Preparation method of waterproof high polymer material

By introducing hydrophobic long chains and fluorine atoms into the aqueous polyurethane, combining specific monomer reactions to form aqueous polyurethanes with high hydrophobic properties, the problem of poor mechanical properties of pure aqueous polyurethanes is solved, and its tensile strength and waterproof properties are significantly improved.

CN118978659APending Publication Date: 2024-11-19NANJING COLLEGE OF CHEM TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411143756.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The linear structure and low crosslinking density of pure water-based polyurethane lead to poor water resistance, heat resistance and mechanical properties of the adhesive film, limiting its application range.

Method used

By introducing hydrophobic long chains and fluorine atoms into aqueous polyurethane, phytools are used as starting materials to carry out epoxidation and fluorine ring opening reactions, combining isophorone diisocyanate, polyether polyol and dibutyltin dilaurate and other monomers. , forming aqueous polyurethane with high hydrophobic properties.

Benefits of technology

It significantly improves the hydrophobic properties of polyurethane, enhances its tensile strength and elongation at break, and improves its mechanical and waterproof properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a waterproof high polymer material, which comprises the following steps: S1, adding phytol into a flask, slowly dropwise adding a mixed solution of formic acid and hydrogen peroxide by taking strong acid ion exchange resin as a catalyst, stirring at 78-85 DEG C for reaction after dropwise adding is finished, filtering to remove the catalyst, washing with saturated saline solution to be neutral, and drying to obtain phytol; performing vacuum rotary evaporation to obtain epoxidized phytol; s2, adding the epoxidized phytol obtained in S1 into cyclohexane, adding HBF4 and excessive fluoroalkyl alcohol, stirring at room temperature for reaction, adding alkali liquor to neutralize the HBF4 after the reaction is finished, drying with anhydrous sodium sulfate, and performing rotary evaporation to remove excessive fluoroalkyl alcohol to obtain the fluorine-substituted open-loop phytol. The fluorine-substituted ring-opening phytol is added in the preparation route of the polyurethane high polymer material, so that the hydrophobic property of the polyurethane high polymer material is improved, the polyurethane high polymer material has excellent tensile strength and elongation at break, and the mechanical property and the waterproof property are obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a method for preparing a waterproof polymer material. Background Art

[0002] Water entering a building will directly affect its function and lifespan. The waterproofing works that come from it can be roughly divided into structural waterproofing and material waterproofing according to the mode of action. Coating waterproof coating is a type of film waterproofing, which belongs to material waterproofing. Waterproof coating is suitable for the surface of the structure. After the liquid coating dries and solidifies, it forms a continuous coating of a certain thickness with waterproof, anti-seepage and moisture-proof functions. The waterproof coating is liquid and easy to use. It is less affected by the surface size and geometric dimensions of the structure during construction. It does not require heating. It dries and solidifies to form a coating that isolates moisture from the surface of the building. With the advancement of urbanization, the demand for waterproof coatings is also increasing.

[0003] Waterborne polyurethane is a high-performance, environmentally friendly, high-molecular elastic waterproof material that is safe, environmentally friendly, non-toxic, and odorless. It has good adhesion on the surfaces of cement-based, stone-based, metal and other substrates. However, pure waterborne polyurethane has a linear structure and a low cross-linking density, which leads to poor water resistance, heat resistance and film mechanical properties. Therefore, in order to make up for the defects, improve material performance and expand the application range of waterborne polyurethane, it is necessary to chemically modify the waterborne polyurethane. Common modification methods include cross-linking modification, epoxy resin modification, silicone modification, acrylate modification, and nanoparticle modification.

[0004] The invention provides a monomer required in the synthesis process of preparing waterborne polyurethane using plant alcohol as a starting material, and the hydrophobic property of the waterborne polyurethane is improved by introducing hydrophobic long chains and fluorine atoms into the waterborne polyurethane. Summary of the invention

[0005] 1. Technical problems to be solved: In view of the above technical problems, the present invention provides a method for preparing a waterproof polymer material.

[0006] 2. Technical solution: A method for preparing a waterproof polymer material comprises the following steps: S1: Add plant alcohol into a flask, use a strongly acidic ion exchange resin as a catalyst, slowly drop a mixture of formic acid and hydrogen peroxide, stir and react at 78-85°C after the dropwise addition is completed, filter to remove the catalyst, wash with saturated brine until neutral, and vacuum rotary evaporate to obtain epoxidized plant alcohol; S2: adding the epoxidized plant alcohol obtained in S1 to cyclohexane, adding HBF4 and an excess of fluoroalkyl alcohol, stirring and reacting at room temperature, adding alkaline solution to neutralize HBF4 after the reaction, drying with anhydrous sodium sulfate and removing excess fluoroalkyl alcohol by rotary evaporation to obtain fluorine-substituted open-ring plant alcohol; S3: adding isophorone diisocyanate, polyether polyol, dibutyltin dilaurate and the fluorine-substituted open-ring plant alcohol obtained in S2 to acetone, stirring and reacting at 50-55° C. under a nitrogen atmosphere, adding dimethylolpropionic acid after cooling to room temperature, continuing to stir and react at 50-55° C., adding triethylamine after the reaction is completed, and then adding deionized water, and evaporating the acetone to obtain an emulsion; S4: Add the emulsion into the mold, air-dry at room temperature, and then place it in a drying oven at 45-55°C, and then demould to obtain a waterproof polymer film.

[0007] Furthermore, the addition amount of the strong acid ion exchange resin catalyst in S1 is 1-3% of the mass of the plant alcohol, and the molar ratio of the plant alcohol, formic acid and H2O2 in hydrogen peroxide is 1:0.25-0.3:3-5.

[0008] Furthermore, the reaction time of S1 is 5-7h, and the temperature of the vacuum rotary evaporation is 75-80°C.

[0009] Furthermore, the mass of HBF4 added to S2 is 5%-10% of the epoxidized plant alcohol, the molar ratio of fluoroalkyl alcohol to epoxidized plant alcohol is 1:1-1.2, and the reaction time is 1-3h.

[0010] Furthermore, the mass of cyclohexane in S2 is 3-5 times that of epoxidized plant alcohol.

[0011] Furthermore, the fluoroalkyl alcohol in S2 is one of trifluoroethanol, trifluoropropanol and trifluoroisopropanol.

[0012] Furthermore, the molecular weight of the polyether polyol in S3 is 1000, the hydroxyl value is 107-117 mg KOH / g, the molar ratio of isophorone diisocyanate, polyether polyol, fluorine-substituted open-ring plant alcohol and dihydroxymethylpropionic acid is 1-1.3:0.4-0.5:0.2-0.3:0.4-0.5, and the ratio of isophorone diisocyanate and dibutyltin dilaurate is 1 g:20-25 μL.

[0013] Furthermore, the amount of acetone added in S3 is 5-10 times the mass of isophorone diisocyanate.

[0014] Furthermore, the amount of deionized water added in S3 is 5-10 times the mass of isophorone diisocyanate.

[0015] Furthermore, the molar ratio of triethylamine to dimethylolpropionic acid in S3 is 1:1.

[0016] 3. Beneficial effects: The present invention adds fluorine-substituted open-ring plant alcohols to the preparation route of polyurethane polymer materials. The fluorine-substituted open-ring plant alcohols are obtained by epoxidizing plant alcohols and then further reacting them with fluoroalkyl alcohols for open-ring addition. Since the polyurethane polymer materials contain hydrophobic long alkyl chains and fluorine atoms, the hydrophobic properties of the polyurethane polymer materials are increased, and the materials have excellent tensile strength and elongation at break, and their mechanical properties and waterproof properties are significantly improved. DETAILED DESCRIPTION

[0017] The present invention is described in detail below.

[0018] Embodiment 1: A method for preparing a waterproof polymer material comprises the following steps: S1: 10g of plant alcohol (MW.296.53, purity 98%) was added into a flask, 0.1g of a strongly acidic ion exchange resin was added as a catalyst, 318mL of a mixture of formic acid and 7mL of 50%wt hydrogen peroxide was slowly added dropwise, after the addition was completed, the mixture was stirred at 80°C for 6h, the catalyst was filtered to remove, the mixture was washed with saturated brine until neutral, and 10.3g of epoxidized plant alcohol was obtained by vacuum rotary evaporation at 80°C; S2: Add the epoxidized plant alcohol obtained in S1 to 40g of cyclohexane, add 6g of HBF4 and 3.5g of fluoroethanol, stir at room temperature for 2h, add sodium bicarbonate solution to neutralize HBF4 after the reaction, dry with anhydrous sodium sulfate and remove excess fluoroethanol by rotary evaporation to obtain 13.5g of fluorine-substituted open-ring plant alcohol; S3: 5.4 g of isophorone diisocyanate, 9.7 g of polyether polyol (MW.1000, hydroxyl value: 107-117 mgKOH / g), 110 μL of dibutyltin dilaurate and 2 g of fluorine-substituted open-ring plant alcohol obtained in S2 were added to 50 g of acetone, stirred and reacted at 55°C for 30 min under a nitrogen atmosphere, and then 1.3 g of dimethylolpropionic acid was added after cooling to room temperature, and the reaction was continued at 55°C for 3 h with stirring. After the reaction was completed, triethylamine was added, and then deionized water was added, and the acetone was evaporated to obtain an emulsion; S4: Add the emulsion into the mold, air-dry at room temperature, and then place it in a drying oven at 45-55°C, and then demould to obtain a waterproof polymer film.

[0019] Embodiment 2: A method for preparing a waterproof polymer material comprises the following steps: S1 and S2 are the same as in Example 1, S3: 4.7 g of isophorone diisocyanate, 8.1 g of polyether polyol (MW.1000, hydroxyl value: 107-117 mgKOH / g), 110 μL of dibutyltin dilaurate and 2 g of fluorine-substituted open-ring plant alcohol obtained in S2 were added to 50 g of acetone, stirred and reacted at 55°C for 30 min under a nitrogen atmosphere, and then 1.1 g of dimethylol propionic acid was added after cooling to room temperature, and the reaction was continued at 55°C for 3 h with stirring. After the reaction was completed, triethylamine was added, and then deionized water was added, and the acetone was evaporated to obtain an emulsion; S4: Add the emulsion into the mold, air-dry at room temperature, and then place it in a drying oven at 45-55°C, and then demould to obtain a waterproof polymer film.

[0020] Embodiment 3: A method for preparing a waterproof polymer material comprises the following steps: S1: 10g of plant alcohol (MW.296.53, purity 98%) was added into a flask, 0.1g of a strongly acidic ion exchange resin was added as a catalyst, 318mL of a mixture of formic acid and 7mL of 50%wt hydrogen peroxide was slowly added dropwise, after the addition was completed, the mixture was stirred at 80°C for 6h, the catalyst was filtered to remove, the mixture was washed with saturated brine until neutral, and 10.3g of epoxidized plant alcohol was obtained by vacuum rotary evaporation at 80°C; S2: Add the epoxidized plant alcohol obtained in S1 to 40g of cyclohexane, add 6g of HBF4 and 3.76g of fluoropropanol, stir at room temperature for 2h, add sodium bicarbonate solution to neutralize HBF4 after the reaction, dry with anhydrous sodium sulfate and remove excess fluoroethanol by rotary evaporation to obtain 13.9g of fluorine-substituted open-ring plant alcohol; S3: 5.4 g of isophorone diisocyanate, 9.7 g of polyether polyol (MW.1000, hydroxyl value: 107-117 mgKOH / g), 110 μL of dibutyltin dilaurate and 2.07 g of fluorine-substituted open-ring plant alcohol obtained in S2 were added to 50 g of acetone, stirred and reacted at 55°C for 30 min under a nitrogen atmosphere, and then 1.3 g of dimethylol propionic acid was added after cooling to room temperature, and the reaction was continued at 55°C for 3 h with stirring. After the reaction was completed, triethylamine was added, and then deionized water was added, and the acetone was evaporated to obtain an emulsion; S4: Add the emulsion into the mold, air-dry at room temperature, and then place it in a drying oven at 45-55°C, and then demould to obtain a waterproof polymer film.

[0021] Embodiment 4: A method for preparing a waterproof polymer material comprises the following steps: S1: 10g of plant alcohol (MW.296.53, purity 98%) was added into a flask, 0.1g of a strongly acidic ion exchange resin was added as a catalyst, 318mL of a mixture of formic acid and 7mL of 50%wt hydrogen peroxide was slowly added dropwise, after the addition was completed, the mixture was stirred at 80°C for 6h, the catalyst was filtered to remove, the mixture was washed with saturated brine until neutral, and 10.3g of epoxidized plant alcohol was obtained by vacuum rotary evaporation at 80°C; S2: Add the epoxidized plant alcohol obtained in S1 to 40g of cyclohexane, add 6g of HBF4 and 3.76g of fluoroisopropanol, and react at room temperature for 2h with stirring. After the reaction, add sodium bicarbonate solution to neutralize HBF4, dry with anhydrous sodium sulfate, and then remove excess fluoroethanol by rotary evaporation to obtain 13.9g of fluorine-substituted open-ring plant alcohol; S3: 5.4 g of isophorone diisocyanate, 9.7 g of polyether polyol (MW.1000, hydroxyl value: 107-117 mgKOH / g), 110 μL of dibutyltin dilaurate and 2.07 g of fluorine-substituted open-ring plant alcohol obtained in S2 were added to 50 g of acetone, stirred and reacted at 55°C for 30 min under a nitrogen atmosphere, and then 1.3 g of dimethylol propionic acid was added after cooling to room temperature, and the reaction was continued at 55°C for 3 h with stirring. After the reaction was completed, triethylamine was added, and then deionized water was added, and the acetone was evaporated to obtain an emulsion; S4: Add the emulsion into the mold, air-dry at room temperature, and then place it in a drying oven at 45-55°C, and then demould to obtain a waterproof polymer film.

[0022] Comparative Example 1: A method for preparing a waterproof polymer material comprises the following steps: S1: 7.3 g of isophorone diisocyanate, 19.62 g of polyether polyol (MW.1000, hydroxyl value: 107-117 mgKOH / g), and 150 μL of dibutyltin dilaurate were added to 50 g of acetone, and stirred at 55°C for 30 min under a nitrogen atmosphere. After cooling to room temperature, 1.76 g of dimethylolpropionic acid was added, and the stirring reaction was continued at 55°C for 3 h. After the reaction was completed, triethylamine was added, and then deionized water was added, and the acetone was evaporated to obtain an emulsion; S2: Add the emulsion into the mold, air dry at room temperature, and then place it in a drying oven at 45-55°C, and then demould to obtain a waterproof polymer film.

[0023] Test Example 1: Mechanical properties determination The mechanical properties test of the film was conducted with reference to GB / T 16777-2008 "Test Methods for Building Waterproof Coatings", and an electronic tensile testing machine was used to test the mechanical properties of the film. The film was cut into strips with a width of 6 mm, parallel markings with a spacing of 25 mm were drawn, the thickness of the specimen was measured with a thickness gauge, and the spacing of the clamps of the tensile testing machine was adjusted to 50 mm. The specimen was clamped on the testing machine and stretched at a stretching speed of 200 mm / min until it broke. The maximum load when the specimen broke was recorded ( P ), the spacing between the marking lines when the fracture occurs ( L 1) Accurate to 0.1 mm, repeat 5 times per set.

[0024] Waterproof performance test The waterproof performance of the coating is divided into two parts: hydrophobicity and water absorption. Pour 0.5 mL of the emulsion on a glass slide, air dry it on a horizontal table at room temperature for 24 h, and then dry it at 50 °C for 24 h. Measure the static water contact angle on the film surface at room temperature, and test each sample 5 times. Test the water absorption of the film using the immersion method. Cut the film into a 5 mm × 5 mm square, weigh the mass of the specimen, and record it as m1. Then immerse the specimen in water at (23 ± 2) °C for (168 ± 2) h, take it out and use filter paper to absorb the water stains on the surface, and weigh it immediately, and record it as m2. The time from taking the specimen out of the water to the weighing should be completed within 1 min, with 3 samples per group. Experimental protocol Tensile strength / MPa Elongation at break / % Water absorption / % Contact angle / ° Example 1 47.6 267.4 0.83 93.75 Example 2 44.6 278.2 0.61 94.12 Example 3 43.5 243.5 1.01 91.75 Example 4 48.9 286.7 0.94 93.33 Comparative Example 1 27.3 119.65 3.21 76.69

[0025] The present invention introduces plant alcohol as a reactant, which is an aliphatic hydrocarbon with double bonds and long chains. The double bonds are oxidized to epoxy structures through oxidation, and further ring-opened by fluoroalkyl alcohol to obtain fluorine-substituted ring-opened plant alcohol containing two hydroxyl groups. The plant alcohol is used as a monomer to react with dimethylol propionic acid, isophorone diisocyanate, and polyether polyol to form waterborne polyurethane, and further triethylamine is reacted with the carboxyl group on the dimethylol propionic acid to form an ion state, and finally a waterborne polyurethane emulsion is obtained. Due to the introduction of hydrophobic alkyl long-chain alkanes and fluorine atoms, and the control of the proportion of each monomer, the hydrophobicity is significantly improved, and the tensile strength and elongation at break are both increased.

[0026] Although the present invention has been disclosed as above in terms of preferred embodiments, they are not intended to limit the present invention. Anyone skilled in the art can make various changes or modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the scope of protection defined by the claims of this application.

Claims

1. A method for preparing a waterproof polymer material, characterized in that: The following steps are involved: S1: Add plant alcohol into a flask, use a strongly acidic ion exchange resin as a catalyst, slowly drop a mixture of formic acid and hydrogen peroxide, stir and react at 78-85°C after the dropwise addition is completed, filter to remove the catalyst, wash with saturated brine until neutral, and vacuum rotary evaporate to obtain epoxidized plant alcohol; S2: adding the epoxidized plant alcohol obtained in S1 to cyclohexane, adding HBF4 and an excess of fluoroalkyl alcohol, stirring and reacting at room temperature, adding alkaline solution to neutralize HBF4 after the reaction, drying with anhydrous sodium sulfate and removing excess fluoroalkyl alcohol by rotary evaporation to obtain fluorine-substituted open-ring plant alcohol; S3: adding isophorone diisocyanate, polyether polyol, dibutyltin dilaurate and the fluorine-substituted open-ring plant alcohol obtained in S2 to acetone, stirring and reacting at 50-55° C. under a nitrogen atmosphere, adding dimethylolpropionic acid after cooling to room temperature, continuing to stir and react at 50-55° C., adding triethylamine after the reaction is completed, and then adding deionized water, and evaporating the acetone to obtain an emulsion; S4: Add the emulsion into the mold, air-dry at room temperature, and then place it in a drying oven at 45-55°C, and then demould to obtain a waterproof polymer film.

2. The method for preparing a waterproof polymer material according to claim 1, characterized in that: The addition amount of the strong acid ion exchange resin catalyst in S1 is 1-3% of the mass of the plant alcohol, and the molar ratio of the plant alcohol, formic acid and H2O2 in hydrogen peroxide is 1:0.25-0.3:3-5.

3. The method for preparing a waterproof polymer material according to claim 2, characterized in that: The reaction time of S1 is 5-7h, and the temperature of vacuum rotary evaporation is 75-80°C.

4. The method for preparing a waterproof polymer material according to claim 3, characterized in that: The mass of HBF4 added to S2 is 5%-10% of the epoxidized plant alcohol, the molar ratio of fluoroalkyl alcohol to epoxidized plant alcohol is 1:1-1.2, and the reaction time is 1-3h.

5. The method for preparing a waterproof polymer material according to claim 3, characterized in that: The mass of cyclohexane in S2 is 3-5 times that of epoxidized plant alcohol.

6. The method for preparing a waterproof polymer material according to claim 5, characterized in that: The fluoroalkyl alcohol in S2 is one of trifluoroethanol, trifluoropropanol and trifluoroisopropanol.

7. The method for preparing a waterproof polymer material according to claim 6, characterized in that: The molecular weight of the polyether polyol in S3 is 1000, the hydroxyl value is 107-117 mg KOH / g, the molar ratio of isophorone diisocyanate, polyether polyol, fluorine-substituted open-ring plant alcohol and dimethylol propionic acid is 1-1.3:0.4-0.5:0.2-0.3:0.4-0.5, and the ratio of isophorone diisocyanate and dibutyltin dilaurate is 1 g:20-25 μL.

8. The method for preparing a waterproof polymer material according to claim 7, characterized in that: The amount of acetone added in S3 is 5-10 times the mass of isophorone diisocyanate.

9. The method for preparing a waterproof polymer material according to claim 8, characterized in that: The amount of deionized water added in S3 is 5-10 times the mass of isophorone diisocyanate.

10. The method for preparing a waterproof polymer material according to claim 9, characterized in that: The molar ratio of triethylamine to dimethylolpropionic acid in S3 is 1:1.