Melamine-glutaraldehyde polycondensate microsphere and adsorption separation application thereof
Melamine-glutaraldehyde polycondensation microspheres prepared by acid-catalyzed one-pot water-phase polycondensation process solve the problems of free formaldehyde pollution and process complexity, and realize low-energy, green and environmentally friendly microsphere preparation, suitable for a variety of micropollutions The adsorption and separation of substances improves application flexibility and regeneration efficiency.
Patent Information
- Application Number
- CN202411002546.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The existing melamine formaldehyde resins have free formaldehyde contamination during the preparation and application process, which leads to health threats. The process of alternative materials such as melamine-glutaraldehyde resins is complex, has high energy consumption or uses toxic raw materials, making it difficult to achieve industrial application.
The melamine-glutaraldehyde polycondensation microspheres are prepared by acid-catalyzed one-pot water-phase polycondensation process. The process is simple and green and energy-saving. The temperature is controlled by switching between room temperature and high temperature, and the material mixing and energy consumption are balanced to prepare microspheres without free formaldehyde. , used to adsorb and separate pollutants.
Achieve low-energy consumption, green and environmentally friendly melamine-glutaraldehyde polycondensate microsphere preparation, with flexible methylene chain and triazine ring structure, suitable for adsorption and separation of micropollutants such as organic small molecules and metal ions, improving application Flexibility and regeneration efficiency.
Smart Images

Figure CN118978657A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer material engineering, and in particular to a melamine-glutaraldehyde polycondensate microsphere and an adsorption and separation application thereof. Background Art
[0002] Imine condensation is an extremely important organic reaction that can be used to synthesize amino resins, covalent organic compounds, and nano-polymer microspheres. The imine condensation of melamine and formaldehyde is often used to prepare melamine formaldehyde resin, referred to as melamine resin. Because melamine resin has excellent flame retardancy, heat resistance, and medium resistance, it has a wide range of important applications in the fields of electronic and electrical accessories, building insulation and flame retardancy, and wood-plastic composite materials. However, there is a problem of free formaldehyde pollution in the preparation and application of melamine resin. Formaldehyde has active chemical properties. The carbonyl group in its molecule can react with the amino group of amino acids to form an imine condensation reaction, which is teratogenic and mutagenic to the human body. It has been listed as a Class 1 carcinogen by the World Health Organization's International Agency for Research on Cancer. In addition, formaldehyde has a small intermolecular attraction and is a colorless gas at room temperature. Once it volatilizes freely from the melamine resin material used in construction, it will pollute the indoor air and seriously threaten human health. In recent years, as green health has become more and more popular, the application scope of melamine resin has become increasingly limited.
[0003] Glutaraldehyde is a broad-spectrum bactericide with low toxicity and fast and strong bactericidal effect. It is a highly effective disinfectant recommended by the World Health Organization and is widely used as a biocide (Advanced Materials Research, 2013, 785-786: 38-41). Thanks to its large molecular weight, the attraction between glutaraldehyde molecules is large, so its boiling point is 187-189°C, which is significantly higher than the -19.5°C of formaldehyde. It is liquid at room temperature and difficult to volatilize. Compared with free formaldehyde, its volatilization pollution is almost negligible. For this reason, some researchers use glutaraldehyde to replace part of the formaldehyde to prepare amino resins such as urea-formaldehyde and melamine to reduce the free formaldehyde therein (Polymer Engineering and Science, 2023, 63: 499-508; Colloids and Surfaces A: Physicochemical and Engineering Aspects, 2022, 648: 129019), but this cannot completely eliminate the volatilization pollution of formaldehyde. The preparation of formaldehyde-free melamine-glutaraldehyde resin materials has become a research hotspot in this field for nearly a decade. Although they are all based on imine condensation reactions, melamine-glutaraldehyde polymer materials with different structures and properties can be flexibly obtained under different process conditions and parameters. Related research has shown bright application prospects in many fields. For example, the ternary copolymer condensation product of sodium aminosulfonate, glutaraldehyde, and melamine can be used as an ideal formaldehyde-free tanning agent (Indian Journal of Chemical Technology, 2015, 22: 48–55); allowing melamine and glutaraldehyde to undergo repeated imine condensation reactions on the surface of silica can produce hyperbranched nano-dendritic macromolecules, which can be used for solid phase extraction and micro-separation of drugs (Journal of Molecular Liquids, 2023, 371: 121142). Zero-valent iron is loaded on melamine and glutaraldehyde porous polymers, which is suitable for the treatment of uranium-containing wastewater (Journal of Radioanalyticaland Nuclear Chemistry, 2020, 326: 845–855). The above-mentioned materials based on the condensation reaction of melamine and glutaraldehyde imine have not yet been industrialized due to complex processes, immature technology, and difficulties in batch manufacturing. In 2012, Lanzhou University disclosed a melamine-dialdehyde condensate and its synthesis method (CN 201210478103.X), which has great application potential in fluorescent nanomaterials and dye-sensitized solar cells; however, due to the use of a non-aqueous phase high-temperature polycondensation process, the process of this method has the characteristics of high energy consumption and organic solvent volatile pollution.In 2019, Dalian University of Technology disclosed a low-temperature (10-50°C) co-condensation process (CN 201910556107.7) of acid and alkali step-catalysis, which can be used to prepare "aromatic amine-melamine-dialdehyde polycondensate" mesocavity nano-microspheres, with the advantages of low process energy consumption and large product specific surface area. However, the aromatic amine raw materials used are highly toxic, and the acid and alkali step-catalysis process is complex, making it difficult to achieve one-pot process preparation. In addition, in 2014, Heilongjiang University disclosed a method for preparing melamine-dialdehyde porous spherical materials based on ultraviolet radiation (CN 201410169633.5), which can well overcome the problems of low pore order, poor structural stability and easy collapse of the products obtained by solvent thermal method or water bath heating method, but the method has the disadvantages of radiation pollution and difficult to control the progress of polycondensation. Summary of the invention
[0004] The invention aims to provide a melamine-glutaraldehyde polycondensate microsphere and its adsorption separation application. The melamine-glutaraldehyde polycondensate microsphere is prepared by an acid-catalyzed one-pot aqueous phase polycondensation process, which has the characteristics of simple process, green energy saving, easy control of polycondensation progress, etc., and can make up for the deficiencies of the prior art.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0006] A melamine-glutaraldehyde polycondensate microsphere, which is prepared from the following components in mass fractions:
[0007]
[0008] The acidic water refers to an aqueous solution with a hydrogen proton concentration of 0.001 to 0.01 mol / L, and the mass fraction of glutaraldehyde in the glutaraldehyde aqueous solution is 25 to 50%.
[0009] The preparation method of the melamine-glutaraldehyde polycondensate microspheres adopts a one-pot water phase mixing reaction, which is specifically as follows: at room temperature, acidic water is injected into a reaction device, and under continuous stirring conditions, a water-soluble polymer, a porogen and melamine are sequentially added into the acidic water, and after being stirred and mixed to be uniformly dispersed, the obtained suspension is heated to be transparent and clear; then the transparent and clear solution is cooled to 40-60° C., and continuously stirred, a glutaraldehyde aqueous solution is added thereto, and the mixture is uniformly mixed, and the system is subjected to constant temperature reaction at 40-60° C. for 8-12 hours, and then the material is cooled, centrifuged, purified, filtered, washed and dried to obtain the melamine-glutaraldehyde polycondensate microspheres.
[0010] Furthermore, the water-soluble polymer is one or a mixture of several of starch, dextrin, polyethylene glycol, polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl acid, polyvinyl methyl ester, polymethacrylic acid, poly-N-isopropylacrylamide, carboxymethyl cellulose, polyacrylamide, polyacrylic acid, polyacrylate, ammonium polyacrylate, sodium polyacrylate, and potassium polyacrylate.
[0011] Furthermore, the porogen is one or a mixture of several of alkyl alcohol, cycloalkyl alcohol, alkyl glycol, alkyl ammonium, alkyl diamine, alkyl ammonium salt, alkyl diamine salt, alkyl acid, alkyl diacid, alkyl acid salt, alkyl diacid salt, alkyl benzoic acid, alkyl phthalic acid, alkyl benzoate, alkyl phthalic acid, alkyl sulfonic acid, alkyl sulfonate, alkylbenzene sulfonic acid, alkylbenzene sulfonate, amino acid, betaine, glucoside, Triton, Span, quaternary ammonium salt.
[0012] Furthermore, the heating temperature is 95-100° C., and the stirring speed is 100-300 rpm.
[0013] The melamine-glutaraldehyde polycondensate microspheres provided by the present invention can be used for adsorbing and separating pollutants, such as using the microspheres for treating industrial wastewater, or for purifying, regenerating or compounding and purifying wet electronic chemicals, or for recycling, regenerating or treating leather industry wastewater.
[0014] For example, the melamine-glutaraldehyde polycondensate microspheres are used to adsorb and separate organic micropollutants, and the steps are as follows:
[0015] (1) Filling a fluidized bed column with melamine-glutaraldehyde polycondensate microspheres, installing a single bed, multiple beds in parallel, or multiple beds in series to build an adsorption separation operation system according to needs and application scenarios;
[0016] (2) introducing nitrogen gas at 100 to 200° C. into the obtained adsorption separation operation system for pretreatment;
[0017] (3) passing the sample to be treated through the adsorption separation operation system at a flow rate of 0.1 to 0.3 L / h at room temperature to obtain an eluate in which the organic micropollutants have been adsorbed and separated;
[0018] (4) After regenerating and activating the fluidized bed column with steam at 100-200°C, the adsorption separation operation system is recycled.
[0019] For another example, the melamine-glutaraldehyde polycondensate microspheres are used to adsorb and separate metal ions or their derivative forms, and the steps are as follows:
[0020] (1) Filling a fluidized bed column with melamine-glutaraldehyde polycondensate microspheres, installing a single bed, multiple beds in parallel, or multiple beds in series to build an adsorption separation operation system according to needs and application scenarios;
[0021] (2) introducing a gas at 100 to 200° C. into the obtained adsorption separation operation system for pretreatment;
[0022] (3) passing the sample to be treated through the adsorption separation operation system at a flow rate of 0.02 to 0.2 L / h at room temperature to obtain an eluent in which the metal ions and the derivatives have been adsorbed and separated;
[0023] (4) After regenerating and activating the fluidized bed column with nitric acid, hydrochloric acid, phosphoric acid or sulfuric acid solution, the adsorption separation operation system is recycled.
[0024] The significant advantages of the present invention are: (1) an acid-catalyzed one-pot aqueous phase polycondensation process is adopted, which has the characteristics of simple process, green environmental protection, and easy control of polycondensation progress; (2) the temperature is controlled by switching between normal temperature, high temperature (95-100°C), and low temperature (40-60°C), which can effectively balance the contradiction between material mixing and reducing energy consumption, so that the overall energy consumption is lower than that of the traditional method using continuous high-temperature mixing and reaction; (3) the melamine-glutaraldehyde polycondensate microspheres obtained by implementing the method of the present invention do not contain free formaldehyde, have flexible methylene chains and triazine ring structures that ordinary melamine resins do not have, and have bright application prospects in the adsorption and separation of micropollutants such as small organic molecules and metal ions; (4) the melamine-glutaraldehyde polycondensate microspheres provided by the present invention are "unitized or modularized" and filled into a fluidized bed column and then connected in series or in parallel for application. Compared with the traditional filling column method, it can not only improve its flexible adaptability in different application scenarios, but also be more conducive to parallel operation and save time and energy consumption for recycling and regeneration. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is an optical microscope image of the monodisperse melamine-glutaraldehyde polycondensate microspheres obtained in Example 1.
[0026] Figure 2 This is an optical microscope image of the monodisperse melamine-glutaraldehyde polycondensate microspheres obtained in Example 2.
[0027] Figure 3 This is an optical microscope image of the monodisperse melamine-glutaraldehyde polycondensate microspheres obtained in Example 3.
[0028] Figure 4 This is an optical microscope image of the monodisperse melamine-glutaraldehyde polycondensate microspheres obtained in Example 4.
[0029] Figure 5 This is an optical microscope image of the monodisperse melamine-glutaraldehyde polycondensate microspheres obtained in Example 5.
[0030] Figure 6 This is an optical microscope image of the monodisperse melamine-glutaraldehyde polycondensate microspheres obtained in Example 6.
[0031] Figure 7 This is an optical microscope image of the monodisperse melamine-glutaraldehyde polycondensate microspheres obtained in Example 7.
[0032] Figure 8 This is an optical microscope image of the monodisperse melamine-glutaraldehyde polycondensate microspheres obtained in Example 8.
[0033] Fig. 9 This is an optical microscope image of the monodisperse melamine-glutaraldehyde polycondensate microspheres obtained in Example 9.
[0034] Fig.10 This is an optical microscope image of the monodisperse melamine-glutaraldehyde polycondensate microspheres obtained in Example 10.
[0035] Fig.11 This is the infrared absorption spectrum of the melamine-glutaraldehyde polycondensate microspheres obtained in Example 1.
[0036] Fig.12 It is the structural unit of melamine-glutaraldehyde condensation polymer microspheres. DETAILED DESCRIPTION
[0037] The present invention is described in more detail below through specific examples, but the present invention is not limited thereto.
[0038] Example 1
[0039] At room temperature of 25°C, 1000 g of acidic water containing a hydrogen proton concentration of 0.001 mol / L, i.e., a pH value of 3, was injected into a 3-liter round-bottom three-necked flask. At a set speed of 100 rpm, 6 g of polyvinyl alcohol, 1 g of n-butanol and 20.2 g of melamine were added to the acidic water in sequence in a continuous stirring manner. After being stirred and mixed to be uniformly dispersed, the suspension was heated to 95°C to make the obtained suspension transparent and clear. The transparent and clear liquid was then cooled to a set temperature of 55°C, and 101.2 g (i.e., 95.2 mL) of 50% glutaraldehyde (density 1.063 g / cm 3 ) aqueous solution, mix them evenly and allow the system to react at the set temperature for 12 hours, then cool the material, centrifuge, purify by filtration, wash and dry to obtain melamine-glutaraldehyde condensation polymer microspheres 1 (MA-GA condensation polymer microspheres 1).
[0040] Example 2
[0041] At room temperature of 25°C, 1000 g of acidic water containing a hydrogen proton concentration of 0.01 mol / L, i.e., a pH value of 2, was injected into a 3-liter round-bottom three-necked flask. At a set speed of 300 rpm, 6 g of polyvinyl alcohol and 20.2 g of melamine were added to the acidic water in sequence in a continuous stirring manner. After being stirred and mixed to be uniformly dispersed, the suspension was heated to 100°C to make the obtained suspension transparent and clear. The transparent and clear liquid was then cooled to a set temperature of 60°C, and 118.0 g (i.e., 111 mL) of 50% glutaraldehyde (density 1.063 g / cm 3 ) aqueous solution, mix well and allow the system to react at the set temperature for 8 hours, cool the material, centrifuge, purify by filtration, wash and dry to obtain melamine-glutaraldehyde condensation polymer microspheres 2 (MA-GA condensation polymer microspheres 2).
[0042] Example 3
[0043] At room temperature of 25°C, 1000 g of acidic water containing a hydrogen proton concentration of 0.0036 mol / L, i.e., a pH value of 2.5, was injected into a 3-liter round-bottom three-necked flask, and 3 g of polyvinyl alcohol, 0.001 g of Triton and 20.2 g of melamine were added to the acidic water in sequence under a set speed of 200 rpm in a continuous stirring manner, and after being stirred and mixed to be uniformly dispersed, the suspension was heated to 97.5°C to make the obtained suspension transparent and clear; the transparent and clear liquid was then cooled to a set temperature of 57.5°C, and 118.0 g (i.e., 111 mL) of 50% glutaraldehyde (density 1.063 g / cm 3 ) aqueous solution, mix well and allow the system to react at the set temperature for 10 hours, cool the material, centrifuge, purify by filtration, wash and dry to obtain melamine-glutaraldehyde condensation polymer microspheres 3 (MA-GA condensation polymer microspheres 3).
[0044] Example 4
[0045] At room temperature of 28° C., 1000 g of acidic water containing a hydrogen proton concentration of 0.0036 mol / L, i.e., a pH value of 2.5, was injected into a 3-liter round-bottom three-necked flask, and a mixture of 4 g of polyvinyl alcohol, 0.1 g of polyethylene glycol and 0.4 g of β-cyclodextrin, 15 g of sodium dodecylbenzenesulfonate and 20.2 g of melamine were added to the acidic water in sequence under a set speed of 200 rpm in a continuous stirring manner, and after being stirred and mixed to be uniformly dispersed, the mixture was heated to 95° C. to make the resulting suspension transparent and clear; the transparent and clear liquid was then cooled to a set temperature of 57.5° C., and 109.7 g (i.e., 103.2 mL) of 50% glutaraldehyde (density 1.063 g / cm 3) aqueous solution, mix well and allow the system to react at the set temperature for 10 hours, cool the material, centrifuge, purify by filtration, wash and dry to obtain melamine-glutaraldehyde condensation polymer microspheres 4 (MA-GA condensation polymer microspheres 4).
[0046] Example 5
[0047] At room temperature of 35° C., 1000 g of acidic water containing a hydrogen proton concentration of 0.001 mol / L, i.e., a pH value of 3, was injected into a 3-liter round-bottom three-necked flask. 6 g of polyvinyl alcohol, a porogen prepared by mixing 0.3 g of aspartic acid, 0.2 g of p-toluic acid, and 0.1 g of hexadecyltrimethylammonium bromide, and 20.2 g of melamine were added to the acidic water in sequence under a set speed of 100 rpm and continuously stirred. After being stirred and mixed to be uniformly dispersed, the mixture was heated to 95° C. to make the obtained suspension transparent and clear. The transparent and clear liquid was then cooled to a set temperature of 55° C., and 101.2 g (i.e., 95.2 mL) of 50% glutaraldehyde (density 1.063 g / cm 3 ) aqueous solution, mix well and allow the system to react at the set temperature for 12 hours, cool the material, centrifuge, purify by filtration, wash and dry to obtain melamine-glutaraldehyde condensation polymer microspheres 5 (MA-GA condensation polymer microspheres 5).
[0048] Example 6
[0049] At room temperature of 30°C, 1000 g of acidic water containing a hydrogen proton concentration of 0.002 mol / L, i.e., a pH value of 2.7, was injected into a 3-liter round-bottom three-necked flask, and 20 g of polyvinyl alcohol and 30.8 g of melamine were added to the acidic water in sequence under a setting speed of 250 rpm in a continuous stirring manner. After being stirred and mixed to be uniformly dispersed, the suspension was heated to 98°C to make the obtained suspension transparent and clear; the transparent and clear liquid was then cooled to a setting temperature of 40°C, and 201.8 g (i.e., 190.4 mL) of 25% glutaraldehyde (density 1.06 g / cm 3 ) aqueous solution, mix evenly and allow the system to react at the set temperature for 24 hours, cool the material, centrifuge, purify by filtration, wash and dry to obtain melamine-glutaraldehyde condensation polymer microspheres 6 (MA-GA condensation polymer microspheres 6).
[0050] Example 7
[0051] At room temperature of 20°C, 1000 g of acidic water containing a hydrogen proton concentration of 0.001 mol / L, i.e., a pH value of 3, was injected into a 3-liter round-bottom three-necked flask, and 12 g of polyvinyl alcohol, 2.2 g of Triton and 50.5 g of melamine were added to the acidic water in sequence under a setting speed of 100 rpm in a continuous stirring manner. After being stirred and mixed to be uniformly dispersed, the suspension was heated to 95°C to make the obtained suspension transparent and clear; the transparent and clear liquid was then cooled to a set temperature of 50°C, and 189.3 g (i.e., 178.6 mL) of 25% glutaraldehyde (density 1.06 g / cm 3 ) aqueous solution, mix well and allow the system to react at the set temperature for 16 hours, cool the material, centrifuge, purify by filtration, wash and dry to obtain melamine-glutaraldehyde condensation polymer microspheres 7 (MA-GA condensation polymer microspheres 7).
[0052] Example 8
[0053] At room temperature of 28°C, 1000 g of acidic water containing a hydrogen proton concentration of 0.001 mol / L, i.e., a pH value of 3, was injected into a 3-liter round-bottom three-necked flask, and 6 g of polyvinyl alcohol, 0.9 g of lauryl dimethylamine oxide and 20.2 g of melamine were added to the acidic water in sequence under a set speed of 200 rpm in a continuous stirring manner. After being stirred and mixed to be uniformly dispersed, the suspension was heated to 95°C to make the obtained suspension transparent and clear; the transparent and clear liquid was then cooled to a set temperature of 55°C, and 201.8 g (i.e., 190.4 mL) of 25% glutaraldehyde (density 1.06 g / cm 3 ) aqueous solution, mix them evenly and allow the system to react at the set temperature for 12 hours, then cool the material, centrifuge, purify by filtration, wash and dry to obtain melamine-glutaraldehyde condensation polymer microspheres 8 (MA-GA condensation polymer microspheres 8).
[0054] Example 9
[0055] At room temperature of 20°C, 1000 g of acidic water containing a hydrogen proton concentration of 0.01 mol / L, i.e., a pH value of 2, was injected into a 3-liter round-bottom three-necked flask, and 6 g of polyvinyl alcohol, 3 g of sodium dodecyl sulfate and 20.2 g of melamine were added to the acidic water in sequence under a set speed of 300 rpm in a continuous stirring manner. After being stirred and mixed to be uniformly dispersed, the suspension was heated to 95°C to make the obtained suspension transparent and clear; the transparent and clear liquid was then cooled to a set temperature of 60°C, and 117.7 g (i.e., 111.0 mL) of 25% glutaraldehyde (density 1.06 g / cm 3) aqueous solution, mix them evenly and allow the system to react at the set temperature for 8 hours, then cool the material, centrifuge, purify by filtration, wash and dry to obtain melamine-glutaraldehyde condensation polymer microspheres 9 (MA-GA condensation polymer microspheres 9).
[0056] Example 10
[0057] At room temperature of 25°C, 1000 g of acidic water containing a hydrogen proton concentration of 0.01 mol / L, i.e., a pH value of 2, was injected into a 3-liter round-bottom three-necked flask, and a mixture of 5.7 g of polyvinyl alcohol, 0.1 g of sodium polyacrylate and 0.2 g of polyethylene glycol, 3 g of hexadecyltrimethylammonium bromide and 20.2 g of melamine were added to the acidic water in sequence under a set speed of 300 rpm in a continuous stirring manner, and after being stirred and mixed to be uniformly dispersed, the mixture was heated to 97.5°C to make the resulting suspension transparent and clear; the transparent and clear liquid was then cooled to a set temperature of 60°C, and 117.7 g (i.e., 111.0 mL) of 25% glutaraldehyde (density 1.06 g / cm 3 ) aqueous solution, mix them evenly and allow the system to react at the set temperature for 8 hours, then cool the material, centrifuge, purify by filtration, wash and dry to obtain melamine-glutaraldehyde condensation polymer microspheres 10 (MA-GA condensation polymer microspheres 10).
[0058] The morphology of the melamine-glutaraldehyde polycondensate microspheres obtained in Examples 1 to 10 was observed using an optical microscope (XSP-10CA, Shanghai Youke Instrument Co., Ltd.). Figures 1 to 10 . It can be seen from these figures that according to the method of the present invention, by carrying out an acid-catalyzed one-pot aqueous phase polycondensation reaction in accordance with the process parameters described in Examples 1 to 10, melamine-glutaraldehyde polycondensation microspheres can be obtained. Moreover, the particle size of the obtained microspheres will vary with the process parameters of each embodiment, fluctuating between 2 and 12 μm. This result shows that the method of the present invention can achieve the regulation of the progress of the polycondensation reaction by flexibly adjusting the process parameters to prepare melamine-glutaraldehyde polycondensation microspheres of different particle sizes.
[0059] The infrared absorption activity of melamine-glutaraldehyde polycondensate microspheres 1 was investigated using a Fourier transform infrared spectrometer (NICOLET iS50, Thermo Fisher Scientific). Fig.11 . At 3370cm -1 There are overlapping peaks of OH stretching of hydroxyl group and NH stretching of amine group; at 2945cm -1 , 2958cm -1 , 1458cm -1 and 1354cm -1The positions are successively assigned to the methylene group (-CH 2 -) CH antisymmetric stretching, symmetric stretching, antisymmetric bending and symmetric bending vibration absorption peaks; at 1578cm -1 、1564cm -1 and 813cm -1 The characteristic absorption peak at 2738cm -1 、1721cm -1 and 591cm -1 The absorption peaks at 1497 cm-1 are attributed to the CH stretching, C=O stretching, and the in-plane bending absorption peaks of CC(CO) connected to the aldehyde group. -1 There is an NH deformation absorption peak of aromatic secondary amine at 1164cm -1 and 1007cm -1 The two stretching absorption peaks are respectively attributed to the CN bond and the CO bond. The infrared spectrum test results show that the melamine-glutaraldehyde polycondensate microspheres 1 have the following characteristics: Fig.12 The structural unit shown.
[0060] Application Examples
[0061] Melamine-glutaraldehyde polycondensate microspheres (MA-GA polycondensate microspheres) were used to adsorb and separate methylene blue and chromium ions. The test results are shown in Table 1.
[0062] The adsorption and separation test of methylene blue was carried out according to the following steps: 2 to 5 grams of MA-GA polycondensation microspheres were filled into a fluidized bed column with a diameter of 2 to 5 cm and a height of 2 to 4 cm; 3 to 12 fluidized bed columns of the same size were prepared in parallel, and connected in series or in parallel according to actual needs to build an organic micropollutant adsorption and separation operation system; nitrogen gas at 100 to 200° C. was introduced into the constructed adsorption and separation operation system for heat treatment for 12 to 4 hours, and then cooled to room temperature; 0.8 to 4.2 liters of 100 mg / L methylene blue sample was passed through the constructed adsorption and separation operation system at a flow rate of 0.1 to 0.3 L / h at room temperature, the eluate was collected and the concentration of methylene blue was detected using an ultraviolet-visible spectrophotometer (T6 New Century, Beijing Puxi General Instrument Co., Ltd.), and whether the concentration of methylene blue in the eluate was lower than the detection limit of the spectrophotometer was examined. If it was lower than the detection limit, it was deemed that methylene blue was not detected. After regenerating and activating the fluidized bed column with 3 to 12 L of water vapor at 100 to 200°C, perform the same methylene blue elution experiment according to the aforementioned method in the same adsorption separation operation system, repeat 3 times, and test and determine whether methylene blue is detected in the eluent.
[0063] The chromium ion adsorption and separation test was carried out according to the following steps: 2 to 5 grams of MA-GA polycondensation microspheres were filled into a fluidized bed column with a diameter of 2 to 5 cm and a height of 2 to 4 cm; 3 to 12 fluidized bed columns of the same size were prepared in parallel, and connected in series or in parallel according to actual needs to build a metal ion micropollutant adsorption and separation operation system; nitrogen gas at 100 to 200° C. was introduced into the constructed adsorption and separation operation system for heat treatment for 12 to 4 hours, and then cooled to room temperature; 0.8 to 4.7 liters of 10 mg / L potassium dichromate (AR, Sinopharm Chemical Reagent Co., Ltd.) aqueous solution with a pH of 1 to 10, referred to as chromium solution sample, was passed through the constructed adsorption and separation operation system at a flow rate of 0.02 to 0.2 L / h, and the eluent was collected and the chromium content was detected using ICP-MS (ICAP Qc, Thermo Fisher Scientific), and the chromium removal rate (R) was calculated according to the following formula: R = (C 0 -C) / C 0 × 100%, where C 0 is the chromium concentration before elution of the chromium solution sample (mg / L); C is the chromium concentration after elution of the chromium solution sample (mg / L); after washing and regenerating the activated fluidized bed column with 0.05-0.2 mol / L nitric acid, hydrochloric acid, phosphoric acid or sulfuric acid solution, the adsorption separation operation system is recycled, and the same chromium elution experiment is performed according to the aforementioned method in the same adsorption separation operation system, repeated 3 times, and the chromium content before and after elution is detected by ICP-MS, and the chromium removal rate (R) is calculated.
[0064] Table 1 Experimental results of separation of methylene blue and chromium ions by melamine-glutaraldehyde polycondensate microspheres
[0065]
[0066]
[0067] As shown in Table 1, the melamine-glutaraldehyde polycondensate microspheres 1-10 (MA-GA polycondensate microspheres 1-10) obtained by implementing the method of the present invention are applied according to the application method provided by the present invention, and not only have a removal rate of 74.9-99.9% for 10 mg / L chromium ions, but also have an adsorption removal rate of nearly 100% for 100 mg / L methylene blue, that is, the residual amount of methylene blue in the eluent is lower than the detection limit of the ultraviolet visible spectrophotometer. In addition, the removal capacity of MA-GA polycondensate microspheres 1-10 for 10 mg / L chromium ions after 1 or 2 regenerations is no different from that when they were first used, and they are also no different from that when they were first used after 1, 2 or 3 regenerations. The above results show that the MA-GA polycondensate microspheres provided by the method of the present invention have good adsorption and separation performance for two simulated industrial micropollutants, methylene blue and chromium ions, and the performance can also be regenerated and activated multiple times without significant degradation.
Claims
1. A melamine-glutaraldehyde polycondensate microsphere, characterized in that: It is prepared from the following components in mass fractions: 100 parts of acidic water Water-soluble polymer 0.3~2.0 parts Porogen 0~1.5 parts Melamine 2.02~5.05 parts 5.06~20.18 parts of glutaraldehyde aqueous solution.
2. The melamine-glutaraldehyde polycondensate microspheres according to claim 1, characterized in that: The acidic water refers to an aqueous solution with a hydrogen proton concentration of 0.001 to 0.01 mol / L, and the mass fraction of glutaraldehyde in the glutaraldehyde aqueous solution is 25 to 50%.
3. The method for preparing melamine-glutaraldehyde polycondensate microspheres according to claim 1 or 2, characterized in that: At room temperature, acidic water is injected into the reaction equipment, and under continuous stirring, a water-soluble polymer, a porogen and melamine are added to the acidic water in sequence, and after being stirred and mixed to be uniformly dispersed, the obtained suspension is heated to be transparent and clear; then the transparent and clear solution is cooled to 40-60° C., and the stirring is continued continuously, and a glutaraldehyde aqueous solution is added thereto, and the mixture is uniformly mixed, and the system is subjected to constant temperature reaction at 40-60° C. for 8-12 hours, and then the material is cooled, centrifuged, purified, filtered, washed and dried to obtain melamine-glutaraldehyde polycondensate microspheres.
4. The method for preparing melamine-glutaraldehyde polycondensate microspheres according to claim 3, characterized in that: The water-soluble polymer is one or a mixture of starch, dextrin, polyethylene glycol, polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl acid, polyvinyl methyl ester, polymethacrylic acid, poly-N-isopropylacrylamide, carboxymethyl cellulose, polyacrylamide, polyacrylic acid, polyacrylate, ammonium polyacrylate, sodium polyacrylate, potassium polyacrylate.
5. The method for preparing melamine-glutaraldehyde polycondensate microspheres according to claim 3, characterized in that: The porogen is one or a mixture of several of alkyl alcohol, cycloalkyl alcohol, alkyl glycol, alkyl ammonium, alkyl diamine, alkyl ammonium salt, alkyl diamine salt, alkyl acid, alkyl diacid, alkyl acid salt, alkyl diacid salt, alkyl benzoic acid, alkyl phthalic acid, alkyl benzoate, alkyl phthalic acid, alkyl sulfonic acid, alkyl sulfonate, alkylbenzene sulfonic acid, alkylbenzene sulfonate, amino acid, betaine, glucoside, Triton, Span, quaternary ammonium salt.
6. The method for preparing melamine-glutaraldehyde polycondensate microspheres according to claim 3, characterized in that: The heating temperature is 95-100°C.
7. The method for preparing melamine-glutaraldehyde polycondensate microspheres according to claim 3, characterized in that: The stirring speed is 100-300 rpm.
8. Use of melamine-glutaraldehyde polycondensate microspheres obtained according to the preparation method according to any one of claims 3 to 7 in the adsorption and separation of pollutants.
9. The use according to claim 8, characterized in that: The melamine-glutaraldehyde polycondensate microspheres are used to adsorb and separate organic micropollutants, and the steps are as follows: (1) Fill the fluidized bed column with melamine-glutaraldehyde polycondensate microspheres, and install a single bed, multiple beds in parallel, or multiple beds in series to build an adsorption separation operation system according to needs and application scenarios; (2) introducing nitrogen gas at 100-200° C. into the obtained adsorption separation operation system for pretreatment; (3) Passing the sample to be treated through the adsorption separation operation system at a flow rate of 0.1-0.3 L / h at room temperature to obtain an eluent in which the organic micropollutants have been adsorbed and separated; (4) After regenerating and activating the fluidized bed column with steam at 100-200°C, the adsorption separation operation system is recycled.
10. The use according to claim 8, characterized in that: The melamine-glutaraldehyde polycondensate microspheres are used to adsorb and separate metal ions or their derivative forms, and the steps are as follows: (1) Fill the fluidized bed column with melamine-glutaraldehyde polycondensate microspheres, and install a single bed, multiple beds in parallel, or multiple beds in series to build an adsorption separation operation system according to needs and application scenarios; (2) introducing nitrogen gas at 100-200° C. into the obtained adsorption separation operation system for pretreatment; (3) Passing the sample to be processed through the adsorption separation operation system at a flow rate of 0.02-0.2 L / h at room temperature to obtain an eluent in which the metal ions and derivatives have been adsorbed and separated; (4) After regenerating and activating the fluidized bed column with nitric acid, hydrochloric acid, phosphoric acid or sulfuric acid solution, the adsorption separation operation system is recycled.
Citation Information
Patent Citations
Ultraviolet radiation-based method for preparing porous spherical material
CN103920435A
Heteroatom doped polymer nano-microsphere and preparation method thereof
CN108822274A
Melamine-thiourea modified soybean protein microsphere, preparation method thereof, and application of melamine-thiourea modified soybean protein microsphere in cadmium adsorption and detection
CN110665476A
Preparation method of large-particle-size melamino-formaldehyde resin microspheres
CN111303363A
Synthesis and application of formaldehyde free melamine glutaraldehyde amino resin as an effective retanning agent
US20170058073A1