiral polydiphenylene, the stability of chiral fluorescent materials under high temperature and strong light irradiation conditions was solved, and the preparation of nanoparticles with high fluorescence quantum yield and morphological diversity was achieved. , provides stable chiral fluorescent nanoparticles and morphologically stable stimulus responsive materials.

CN118978622AActive Publication Date: 2024-11-19SHANGHAI UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411278824.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

Acquisition of high-stability chiral fluorescent materials remains one of the major challenges, especially under high temperature and strong light irradiation conditions, the prior art is difficult to provide stable chiral fluorescent nanoparticles and morphologically stable stimulus-responsive materials.

Method used

By developing branched spiral polydiphenylene and its preparation method, cinnamate motifs are introduced and cross-linked through auratic reaction, chiral fluorescent nanoparticles with high fluorescence quantum yield and good photothermal stability can be formed in different ways. The spiral conformation and self-assembly in the solvent are nanostructures that regulate the helical conformation and self-assembly into various morphologies.

Benefits of technology

The preparation of chiral fluorescent nanoparticles with stability and morphological diversity under high temperature and strong light irradiation conditions is achieved, providing spiral polymers suitable for harsh environments, and supporting the formation of nanostructures of various morphology. The optical properties and stability of the material are significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978622A_ABST
    Figure CN118978622A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of dendronized spiral polydiphenylacetylene and a chiral fluorescent nanoparticle of the dendronized spiral polydiphenylacetylene. Cinnamic acid ester is introduced to a polydiphenylacetylene side group dendronized alkoxy ether element nuclear point through molecular design, the synthesis steps are simple, the reaction is rapid, and the prepared dendronized spiral polydiphenylacetylene can regulate and control the spiral conformation and the chiral circular polarization luminescence property through solvation. In addition, the dendronized spiral polydiphenylacetylene can be self-assembled into various chiral fluorescent nanoparticles, and cross-linking curing is initiated by ultraviolet radiation, so that the structure and chirality of the nanoparticles have good stability. The chiral fluorescent nano material is high in fluorescence quantum yield and good in light and heat stability, and has a good application prospect in the field of chiral photoelectric materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chiral fluorescent materials, in particular to a dendrite helical polytolane and a method for preparing chiral fluorescent nanoparticles based on the dendrite helical polytolane. Background Art

[0002] Chiral circularly polarized fluorescent materials have attracted widespread attention in recent years due to their potential application value in three-dimensional optical imaging, information storage encryption, and biological probes. Self-assembly strategies are widely used in the construction of chiral fluorescent nanomaterials because they can effectively enhance the asymmetric factor of chiral fluorescence. At present, obtaining highly stable chiral fluorescent materials is still one of the major challenges. Helical polymers, combined with their rigid main chain and inherent chirality, can self-assemble to form chiral nanostructures with multiple morphologies, including vesicles, nanorings, supramolecular helical fibers, etc. Helical poly(phenylacetylene) is a class of polyacetylene derivatives with highly conjugated main chains. Compared with monosubstituted poly(phenylacetylene), it has higher photothermal stability and photoinduced fluorescence quantum yield, making it an ideal platform for the preparation of stable chiral fluorescent materials. Photodimerization reactions are of great significance in the synthesis of natural products and drug chemistry. These photodimerization units can be integrated into polymer materials as main chains, side groups or additives. Because they can directly and non-destructively adjust the physicochemical properties of polymer structures, they have been widely used in materials science in recent years. However, the modified photodimerization groups in polymers obviously have a larger free movement space than in crystals. The random collision of photodimerization groups can satisfy the above reaction conditions at a certain moment in time and space, which significantly reduces the difficulty of designing the introduction of reactive groups. However, the appropriate structure can still significantly accelerate the speed of photodimerization or increase the degree of dimerization, and provide new opportunities for regulating the photodimerization of polymer bases. Based on the spatial requirements of photodimerization, the selectivity of photodimerization between adjacent side groups within the molecule, between non-adjacent side groups within the molecule, and between molecules can be manipulated through structural design to obtain polymer materials of different scales. Summary of the invention

[0003] The purpose of the present invention is to prepare a chiral fluorescent material with stable structure and chirality; a method for preparing a branched helical polytolane and chiral fluorescent nanoparticles thereof is developed. The branched helical polytolane developed by the present invention can regulate the helical conformation and circularly polarized fluorescence of the polymer by solvation, has high fluorescence quantum yield, good light and thermal stability, and can self-assemble into a variety of chiral fluorescent nanoparticles, including dense spheres, loose spheres and nanobowls. Cinnamate moieties are introduced into the core points of the side-group branched alkoxy ether moieties, and after appropriate ultraviolet irradiation, photocyclization reactions are initiated and nanoassemblies are cross-linked and cured, so that the supramolecular structure and chirality of the nanoparticles have good stability to the environment. This technology lays a foundation for the development of helical polymers suitable for harsh environmental conditions such as high temperature and strong light irradiation. At the same time, it provides an effective strategy for supporting the preparation of chiral and morphologically stable stimulus-responsive chiral fluorescent nanoparticles by photocrosslinking of helical polymers, especially the strategy allows the preparation of nanostructures with various morphologies with opposite fluorescent optical activities from a helical polymer.

[0004] One of the purposes of the present invention is to provide a helical polytolane modified with a dendronized alkoxy ether. The polymer has polytolane as the main chain, a dendronized alkoxy ether modified with cinnamate at the core point as the side group, and alanine alcohol as the connecting unit.

[0005] As an embodiment of the present invention, the branched alkoxy ether modified helical polytolane has the structural formula:

[0006]

[0007] Preferably, the degree of polymerization of the dendritic polyphenylene vinylene used is n=50-1000.

[0008] Preferably, the substituent R of the dendronized polytolane is a lower alkyl group, which is a C1-C6 alkyl group, such as methyl, ethyl, etc.

[0009] Preferably, the chiral configuration of the chiral amino alcohol is R-type or S-type. * indicates the connection site.

[0010] Preferably, the degree of polymerization of the oligomeric alkoxy ether may be m=1-4.

[0011] The helical polytolane modified by the branched alkoxy ether of the present invention can provide circularly polarized luminescence and can be cross-linked by light irradiation. Moreover, the helical polytolane modified by the branched alkoxy ether of the present invention can form two opposite helical conformations according to the polarity of the solvent at high temperature in different solvents, and retain the conformation induced at high temperature at room temperature. It also has the ability to maintain stable chiral optical properties when irradiated with high temperature or strong light.

[0012] The present invention also relates to a method for preparing a spiral polytolane modified by a dendronized alkoxy ether, which comprises first synthesizing a polytolane polymer precursor functionalized by an active ester of pentafluorophenol, and then combining the precursor with a dendronized macromolecule modified with cinnamate through an amidation reaction to obtain the spiral polytolane modified by a dendronized alkoxy ether.

[0013] As a preferred technical solution of the present invention, the method for preparing the dendrite helical polytolane of the present invention comprises the following steps:

[0014] S1, Compound B Polymer C was obtained by polymerization under the catalysis of tetraphenyltin and tungsten hexachloride. n = 50 to 1000;

[0015] S2, Compound C and Compound D Amidation reaction occurs to obtain polymer A That is, the helical polytolane modified by the dendrite alkoxy ether; in the structural formula of compound D, m=1-4, R is a lower alkyl group, and the chiral configuration of the chiral amino alcohol is R-type or S-type. The lower alkyl group is a C1-C6 alkyl group, such as methyl, ethyl, etc.

[0016] Preferably, in step S1, the polymerization reaction is carried out in toluene.

[0017] Preferably, in step S1, the molar ratios of compound B to tetraphenyltin and tungsten hexachloride are 1:5-50 and 1:10-1:100 respectively, and the reaction temperature is 80-100°C.

[0018] Preferably, in step S2, the reaction is an amidation reaction in the presence of an organic base;

[0019] Preferably, in step S2, the molar ratio of the polymerized unit of compound C to the polymerized unit of compound D is 1:1.5-5.

[0020] The second object of the present invention is to provide a self-assembled aggregate (chiral fluorescent nanoassembly) and a preparation method thereof, which comprises adding a poor solvent to a solution containing the branched alkoxy ether-modified helical polytolane, inducing self-assembly by a nanoprecipitation method, and obtaining the self-assembled aggregate.

[0021] Preferably, the selective organic solvent used for the solution of the dendronized alkoxy ether-modified helical polytolane is a polar protic solvent, such as MeOH, ethanol, and the like.

[0022] Preferably, the poor solvent is water.

[0023] Preferably, the solution of the branched alkoxy ether-modified helical polytolane further contains a good solvent, and the good solvent is a polar aprotic solvent, such as THF, DMF, DMSO, and the like.

[0024] Preferably, the volume ratio of the selective organic solvent, the good solvent and the poor solvent is 1:(0-4):(0.5-19).

[0025] Preferably, in the solution of the helical polytolane modified by dendronized alkoxy ether, the mass fraction of the helical polytolane modified by dendronized alkoxy ether is 0.01 to 0.5 wt %.

[0026] In some specific implementation examples, the above-mentioned helical polytolane modified with dendronized alkoxy ether is dissolved in an organic solvent and water is added to the solution, which can self-assemble to form spherical or bowl-shaped nanoparticles.

[0027] The third object of the present invention is to provide a method for photo-crosslinking the dendritic polytolane nanoassembly and photo-crosslinked nanoparticles; the photo-crosslinked nanoparticles are obtained by inducing a photocyclization reaction between cinnamate esters through light irradiation of the self-assembled aggregates.

[0028] Preferably, ultraviolet light is used to irradiate the dendritic polyphenylene nanoassembly solution to induce a photodimerization reaction between cinnamate esters, thereby achieving photo-crosslinking of the nanoassembly.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] 1) The present invention provides a method for preparing a dendritic polyphenylene vinylene. Through molecular design and synthesis, a polymer precursor functionalized with pentafluorophenol active ester is first synthesized, and then combined with a dendritic macromolecule through an amidation reaction to successfully prepare the dendritic polyphenylene vinylene. The steps are simple and the reaction is rapid. The prepared dendritic polyphenylene vinylene has good application prospects in the fields of fluorescence sensing and the like.

[0031] 2) The alkoxy ether dendronized polytolane prepared by the present invention introduces cinnamate at the core point of the dendronized alkoxy ether moiety, giving this type of thermosensitive dendronized polytolane a photodimerization reaction characteristic. The helical conformation, fluorescence optical activity and self-assembly behavior of the polytolane can be regulated by solvation, and a cross-linked assembly can be prepared by light-induced photocyclization reaction; the method is simple to prepare, and the structure and optical properties are highly stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0033] Figure 1 For polymer C1 H NMR spectrum;

[0034] Figure 2 For polymer C 19 F NMR spectrum;

[0035] Figure 3 For polymer A 1 H NMR spectrum;

[0036] Figure 4 For polymer A 13 C NMR spectrum;

[0037] Figure 5 Circular dichroism spectra of polymer A treated at 80℃ for different time in toluene (a) and DMSO (b) solution;

[0038] Figure 6 The chiral fluorescence spectra of polymer A after being treated with DMSO (blue line) or Toluene (red line) at high temperature and then transferred to DMSO solution at room temperature;

[0039] Figure 7 is the hydrodynamic radius distribution diagram of polymer A in different solvents;

[0040] Figure 8 Atomic force microscopy images of self-assembled polymers A in different solvents; (a) methanol solution, and (b) solvent ratios are v MeOH / v THF / v water =1 / 0 / 4, (c)v MeOH / v THF / v water =1 / 1 / 4,(d)v MeOH / v THF / v water = 1 / 1 / 19 mixed solution, scale bar is 100 nm;

[0041] Fig. 9 The UV / visible spectra of polymer A at different UV irradiation times;

[0042] Fig.10 Nanoparticles prepared from polymer A, (a) main chain molar ellipticity at different times after being transferred to toluene solution and heated to 100 °C, and (b) fluorescence spectra at different temperatures in aqueous solution;

[0043] Fig.11 Circular dichroism spectra (a) and fluorescence spectra (b) of nanoparticles prepared from polymer A after different UV irradiation times. DETAILED DESCRIPTION

[0044] The present invention is described in detail below in conjunction with examples and drawings. The following examples will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0045] Example 1. Synthesis of dendrite helical polytolane

[0046] In this example, the following synthetic route was used to prepare the dendritic helical polytolane:

[0047]

[0048] The specific steps include:

[0049] Compound B is polymerized under the catalysis of tetraphenyltin and tungsten hexachloride to obtain polymer C; wherein compound B is synthesized according to reference (Angew. Chem. Int. Ed., 2022, 134, e202115070);

[0050] The polymerization reaction is carried out in toluene, the molar ratios of compound B to tetraphenyltin and tungsten hexachloride are 1:10 and 1:50 respectively, and the reaction temperature is 100°C.

[0051] Polymer C and compound D The reaction yields polymer A, namely the branched alkoxy ether-modified helical polytolane.

[0052] The reaction is an amidation reaction in the presence of an organic base, triethylamine, and the molar ratio of the polymerized unit of polymer C to compound D is 1:5. The reaction solvent is tetrahydrofuran, and the reaction temperature is 40°C.

[0053] Among them, compound D can be synthesized according to the following route (reference (J.Colloid Interface Sci.2025,667,928-940)):

[0054]

[0055] The specific steps include:

[0056] Compound E is subjected to an esterification reaction with N-tert-butyloxycarbonyl-D-alaninol in the presence of a coupling agent 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and a catalyst 4-dimethylaminopyridine to obtain compound F, wherein compound E is synthesized according to reference (Macromolecules 2020, 53, 10866-10873).

[0057] The esterification reaction is carried out in a dichloromethane solution, the molar ratio of compound E, N-tert-butyloxycarbonyl-D-alaninol, coupling agent and catalyst is 1:0.8:1.5:0.2, and the reaction temperature is 0°C.

[0058] Subsequently, compound F is subjected to a deprotection reaction in an acidic environment. After the reaction is completed, the organic phase is washed with a saturated sodium bicarbonate aqueous solution to obtain compound D.

[0059] The deprotection reaction was carried out in a mixed solution of dichloromethane and trifluoroacetic acid in a volume ratio of 4:1, and the compound concentration was 0.1 g mL -1 , the reaction temperature is 0℃.

[0060] The key intermediates and the desired products were characterized by NMR and the molecular weight of the polymers was determined by GPC and are summarized in Table 1. The details are given in Figures 1 to 4 Available in.

[0061] Table 1 Polymerization conditions and results of dendritic polyphenylene vinylene

[0062]

[0063] Example 2: Photophysical properties

[0064] In this embodiment, polymer A has good solubility in a variety of solvents and exhibits excellent circularly polarized luminescence performance. When it is dissolved in DMSO and toluene, the fluorescence quantum yield is 45% and 28% respectively, and the peak intensity of the first Codon signal corresponding to the main chain at 397nm in the circular dichroism spectrum is about 2.8×10 4 deg cm 2 dmol -1 , indicating that the main chain conformation of dendrite polydiphenylvinylene is independent of solvent polarity at room temperature. Subsequently, the polymer solution temperature was raised to 80 °C and maintained for different time periods, then cooled to room temperature and subjected to CD testing. With the extension of high temperature annealing time, the CD signal intensity of the toluene solution gradually increased and reached a maximum value of about -9×10 4 deg cm 2 dmol -1 However, after high-temperature annealing in the highly polar solvent DMSO, the CD signal of the polymer reversed with time, and the Cotton signal intensity finally increased to about 9×10 4 deg cm 2 dmol -1 The above results show that dendritic poly(diphenylvinylene) can be induced into a dominant right-handed helical conformation and a dominant left-handed helical conformation after high-temperature annealing in low-polarity solvent toluene or high-polarity solvent DMSO, respectively ( Figure 5). The CPL signal direction of these polymer solutions is consistent with the CD signal, and g lum The maximum value is close to + / -1×10 -3 ( Figure 6 ).

[0065] Example 3: Self-assembly properties

[0066] In this example, by taking advantage of the significant radial amphiphilicity of the dendritic helical polytolane, a poor solvent, water, was added to the MeOH solution of the above-mentioned dendritic polytolane A to induce self-assembly by nanoprecipitation. DLS showed that at a solvent ratio of v MeOH / v water =1 / 4 of the polymer solution formed chiral nanoparticles with a hydrodynamic radius of about 110 nm. It is worth noting that when a small amount of good solvent THF was introduced into the above solution (v MeOH / v THF / v water =1 / 1 / 4), the hydrodynamic radius of the nanoparticles increased significantly to 154nm. The further increase in the content of poor solvent water (v MeOH / v THF / v water =1 / 1 / 19), resulting in the hydrodynamic radius of the nanoparticles being reduced to 86 nm ( Figure 7 ). Atomic force microscopy characterized the morphology of the above aggregates ( Figure 8 ).

[0067] Example 4: Photo-crosslinking behavior of dendritic polytolane

[0068] In this embodiment, the dendritic helical polytolane A self-assembles into nanoparticles in a mixed solution of water and methanol in a volume ratio of 4 to 1. Subsequently, the nanoparticle solution is irradiated with a wavelength of 365 nm and an intensity of 12 mW cm -2 The photocycloaddition reaction of the aggregates formed by dendritic poly(tolanthylene A) was studied by UV-visible spectroscopy. Fig. 9 ). As the illumination time increases, the absorption peak at 305nm attributed to the cinnamate chromophore decreases significantly, indicating that efficient photodimerization occurs. The dimerization degree x increases rapidly with the illumination time and reaches about 62% at 30min. Further extension of the illumination time does not lead to a significant increase in the dimerization degree. This indicates that the photocrosslinking of self-assembled nanoparticles was successfully achieved.

[0069] Example 5: Photothermal stability of cross-linked chiral fluorescent nanoparticles

[0070] In this example, the cross-linked chiral fluorescent nanoparticles prepared in Example 4 were transferred to a toluene solution, and the photothermal stability of their chirality and fluorescence emission properties were studied. After the cross-linked chiral fluorescent nanoparticles were transferred to a toluene solution and subjected to a high temperature treatment for 6 h, their Cotton signal remained at about 9×10 4 deg cm 2 dmol -1 This indicates that even at a high temperature of 100°C, the photocrosslinked dendritic poly(diphenylvinylene) nanoparticles can still maintain a stable helical conformation. Fig.10 a). The fluorescence spectrum shows that in the test temperature range of 10 to 80°C, the photo-crosslinked nanoparticle aqueous solution has a similar intensity of fluorescence emission ( Fig.10 b). After the photo-crosslinked nanoparticles were further exposed to different illumination times, the CD spectra and fluorescence spectra were almost identical ( Fig.11 ) indicates that the helical conformation and fluorescence emission properties of the photocross-linked nanoparticles have good photostability.

[0071] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A helical polytolane modified with a dendrite alkoxy ether, characterized in that: The polymer has polyphenylene vinylene as the main chain, branched alkoxy ether modified with cinnamate at the core point as the side group, and alanine alcohol as the connecting unit.

2. The helical polytolane modified with dendrite alkoxy ether according to claim 1, characterized in that: The structural formula of the helical polytolane modified by the branched alkoxy ether is: Wherein n=50-1000, m=1-4, R is a lower alkyl group, * indicates a connection site, and the chiral configuration of the chiral amino alcohol is R-type or S-type.

3. A method for preparing the helical polytolane modified with dendrite alkoxy ether according to claim 1, characterized in that: The polydiphenylene polymer precursor functionalized with pentafluorophenol active ester is firstly synthesized, and then combined with a branched macromolecule modified with cinnamate through an amidation reaction to obtain the branched alkoxy ether modified spiral polydiphenylene.

4. The method for preparing the helical polytolane modified by dendrite alkoxy ether according to claim 3, characterized in that: The method comprises the following steps: S1, Compound B The polymer was obtained by polymerization under the catalysis of tetraphenyltin and tungsten hexachloride. n=50~1000; S2, Compound C and Compound D Amidation reaction occurs to obtain polymer A That is, the helical polytolane modified by the branched alkoxy ether; in the structural formula of compound D, m=1-4, R is a lower alkyl group, and the chiral configuration of the chiral amino alcohol is R-type or S-type.

5. The method for preparing the helical polytolane modified by dendrite alkoxy ether according to claim 4, characterized in that: In step S1, the polymerization reaction is carried out in toluene; And / or, the molar ratio of compound B to tetraphenyltin and tungsten hexachloride is 1:5-50 and 1:10-1:100 respectively, and the reaction temperature is 80-100°C.

6. The method for preparing the helical polytolane modified by dendrite alkoxy ether according to claim 4, characterized in that: In step S2, the reaction is an amidation reaction in the presence of an organic base; And / or, the molar ratio of the polymerized units of compound C to compound D is 1:1.5-5.

7. A self-assembled aggregate, characterized in that A poor solvent is added to a solution containing the helical polytolane modified with dendrite alkoxy ether as claimed in claim 1 or 2, and self-assembly is induced by a nanoprecipitation method to obtain the self-assembled aggregate.

8. The self-assembled aggregate according to claim 7, characterized in that The selective organic solvent used in the solution of the branched alkoxy ether modified helical polytolane is a polar protic solvent; And / or, the poor solvent is water; And / or, the solution of the dendronized alkoxy ether modified helical polytolane further contains a good solvent, which is a polar aprotic solvent; and the volume ratio of the selective organic solvent, the good solvent and the poor solvent is 1:(0-4):(0.5-19).

9. The self-assembled aggregate according to claim 7 or 8, characterized in that In the solution of the helical polytolane modified by the dendronized alkoxy ether, the mass fraction of the helical polytolane modified by the dendronized alkoxy ether is 0.01-0.5 wt %.

10. A photo-crosslinked nanoparticle, characterized in that: The photo-crosslinked nanoparticles are obtained by inducing a photocyclization reaction between cinnamate esters through light irradiation of the self-assembled aggregates as claimed in claim 7.

Citation Information

Patent Citations

  • Thermo-sensitive type polyphenylacetylene and preparation method thereof

    CN104017123A

  • Temperature induced helical conformation reversible regulation type polyphenylacetylene derivatives and production method thereof

    CN104861100A

  • Thermosensitive dendronized helical polymer and preparation method thereof

    CN114891139A

  • Method for preparing temperature-sensitive dendritic macromolecular microgel through [2 +2] light ring addition reaction

    CN116655489A

  • Polyphenyleneethynylene having dendoron side chain, resin composition containing the same, luminescent coating, and luminescent sheet-like molded material

    JP2000239360A