Bromine functional polyester and preparation method thereof

By developing bromine functionalized polyester and its preparation method, the problem of single functionalization of polyester materials has been solved, efficient recyclability and diversified application expansion has been achieved, diverse application needs have been met, and plastic recycling has been improved efficiency.

CN118978679AActive Publication Date: 2024-11-19NANJING TECH UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410775373.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-17
Publication Date
2024-11-19
Estimated Expiration
2044-06-17

AI Technical Summary

Technical Problem

The existing polyester materials are single functional and cannot meet the diverse practical application needs. There is a lack of efficient recyclable material solutions in plastic recycling.

Method used

A bromine functionalized polyester and its preparation method were developed. Bromine functionalized polyester with excellent properties was prepared by reaction of urea or thiourea, Bronst base, solvent and initiator with bromine substituted bridging lactone monomer. Polyester can be quickly depolymerized to monomer under certain conditions, achieving high recovery rate.

Benefits of technology

The prepared bromine functionalized polyesters have a wide range of physical and chemical properties, including excellent flame retardancy and can induce radical reactions, expanding the application field and achieving high recovery and simple and controllable production processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978679A_ABST
    Figure CN118978679A_ABST
Patent Text Reader

Abstract

The invention discloses a bromine-functionalized polyester and a preparation method thereof, the structural formula of the bromine-functionalized polyester is as shown in formula I. The preparation method of the bromine-functionalized polyester comprises the step of reacting urea or thiourea, a Bronsted base, a solvent, an initiator and a bromine-substituted bridged ring lactone monomer. Compared with the existing aliphatic polyester high polymer material, the bromine-functionalized polyester provided by the invention enriches the multifunctionality of the material, improves the application value and expands the application field. Meanwhile, the prepared bromine-functionalized polyester has recoverability. And secondly, the preparation method of the bromine-functionalized polyester is simple to operate, strong in controllability and high in product yield, and various transformations can be generated subsequently. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer synthesis chemistry, and in particular to a bromine functionalized polyester and a preparation method thereof. Background Art

[0002] This section merely provides background information related to the present disclosure and is not necessarily prior art.

[0003] The widespread use of plastics has resulted in millions of plastic wastes being generated every year, most of which are eventually incinerated, landfilled or discarded into the ocean. This leads to huge energy losses and serious environmental pollution. Plastic pollution and energy waste have attracted the attention of governments around the world, and how to solve the plastic crisis has become a topic of global concern. In this context, the recycling of plastics is an effective way to solve the plastic problem. Among them, chemical recycling methods provide a solution to the plastic problem. Recycled plastics are depolymerized into original monomers under mild conditions, and the depolymerized monomers are repolymerized to make plastics with excellent properties, establishing a closed-loop life cycle of "monomer-polymer-monomer". At present, polyesters, polythioesters, polycarbonates, polyamides, etc. have made important progress in the chemical recycling of monomers. Among these recyclable polymers, aliphatic polyesters are expected to become a substitute for petroleum-based plastics due to their excellent properties.

[0004] However, the current functionalization of polyester is single and cannot meet the diverse practical application needs. As an important type of polymer material, bromine-functionalized polyester materials can undergo a variety of subsequent transformations, such as copolymerization, cross-linking, grafting, etc., to prepare materials with special properties. Summary of the invention

[0005] Purpose of the invention: The technical problem to be solved by the present invention is to provide a bromine functional polyester and a preparation method thereof in view of the deficiencies in the prior art.

[0006] In order to solve the above technical problems, the present invention discloses the following technical solutions:

[0007] In a first aspect, the present invention discloses a bromine-functionalized polyester, the general formula of which is shown in Formula I:

[0008]

[0009] in,

[0010] Y is selected from methoxy, ethoxy, isopropoxy, tert-butoxy, benzyloxy, phenylethoxy, phenylpropoxy, diphenylmethoxy, 2,2-diphenylethoxy;

[0011] n is any integer selected from 10 to 2000;

[0012] The number average molecular weight of the bromine-functionalized polyester is 2,000 to 400,000 g mol -1 , such as 4000, 5000, 6000, 7000, 15000, 16000, 56000, 80000, 90000, 190000, 370000, 380000 g mol -1 In some embodiments, n is selected from any integer between 10 and 2000 so that the number average molecular weight of the bromine-functionalized polyester is 2000 to 400000 g mol -1 ;

[0013] The dispersion coefficient of the bromine functionalized polyester is 1.00-1.50, such as 1.20, 1.30, 1.40.

[0014] In some embodiments, the bromine-functionalized polyester is any one of Formula II;

[0015]

[0016] In a second aspect, the present invention discloses a method for preparing the above polymer.

[0017] The method comprises the following steps: reacting urea or thiourea shown in formula III, Bronsted base, solvent, initiator and bromine-substituted bridged ring lactone monomer shown in formula IV; further, the method comprises the following steps: stirring urea or thiourea shown in formula III, Bronsted base, solvent and initiator for 1-8 minutes, and then adding bromine-substituted bridged ring lactone monomer shown in formula IV to react; further, the method comprises the following steps: stirring urea or thiourea shown in formula III, Bronsted base, solvent and initiator for 3-6 minutes, and then adding bromine-substituted bridged ring lactone monomer shown in formula IV to react.

[0018] In some embodiments, the method comprises the following steps: stirring the urea or thiourea shown in formula III, the Bronsted base, the first solvent and the initiator at 25-100°C for 3-6 minutes, and then adding the solution of the bromine-substituted bridged ring lactone monomer and the second solvent shown in formula IV and continuing to stir and react at 25-100°C for 5 minutes to 24 hours; the first solvent and the second solvent are the same solvent; in some embodiments, the molar volume ratio of the bromine-substituted bridged ring lactone monomer shown in formula IV to the first solvent and the second solvent is 1.5-2.5 mol / L, preferably 2 mol / L.

[0019] Wherein, the structure of urea or thiourea shown in formula III is as follows:

[0020]

[0021] in,

[0022] X is selected from O or S;

[0023] R 1 -R 4 Each is independently selected from H, OMe, Cl, and CF3.

[0024] Further,

[0025] When X is selected from O, R 1 -R 4 The groups are:

[0026] R 1 =OMe, R 2 -R 4 =H;

[0027] or R 1 -R 4 =H;

[0028] or R 1 =Cl, R 2 -R 4 =H;

[0029] or R 1 =CF 3 , R 2 -R 4 =H;

[0030] or R 1 -R 2 =CF 3 , R 3 -R 4 =H;

[0031] or R 1 -R 3 =CF 3 , R 4 =H;

[0032] or R 1 -R 4 =CF 3 ;

[0033] When X is selected from S, R 1 -R 4 =CF 3 .

[0034] Further, the structure of the urea or thiourea represented by Formula III is any one of U1 to U 9 or TU 1;

[0035]

[0036]

[0037] Among them, the Bronsted base includes 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD), diphenyl phosphate (DPP), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), 1,3-di-mesityl imidazol-2-ylidene (IMes), and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene (MTBD).

[0038] Wherein, the reaction solvent is one of toluene, tetrahydrofuran, dichloromethane and N,N-dimethylformamide.

[0039] Wherein, the initiator is an alcohol; preferably, the initiator is methanol, ethanol, isopropanol, tert-butanol, benzyl alcohol, phenylethyl alcohol, phenylpropanol, diphenylmethanol, and 2,2-diphenylethanol.

[0040] The structural formula of the bromine-substituted bridged lactone monomer shown in Formula IV is as follows:

[0041]

[0042] Wherein, the molar ratio of the bromine-substituted bridged ring lactone monomer shown in formula IV, the urea or thiourea shown in formula III, the Bronsted base, and the initiator is 10-2000:1-20:1-20:1, such as 30-50:1:1:1, such as 100-300:1:1:1, such as 500:2:2:1, such as 55:9:9:1, such as 1000-200:10-20:10-20:1.

[0043] Wherein, the reaction temperature is 25-100°C; and the reaction time is 5-1440 minutes.

[0044] In a third aspect, the present invention discloses the use of the bromine-functionalized polyester described in the first aspect or the bromine-functionalized polyester prepared by the method described in the second aspect in the preparation of chemically recyclable materials.

[0045] The bromine functional polyester prepared by the present invention can be rapidly depolymerized to monomers under certain conditions, and the purity is 99%, and the degradation conditions are as follows: the catalyst is p-toluenesulfonic acid (2-10 mol% of the polymer), the reaction temperature is 60-120° C., toluene is the solvent (the polymer concentration is 0.3-0.7 g / mL), the reaction time is 2-12 hours, and the recovery rate is 60-80%.

[0046] Beneficial effects:

[0047] (1) The bromine-functionalized polyester synthesized in the present invention is a new type of polymer material. The bromine functional group thereof has a wide range of physical and chemical properties, including excellent flame retardancy, initiation of free radical reactions (crosslinking or graft polymerization), etc., which can give the material a variety of functionalization and properties and expand the application field.

[0048] (2) The bromine-functionalized polyester prepared by the present invention can be depolymerized under certain conditions and is recyclable.

[0049] (3) The synthesis method provided by the present invention is simple, highly controllable and has a high product yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.

[0051] Figure 1 For the polymer of Example 1 1 H NMR spectra.

[0052] Figure 2 The polymer of Example 1 13 C HMR diagram.

[0053] Figure 3 This is the matrix-assisted laser ionization desorption / reaction time-of-flight mass spectrum of the polymer in Example 1.

[0054] Figure 4 This is the GPC chart of the polymer in Example 1. DETAILED DESCRIPTION

[0055] The present invention can be better understood according to the following examples. However, it is easy for those skilled in the art to understand that the contents described in the examples are only used to illustrate the present invention, and should not and will not limit the present invention described in detail in the claims.

[0056] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0057] In the following examples, a 400 MHz Bruker NMR instrument was used to measure the product: the deuterated reagent used tetramethylsilane (TMS) as the internal standard, the H NMR test concentration was about 10 mg / mL, the C NMR test concentration was about 20 mg / mL, and the deuterated reagent was deuterated chloroform.

[0058] The molecular weight and molecular weight distribution of the bromine functionalized polyester described in the present invention are obtained by testing with a Wyatt gel permeation chromatograph. Tetrahydrofuran (THF) is used as the mobile phase, the flow rate is 0.70 mL / min, the concentration of the polymer in chromatographic grade tetrahydrofuran is about 4 mg / mL, polystyrene (PS) is used as the standard sample, and the molecular weight and molecular weight distribution of the polymer are obtained by testing with a relative method.

[0059] The topological structure of the polymer in the present invention is tested by a Microflex LRF mass spectrometer provided by Bruker Spectroscopy Instruments. The sample concentration is 10 mg / mL, 2,5-dihydroxybenzoic acid (DHB) is used as the matrix, the matrix concentration is 20 mg / mL, the solvent is 60% isopropanol and 40% chloroform, sodium iodide is used as the cationic reagent, the concentration is 20 mg / mL, and the solvent is methanol. Finally, the sample / matrix / cationic reagent = 1 / 10 / 1 is mixed and dropped on the test sample plate and dried before testing.

[0060] The catalysts described in the following examples are Bronsted base and (thio)urea. The (thio)urea described in the present invention is thiourea or urea, and the specific structure is any one of U1 to U 9 or TU 1.

[0061] Embodiment 1:

[0062] The two ampoules were evacuated with a Schlenk apparatus and baked with a Bunsen burner to remove the residual moisture in the ampoules. After baking, argon was filled for protection. This process was repeated three times and cooled to room temperature and transferred to a glove box. In the glove box, 1.5 mmol of bromine-substituted bridged lactone monomer was weighed and placed in ampoule No. 1. 400 μl of redistilled toluene was added to dissolve it. 0.05 mmol of Bronsted base (DBU) and 0.05 mmol of (thio)urea (U 9) were weighed and placed in ampoule No. 2. 300 μl of toluene was added to dissolve the catalyst. 0.05 mmol of benzyl alcohol was added and stirred at 25°C for 5 minutes. Finally, the dissolved monomer was added to the ampoule containing the catalyst and initiator to start polymerization.

[0063] After stirring at 25°C for 10 minutes, 3-4 drops of the polymer solution were added to deuterated chloroform of benzoic acid to test the monomer conversion rate, and the rest were added to ice methanol dissolved with benzoic acid to quench and precipitate. After centrifugation at 10000r / min for 3 minutes, the supernatant was poured off, and a small amount of dichloromethane (DCM) was used to completely dissolve the polymer and added to ice methanol for precipitation. This was repeated three times, and the polymer product was placed in a drying dish and then vacuumed with a Schlenk device for 12 hours. The conversion rate was measured by the reaction solution. 1 The polymer structure and molecular weight were calculated by H NMR. 1The polymer was identified by H NMR and its dispersion was determined by GPC. The conversion rate was 98%, the polymer number average molecular weight was 5070 g / mol, and the dispersion coefficient was 1.20.

[0064] Embodiment 2:

[0065] The two ampoules were evacuated with a Schlenk apparatus and baked with a Bunsen burner to remove the residual moisture in the ampoules. After baking, argon was filled for protection. This process was repeated three times and cooled to room temperature and transferred to a glove box. In the glove box, 1.5 mmol of bromine-substituted bridged lactone monomer was weighed and placed in ampoule No. 1. 400 μl of redistilled toluene was added to dissolve it. 0.03 mmol of Bronsted base (MTBD) and 0.03 mmol of (thio)urea (U 8) were weighed and placed in ampoule No. 2. 320 μl of toluene was added to dissolve the catalyst. 0.03 mmol of phenylethanol was added and stirred at 100°C for 5 minutes. Finally, the dissolved monomer was added to the ampoule containing the catalyst and initiator to start polymerization.

[0066] After stirring at 100°C for 20 minutes, 3-4 drops of the polymer solution were added to the deuterated chloroform of benzoic acid to test the monomer conversion rate, and the rest were added to the ice methanol in which benzoic acid was dissolved to quench and precipitate. After centrifugation at 10000r / min for 3 minutes, the supernatant was poured off, and a small amount of dichloromethane (DCM) was used to completely dissolve the polymer and added dropwise to the ice methanol for precipitation. This was repeated three times, and the polymer product was placed in a drying dish and then vacuumed for 12 hours using a Schlenk device. The conversion rate was calculated by 1H NMR of the reaction solution, the polymer structure and molecular weight were identified by 1H NMR, and the polymer dispersion was determined by GPC. The conversion rate was 75%, the polymer number average molecular weight was 7290g / mol, and the dispersion coefficient was 1.26.

[0067] Embodiment 3:

[0068] The two ampoules were evacuated with a Schlenk apparatus and baked with a Bunsen burner to remove the residual moisture in the ampoules. After baking, argon was filled for protection. This process was repeated three times and cooled to room temperature and transferred to a glove box. In the glove box, 5 mmol of bromine-substituted bridged lactone monomer was weighed and placed in ampoule No. 1. 2000 μl of redistilled tetrahydrofuran (THF) was added to dissolve it. 0.05 mmol of Bronsted base (TBD) and 0.05 mmol of (thio)urea (U 7) were weighed and placed in ampoule No. 2. 450 μl of tetrahydrofuran (THF) was added to dissolve the catalyst. 0.05 mmol of phenylpropanol was added and stirred at 25°C for 5 minutes. Finally, the dissolved monomer was added to the ampoule containing the catalyst and initiator to start polymerization.

[0069] After stirring at 25°C for 1 hour, 3-4 drops of the polymer solution were added to deuterated chloroform of benzoic acid to test the monomer conversion rate, and the rest was added to ice methanol dissolved with benzoic acid to quench and precipitate. After centrifugation at 10000r / min for 3 minutes, the supernatant was poured off, and a small amount of dichloromethane (DCM) was used to completely dissolve the polymer and added to ice methanol for precipitation. This was repeated three times, and the polymer product was placed in a drying dish and then vacuumed with a Schlenk device for 12 hours. The conversion rate was measured by the reaction solution. 1 The polymer structure and molecular weight were calculated by H NMR. 1 The polymer was identified by H NMR and its dispersion was determined by GPC. The conversion rate was 82%, the polymer number average molecular weight was 15720 g / mol, and the dispersion coefficient was 1.32.

[0070] Embodiment 4:

[0071] The two ampoules were evacuated with a Schlenk apparatus and baked with a Bunsen burner to remove the residual moisture in the ampoules. After baking, argon was filled for protection. This process was repeated three times and cooled to room temperature and transferred to a glove box. In the glove box, 3 mmol of bromine-substituted bridged lactone monomer was weighed and placed in ampoule No. 1. 1000 μl of redistilled toluene was added to dissolve it. 0.01 mmol of Bronsted base (TBD) and 0.01 mmol of (thio)urea (U 7) were weighed and placed in ampoule No. 2. 490 μl of toluene was added to dissolve the catalyst. 0.01 mmol of diphenylmethanol was added and stirred at 25°C for 5 minutes. Finally, the dissolved monomer was added to the ampoule containing the catalyst and initiator to start polymerization.

[0072] After stirring at 25°C for 2 hours, 3-4 drops of the polymer solution were added to deuterated chloroform of benzoic acid to test the monomer conversion rate, and the rest was added to ice methanol dissolved with benzoic acid to quench and precipitate. After centrifugation at 10000r / min for 3 minutes, the supernatant was poured off, and a small amount of dichloromethane (DCM) was used to completely dissolve the polymer and added to ice methanol for precipitation. This was repeated three times, and the polymer product was placed in a drying dish and then vacuumed with a Schlenk device for 12 hours. The conversion rate was measured by the reaction solution. 1 The polymer structure and molecular weight were calculated by H NMR. 1 The polymer was identified by H NMR and its dispersion was determined by GPC. The conversion rate was 97%, the polymer number average molecular weight was 55700 g / mol, and the dispersion coefficient was 1.35.

[0073] Embodiment 5:

[0074] The two ampoules were evacuated with a Schlenk apparatus and baked with a Bunsen burner to remove the residual moisture in the ampoules. After baking, argon was filled for protection. This process was repeated three times and cooled to room temperature and transferred to a glove box. In the glove box, 5 mmol of bromine-substituted bridged lactone monomer was weighed and placed in ampoule No. 1. 2000 μl of redistilled toluene was added to dissolve it. 0.02 mmol of Bronsted base (IMes) and 0.02 mmol of (thio)urea (U 1) were weighed and placed in ampoule No. 2. 490 μl of toluene was added to dissolve the catalyst. 0.01 mmol of 2,2-diphenylethanol was added and stirred at 25°C for 5 minutes. Finally, the dissolved monomer was added to the ampoule containing the catalyst and initiator to start polymerization.

[0075] After stirring at 25°C for 18 hours, 3-4 drops of the polymer solution were added to deuterated chloroform of benzoic acid to test the monomer conversion rate, and the rest was added to ice methanol dissolved with benzoic acid to quench and precipitate. After centrifugation at 10000r / min for 3 minutes, the supernatant was poured off, and a small amount of dichloromethane (DCM) was used to completely dissolve the polymer and added to ice methanol for precipitation. This was repeated three times, and the polymer product was placed in a drying dish and then vacuumed with a Schlenk device for 12 hours. The conversion rate was measured by the reaction solution. 1 The polymer structure and molecular weight were calculated by H NMR. 1 The polymer was identified by H NMR and its dispersion was determined by GPC. The conversion rate was 83%, the polymer number average molecular weight was 79460 g / mol, and the dispersion coefficient was 1.28.

[0076] Embodiment 6:

[0077] The two ampoules were evacuated with a Schlenk apparatus and baked with a Bunsen burner to remove the residual moisture in the ampoules. After baking, argon was filled for protection. This process was repeated three times and cooled to room temperature and transferred to a glove box. In the glove box, 5 mmol of bromine-substituted bridged lactone monomer was weighed and placed in ampoule No. 1. 1000 μl of redistilled toluene was added to dissolve it. 0.09 mmol of Bronsted base (DBU) and 0.09 mmol of (thio)urea (U 9) were weighed and placed in ampoule No. 2. 1490 μl of toluene was added to dissolve the catalyst. 0.01 mmol of benzyl alcohol was added and stirred at 25°C for 5 minutes. Finally, the dissolved monomer was added to the ampoule containing the catalyst and initiator to start polymerization.

[0078] After stirring at 25°C for 18 hours, 3-4 drops of the polymer solution were added to deuterated chloroform of benzoic acid to test the monomer conversion rate, and the rest was added to ice methanol dissolved with benzoic acid to quench and precipitate. After centrifugation at 10000r / min for 3 minutes, the supernatant was poured off, and a small amount of dichloromethane (DCM) was used to completely dissolve the polymer and added to ice methanol for precipitation. This was repeated three times, and the polymer product was placed in a drying dish and then vacuumed with a Schlenk device for 12 hours. The conversion rate was measured by the reaction solution. 1 The polymer structure and molecular weight were calculated by H NMR. 1 The polymer was identified by H NMR and its dispersion was determined by GPC. The conversion rate was 99%, the polymer number average molecular weight was 91800 g / mol, and the dispersion coefficient was 1.22.

[0079] Embodiment 7:

[0080] The two ampoules were evacuated with a Schlenk apparatus and baked with a Bunsen burner to remove the residual moisture in the ampoules. After baking, argon was filled for protection. This process was repeated three times and cooled to room temperature and transferred to a glove box. In the glove box, 10 mmol of bromine-substituted bridged lactone monomer was weighed and placed in ampoule No. 1. 2500 μl of redistilled toluene was added to dissolve it. 0.1 mmol of Bronsted base (DBU) and 0.1 mmol of (thio)urea (U 9) were weighed and placed in ampoule No. 2. 2490 μl of toluene was added to dissolve the catalyst. 0.01 mmol of benzyl alcohol was added and stirred at 25°C for 5 minutes. Finally, the dissolved monomer was added to the ampoule containing the catalyst and initiator to start polymerization.

[0081] After stirring at 25°C for 24 hours, 3-4 drops of the polymer solution were added to deuterated chloroform of benzoic acid to test the monomer conversion rate, and the rest was added to ice methanol dissolved with benzoic acid to quench and precipitate. After centrifugation at 10000r / min for 3 minutes, the supernatant was poured off, and a small amount of dichloromethane (DCM) was used to completely dissolve the polymer and added to ice methanol for precipitation. This was repeated three times, and the polymer product was placed in a drying dish and then vacuumed with a Schlenk device for 12 hours. The conversion rate was measured by the reaction solution. 1 The polymer structure and molecular weight were calculated by H NMR. 1 The polymer was identified by H NMR and its dispersion was determined by GPC. The conversion rate was 99%, the polymer number average molecular weight was 189220 g / mol, and the dispersion coefficient was 1.22.

[0082] Embodiment 8:

[0083] The two ampoules were evacuated with a Schlenk device and baked with a Bunsen burner to remove the residual moisture in the ampoules. After baking, argon was filled for protection. This process was repeated three times and cooled to room temperature and transferred to a glove box. In the glove box, 20 mmol of bromine-substituted bridged lactone monomer was weighed and placed in ampoule No. 1. 5000 μl of redistilled toluene was added to dissolve it. 0.2 mmol of Bronsted base (DBU) and 0.2 mmol of (thio)urea (U 9) were weighed and placed in ampoule No. 2. 4990 μl of toluene was added to dissolve the catalyst. 0.01 mmol of benzyl alcohol was added and stirred at 25°C for 5 minutes. Finally, the dissolved monomer was added to the ampoule containing the catalyst and initiator to start polymerization.

[0084] After stirring at 25°C for 24 hours, 3-4 drops of the polymer solution were added to deuterated chloroform of benzoic acid to test the monomer conversion rate, and the rest was added to ice methanol dissolved with benzoic acid to quench and precipitate. After centrifugation at 10000r / min for 3 minutes, the supernatant was poured off, and a small amount of dichloromethane (DCM) was used to completely dissolve the polymer and added to ice methanol for precipitation. This was repeated three times, and the polymer product was placed in a drying dish and then vacuumed with a Schlenk device for 12 hours. The conversion rate was measured by the reaction solution. 1 The polymer structure and molecular weight were calculated by H NMR. 1 The polymer was identified by H NMR and its dispersion was determined by GPC. The conversion rate was 98%, the polymer number average molecular weight was 374510 g / mol, and the dispersion coefficient was 1.24.

[0085] Embodiment 9:

[0086] The polymer prepared in Example 1 (0.5000 g), p-toluenesulfonic acid (2 mol%), and toluene (1 mL) were transferred to a pressure bottle and heated at 120° C. for 12 hours. The yield was determined by the reaction mixture. 1 The structure was obtained by H NMR calculation. 1 H NMR analysis showed that the product was a bromine-substituted bridged lactone monomer with a recovery rate of 70%.

[0087] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A bromine-functionalized polyester as shown in formula I; in, Y is selected from methoxy, ethoxy, isopropoxy, tert-butoxy, benzyloxy, phenylethoxy, phenylpropoxy, diphenylmethoxy, 2,2-diphenylethoxy; The number average molecular weight of the bromine-functionalized polyester is 2,000 to 400,000 g mol -1 .

2. The bromine-functionalized polyester according to claim 1, characterized in that The bromine-functionalized polyester is any one of formula II; 3. The method for preparing the bromine-functionalized polyester according to claim 1 or 2, characterized in that: The following steps are involved: Reaction of urea or thiourea represented by formula III, Bronsted base, solvent, initiator and bromine-substituted bridged ring lactone monomer represented by formula IV; in, X is selected from O or S; R 1 -R 4 Each independently selected from H, OMe, Cl, CF3; 4. The preparation method according to claim 2, characterized in that: In the urea or thiourea of ​​formula III; When X is selected from O, R 1 -R 4 The groups are: R 1 =OMe,R 2 -R 4 =H; or R 1 -R 4 =H; or R 1 = Cl, R 2 -R 4 = H; or R 1 =CF3, R 2 -R 4 =H; or R 1 -R 2 =CF3, R 3 -R 4 =H; or R 1 -R 3 =CF3, R 4 =H; or R 1 -R 4 =CF3; When X is selected from S, R 1 -R 4 =CF3.

5. The preparation method according to claim 2, characterized in that: The Bronsted base includes 1,5,7-triazabicyclo[4.4.0]dec-5-ene, diphenyl phosphate, 1,8-diazabicyclo[5.4.0]undec-7-ene, 1,3-di-mesityl imidazole-2-ylidene, and 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene.

6. The preparation method according to claim 2, characterized in that: The solvent is any one of toluene, tetrahydrofuran, dichloromethane and N,N-dimethylformamide.

7. The preparation method according to claim 2, characterized in that: The initiator is an alcohol; preferably, the initiator is any one of methanol, ethanol, isopropanol, tert-butanol, benzyl alcohol, phenylethanol, phenylpropanol, diphenylmethanol and 2,2-diphenylethanol.

8. The preparation method according to claim 2, characterized in that: The molar ratio of the bromine-substituted bridged lactone monomer represented by formula IV, the urea or thiourea represented by formula III, the Bronsted base, and the initiator is 10-2000:1-20:1-20:1; preferably, the reaction temperature is 25-100°C; and the reaction time is 5-1440 min.

9. The preparation method according to claim 2, characterized in that: The following steps are involved: The urea or thiourea shown in formula III, the Bronsted base, the solvent and the initiator are stirred first, and then the bromine-substituted bridged ring lactone monomer shown in formula IV is added for reaction; preferably, the stirring time is 1-8 minutes.

10. Use of the bromine-functional polyester according to claim 1 or 2 or the bromine-functional polyester prepared by the method according to any one of claims 3 to 9 in the preparation of chemically recyclable materials.

Citation Information

Patent Citations

  • Preparation method of polyester

    CN110092892A

  • Preparation method of bio-based copolyester containing modifiable functional group

    CN110804163A

  • Functionalized recyclable polymer homopolymer and preparation method and application thereof

    CN111253556A

  • Benzo five-membered and six-membered ring (thio) urea catalyst and application thereof in ring-opening polymerization

    CN111704714A

  • Method for preparing 3-bromobutyrate compound and 3-hydroxybutyrate compound by degrading poly-3-hydroxybutyrate