Solder resist ink resin for foldable multilayer circuit board

By reacting homemade epoxy resin intermediate with acrylic monomer and acid anhydride, combining tetrahydrophenyl anhydride or hexahydrophenyl anhydride, PCB solder-resistant ink resin with high rigidity and flexibility, the solution is to solve the problem of high temperature resistance and flexibility of traditional ink resins. The shortcomings have achieved better high temperature and yellowing resistance.

CN118978663APending Publication Date: 2024-11-19东胜化学(上海)有限公司
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411278753.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

On the basis of maintaining high temperature resistance and easy development performance, traditional PCB soldering ink resins are difficult to improve flexibility to meet the high requirements of modern electronic products for volume and flexibility.

Method used

The homemade epoxy resin intermediate is used to open the ring reaction with acrylic monomer and acid anhydride, and react with tetrahydrophenyl anhydride or hexahydrophenyl anhydride to form a product with high rigidity and high temperature resistance, while improving flexibility through the long side chain segments. , prepare PCB solder resist ink resin with better resistance to high temperature and yellowing.

Benefits of technology

It significantly improves the flexibility and bending resistance of PCB solder-resistant ink resin, while maintaining excellent high temperature resistance, shortening development time, and enhancing the overall performance of the ink.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978663A_ABST
    Figure CN118978663A_ABST
Patent Text Reader

Abstract

The invention relates to a solder resist ink resin for a foldable multilayer circuit board, and belongs to the technical field of polymer synthesis. A self-made epoxy resin intermediate is adopted, the self-made epoxy resin intermediate can be subjected to a ring-opening reaction with an acrylic monomer and then react with tetrahydrophthalic anhydride or hexahydrophthalic anhydride, and in the finally obtained product, a benzene ring in the self-made epoxy resin intermediate provides rigidity and high temperature resistance; and the long chain segment of the side chain provides flexibility and yellowing resistance, so that the prepared PCB solder resist ink resin has better high temperature resistance and yellowing resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer synthesis, in particular to a solder resist ink resin for a foldable multi-layer circuit board. Background Art

[0002] PCB ink is a layer of ink coated on the PCB that can protect the circuit. Its core material is an organic polymer with a certain viscosity, which we call PCB solder mask ink resin. In recent years, with the rapid development of mobile phones, notebooks, and outdoor wearable electronic products, the PCB equipped with chips has higher and higher requirements for volume and flexibility. Traditional PCB boards are not flexible. Therefore, based on this requirement, in addition to the PCB needing to have good flexibility, the ink used for PCB also needs to have considerable flexibility. This puts forward new requirements for its core component, namely the polymer. In addition to having the same excellent high temperature resistance and easy development performance as traditional PCB solder mask ink resin, it must also have flexibility so that it can be used in the PCB coating process.

[0003] After searching, the Chinese invention patent: A PCB solder mask ink resin and its preparation method (publication number CN113174030A, publication date 2021.07.27), the application discloses a PCB solder mask ink resin, which includes the following components by mass percentage: 10-25% acrylic monomer, 25-40% epoxy resin, 6-10% organic acid, 5-20% special intermediate, 30-60% solvent; wherein, the special intermediate is obtained by the following steps: a diol is reacted with maleic anhydride or tetrahydrophthalic anhydride at 80°C for 0.5-2h, then cooled to 45-60°C, isocyanate is added, and the reaction is carried out for 1-3h. By mass percentage, the input amount of diol is 10-20%, the input amount of maleic anhydride or tetrahydrophthalic anhydride is 20-30%, and the input amount of isocyanate is 50-60%. Although this application also uses special monomers, the monomers in this solution can only increase the flexibility of the product and do not solve the high temperature resistance problem well.

[0004] Therefore, there is an urgent need for a PCB solder mask ink resin that improves flexibility while maintaining excellent high temperature resistance and easy development performance, and a preparation method thereof to solve the above technical problems. Summary of the invention

[0005] 1. Technical problem to be solved by the invention

[0006] The purpose of the present invention is to solve the problem that the existing heat collector is heated unevenly under sunlight.

[0007] 2. Technical solution

[0008] In order to achieve the above object, the technical solution provided by the present invention is:

[0009] The solder resist ink resin for a foldable multi-layer circuit board of the present invention comprises the following components (calculated by mass percentage):

[0010] 10-25% acrylic monomer, 25-40% epoxy resin, 6-10% acid anhydride, 5-20% isocyanate, 30-60% solvent, wherein the epoxy resin is a self-made epoxy resin intermediate, and the structure is as follows:

[0011]

[0012] Preferably, the acrylic acid monomer is an acrylic acid monomer and / or a methacrylic acid monomer.

[0013] Preferably, the isocyanate is IPDI or HDI or isocyanate ethyl acrylate.

[0014] Preferably, the acid anhydride is one or more of maleic anhydride, tetrahydrophthalic anhydride, succinic acid, dihydroxymethylbutyric acid and hexahydrophthalic anhydride.

[0015] Preferably, the solvent is one or more of DBE, No. 150 solvent oil and DCAC.

[0016] A method for preparing a solder resist ink resin for a foldable multi-layer circuit board comprises the following steps:

[0017] S1. Heat the reactor to 90-150° C., add a solvent, add an acrylic monomer, an epoxy resin and a catalyst within 1-5 hours, and keep the temperature for 1-10 hours. The epoxy resin is a homemade epoxy resin intermediate.

[0018] S2, add anhydride, the reaction time is 2 to 6 hours, and the reaction temperature is controlled at 90 to 130°C;

[0019] S3. Add IPDI or HDI or isocyanate ethyl acrylate, the reaction time is 1 to 5 hours, and the reaction temperature is controlled at 40 to 110°C.

[0020] Preferably, the catalyst in step S1 is triphenylphosphine, dimethylaniline or triethylamine.

[0021] Preferably, in step S1, the addition time of acrylic monomer and epoxy resin is 2 hours, and the insulation time is 10 hours; in step S2, the reaction time is 5 hours.

[0022] Preferably, the preparation process of the homemade epoxy resin intermediate is as follows:

[0023] Add epoxy bisphenol A resin into the reaction kettle, raise the temperature to 130-150°C, add caprolactone and catalyst, and control the reaction time to 3-8h;

[0024] The mass ratio of epoxy bisphenol A type resin to caprolactone is 1:1 to 1:4, and the total mass ratio of the catalyst to the epoxy bisphenol A type resin and caprolactone is 1 / 10,000 to 5 / 10,000.

[0025] Preferably, the catalyst is stannous octoate or monobutyltin oxide; and the time for adding caprolactone dropwise is 0.5 to 3 hours.

[0026] 3. Beneficial effects

[0027] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0028] The invention discloses a solder resist ink resin for a foldable multilayer circuit board. The self-made epoxy resin intermediate can undergo a ring-opening reaction with an acrylic acid monomer, and then react with tetrahydrophthalic anhydride or hexahydrophthalic anhydride. In the final product, the benzene ring in the self-made epoxy resin intermediate provides rigidity and high temperature resistance, and the long chain segment of the side chain provides flexibility and yellowing resistance. Therefore, the prepared PCB solder resist ink resin has better high temperature resistance and yellowing resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the molecular structure of the self-made epoxy resin intermediate of the present invention;

[0030] Figure 2 This is a flexible circuit board obtained by using the resin prepared in Example 1. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.

[0032] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present application described here. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0033] In the present application, the terms "upper", "lower", "left", "right", "front", "back", "top", "bottom", "inner", "outer", "middle", "vertical", "horizontal", "lateral", "longitudinal" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings. These terms are mainly used to better describe the present application and its embodiments, and are not used to limit the indicated devices, elements or components to have a specific orientation, or to be constructed and operated in a specific orientation.

[0034] In addition, some of the above terms may be used to express other meanings in addition to indicating orientation or positional relationship. For example, the term "on" may also be used to express a certain dependency or connection relationship in some cases. For those of ordinary skill in the art, the specific meanings of these terms in this application can be understood according to specific circumstances.

[0035] In addition, the terms "installed", "set", "provided with", "connected", "connected", and "socketed" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral structure; it can be a mechanical connection, or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be an internal connection between two devices, elements, or components. For those of ordinary skill in the art, the specific meanings of the above terms in this application can be understood according to specific circumstances.

[0036] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0037] Example 1

[0038] The present embodiment provides a PCB solder mask ink resin, comprising the following components: 15.8 kg acrylic acid monomer, 30 kg homemade epoxy intermediate, 0.2 kg triethylamine, 10 kg maleic anhydride, 5 kg HDI, 3 kg IPDI and 36 kg DCAC solvent.

[0039] The preparation method of the PCB solder mask ink resin of this embodiment is:

[0040] S1. Heat the reactor to 100°C, add DCAC solvent, add homemade epoxy intermediate, triethylamine, add acrylic acid dropwise, add for 2 hours, and keep warm for 10 hours.

[0041] S2, add maleic anhydride, the reaction time is 5h, and the reaction temperature is controlled at 130℃;

[0042] S3, add IPDI and HDI, the reaction time is 5h, and the reaction temperature is controlled at 80℃.

[0043] Example 2

[0044] The present embodiment provides a PCB solder mask ink resin, comprising the following components: 14.8 kg acrylic acid monomer, 28 kg homemade epoxy resin intermediate, 0.2 kg triphenylphosphine, 9 kg tetrahydrophthalic anhydride, 10 kg HDI, 2 kg IPDI and 36 kg DBE solvent.

[0045] S1. Heat the reactor to 120°C, add DBE solvent, add homemade epoxy resin intermediate and triphenylphosphine, add acrylic acid dropwise for 2 hours, and keep warm for 10 hours;

[0046] S2, add tetrahydrophthalic anhydride, the reaction time is 5h, and the reaction temperature is controlled at 130°C;

[0047] S3, add IPDI or HDI, the reaction time is 5h, and the reaction temperature is controlled at 80℃.

[0048] Comparative Example 1

[0049] The present embodiment provides a PCB solder mask ink resin, comprising the following components: 15.8 kg acrylic acid, 30 kg bisphenol A epoxy resin (commercially available brand Changchun 188 epoxy resin), 0.2 g triethylamine, 10 kg maleic anhydride, 5 kg HDI, 3 kg IPDI and 36 kg DCAC solvent.

[0050] The preparation method of the PCB solder mask ink resin of this embodiment is:

[0051] S1. DCAC is put into the reactor, the temperature is raised to 100°C, 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexylmethyl ester and triethylamine are added, acrylic acid is added dropwise for 2 hours, and the temperature is kept for 10 hours;

[0052] S2, add maleic anhydride, raise the temperature to 130°C, and react for 5 hours;

[0053] S3. Cool down to 80°C, add HDI and IPDI, and react for 5 hours.

[0054] Except for the epoxy resin, the ratio of other raw materials and the synthesis route of this comparative example are the same as those of Example 1.

[0055] Comparative Example 2

[0056] The present embodiment provides a PCB solder mask ink resin, comprising the following components: 16.5 kg acrylic acid, 32 kg bisphenol A epoxy resin (commercially available brand Nan Ya 128 epoxy resin), 0.2 kg triphenylphosphine, 11 kg tetrahydrophthalic anhydride, 5 kg HDI, 2 kg IPDI and 36 kg DBE solvent.

[0057] The preparation method of the PCB solder mask ink resin of this embodiment is:

[0058] S1, DBE were put into the reactor, the temperature was raised to 120℃, bis((3,4-epoxycyclohexyl)methyl)adipate, triphenylphosphine were added, acrylic acid was added dropwise, the addition was continued for 2h, and the temperature was kept for 10h;

[0059] S2, add tetrahydrophthalic anhydride, raise the temperature to 130°C, and react for 5 hours;

[0060] S3. Cool down to 80°C, add HDI and IPDI, and react for 5 hours.

[0061] Compared with Example 2, this comparative example has different epoxy resin parts and different raw material ratios, but the synthesis route is the same.

[0062] The high temperature resistance, developing performance and flexibility of Examples 1 and 2 and Comparative Examples 1 and 2 were tested, and the test results are shown in Table 1 below:

[0063] Table 1 Comparative data of product effects of Examples 1, 2 and Comparative Examples 1, 2

[0064] sample High temperature resistance (280℃*10s)*3 times Development time Flexibility and bending resistance Example 1 High temperature resistance without problems 120s 20 times bending without cracks Example 2 High temperature resistance without problems 120s 30 times bending without cracks Comparative Example 1 High temperature resistance without problems 180s 4 times bending without cracks Comparative Example 2 High temperature resistance without problems 160s No crack after 2 bendings

[0065] The high temperature resistance test method is as follows: after mixing the main resin with a fixed amount of active monomer, photoinitiator, epoxy resin, epoxy curing agent, and leveling agent, evenly apply it on the PCB copper foil, bake it in an 80℃ oven for 0.5 hours, then bake it at 160℃ for 2 hours, then put it in a 280℃ tin furnace for 10 seconds, and take it out. After repeating three times, observe whether there is cracking on the surface of the copper foil.

[0066] The developing time test method is as follows: the main resin is mixed with a fixed amount of active monomer, photoinitiator, epoxy resin, epoxy curing agent, and leveling agent, and then evenly coated on the PCB copper foil, placed in an 80°C oven for 0.5 hours, exposed by an exposure machine, and then exposed with a 1% sodium carbonate aqueous solution at 2kg / cm 2Spray on the copper foil under pressure, and record the time when the pattern on the copper foil is completely revealed.

[0067] The test method for the number of times the flexibility is bent is as follows: fold the copper foil at an angle of 180 degrees, then unfold it and repeat this process multiple times. When the coating on the copper foil cracks, record the number of folds.

[0068] It can be seen from the technical effects of the above embodiments and comparative examples that the PCB solder mask ink resin of the present application, when using a special epoxy resin as a raw material, can shorten the development time while ensuring the high temperature resistance of the ink, and greatly improve the flexibility and bending resistance, compared with the synthetic products made from common commercially available epoxy resin brands. This is because the homemade epoxy resin intermediate used in the present application can undergo a ring-opening reaction with an acrylic acid monomer, and then react with tetrahydrophthalic anhydride or hexahydrophthalic anhydride. In the final product, the benzene ring in the homemade epoxy resin intermediate provides rigidity and high temperature resistance, and the long chain segment of the side chain provides flexibility and yellowing resistance. Therefore, the prepared PCB solder mask ink resin has better high temperature resistance and yellowing resistance.

[0069] The above-described embodiments only express a certain implementation mode of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the patent scope of the present invention. It should be pointed out that, for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.

Claims

1. A solder resist ink resin for a foldable multi-layer circuit board, characterized in that: Includes the following components (calculated by mass percentage) 10-25% acrylic monomer, 25-40% epoxy resin, 6-10% acid anhydride, 5-20% isocyanate, 30-60% solvent, wherein the epoxy resin is a self-made epoxy resin intermediate, and the structure is as follows:

2. The solder resist ink resin for a foldable multi-layer circuit board according to claim 1, characterized in that: The acrylic acid monomer is an acrylic acid monomer and / or a methacrylic acid monomer.

3. The solder resist ink resin for a foldable multi-layer circuit board according to claim 1, characterized in that: The isocyanate is IPDI or HDI or isocyanate ethyl acrylate.

4. The solder resist ink resin for a foldable multi-layer circuit board according to claim 1, characterized in that: The acid anhydride is one or more of maleic anhydride, tetrahydrophthalic anhydride, succinic acid, dihydroxymethylbutyric acid and hexahydrophthalic anhydride.

5. The solder resist ink resin for a foldable multi-layer circuit board according to claim 1, characterized in that: The solvent is one or more of DBE, No. 150 solvent oil and DCAC.

6. The method for preparing a solder resist ink resin for a foldable multi-layer circuit board according to any one of claims 1 to 5, characterized in that: The steps include: S1. Heat the reactor to 90-150° C., add a solvent, add an acrylic monomer, an epoxy resin and a catalyst within 1-5 hours, and keep the temperature for 1-10 hours. The epoxy resin is a homemade epoxy resin intermediate. S2, add anhydride, the reaction time is 2 to 6 hours, and the reaction temperature is controlled at 90 to 130°C; S3. Add IPDI or HDI or isocyanate ethyl acrylate, the reaction time is 1 to 5 hours, and the reaction temperature is controlled at 40 to 110°C.

7. The method for preparing a solder resist ink resin for a foldable multi-layer circuit board according to claim 6, characterized in that: The catalyst in step S1 is triphenylphosphine, dimethylaniline or triethylamine.

8. The method for preparing a solder resist ink resin for a foldable multi-layer circuit board according to claim 6, characterized in that: In the step S1, the addition time of the acrylic monomer and the epoxy resin is 2 hours, and the heat preservation time is 10 hours; in the step S2, the reaction time is 5 hours.

9. The method for preparing a solder resist ink resin for a foldable multi-layer circuit board according to claim 6, characterized in that: The preparation process of the homemade epoxy resin intermediate is as follows: Add epoxy bisphenol A resin into the reaction kettle, raise the temperature to 130-150°C, add caprolactone and catalyst, and control the reaction time to 3-8h; The mass ratio of epoxy bisphenol A type resin to caprolactone is 1:1 to 1:4, and the total mass ratio of the catalyst to the epoxy bisphenol A type resin and caprolactone is 1 / 10,000 to 5 / 10,000.

10. The method for preparing a solder resist ink resin for a foldable multi-layer circuit board according to claim 9, characterized in that: The catalyst is stannous octoate or monobutyl tin oxide; the time for dripping caprolactone is 0.5 to 3 hours.

Citation Information

Cited By

  • Solder resist ink resin for foldable multilayer circuit board

    WO2026056357A1