Preparation method of lignin with high phenolic hydroxyl content
Through high-temperature hydrothermal pretreatment and mechanical loosening of twin-screw extruders, combined with organic solvent extraction, the problems of complexity and pollution of existing lignin extraction methods are solved, the phenolic hydroxyl content and extraction rate of lignin are improved, and high efficiency is achieved. Environmentally friendly industrial production.
Patent Information
- Application Number
- CN202411293957.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-19
AI Technical Summary
The existing lignin extraction methods are complex and the reaction conditions are harsh, which leads to denaturation and reduced activity of lignin, which limits its efficient use. The existing processes produce pollution or equipment corrosion resistance requirements, making it difficult to achieve large-scale production.
High-temperature hydrothermal pretreatment breaks the cell wall structure, combines with a twin-screw extruder to perform mechanical loosening, increase the specific surface area of fiber raw materials, and extracts using ethanol or propanol as organic solvents to avoid the addition of additional acid and alkali chemical reagents and use recyclable Organic alcohol solvents achieve high phenolic hydroxyl content of lignin.
It improves the phenolic hydroxyl content and extraction rate of lignin, reduces energy consumption and pollution, simplifies the process flow, is suitable for industrial applications, and realizes the resource utilization of fiber raw materials.
Smart Images

Figure CN118978712A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of pulp papermaking and biomass resource utilization, and particularly relates to a method for preparing lignin with a high phenolic hydroxyl content. Background Art
[0002] The gradual reduction in reserves of non-renewable resources such as petroleum has led to dramatic price fluctuations in the global industry chain based on petrochemicals as raw materials, especially phenolic intermediates used in the production of daily chemicals. Finding, developing and using alternative resources from renewable biomass has become a research focus for scientific researchers. Lignin is an important component of forest and its residue resources. As the only renewable aromatic compound in nature, it has the advantages of wide sources, renewable and degradable. It is currently the only natural substance that can replace fossil raw materials to produce phenolic aromatic structural compounds. However, due to its complex three-dimensional network structure and complex structure-activity relationship with other components in the cell wall, its conversion and utilization are inhibited. Among the 150-200 million tons of lignin produced each year, most of them are burned as fuel or directly discarded and discharged into the natural environment to pollute the environment. The main reason is that the existing lignin separation and extraction process is complex and the reaction conditions are drastic, resulting in severe denaturation and reduced activity of lignin. When used in downstream fields, poor dispersibility and poor reaction activity limit the efficient utilization of lignin.
[0003] Phenolic hydroxyl is one of the important functional groups of lignin. It is small in size and highly reactive. Its content has a great influence on the physical and chemical properties of lignin. In practical applications, if the phenolic hydroxyl content of lignin can be greatly increased, lignin can be used to replace part of phenol to prepare some chemical necessities, which is of great significance for the efficient utilization of lignin and relieving the pressure on petroleum resources.
[0004] The main reported lignin extraction methods include alkali method, sulfite method, organic solvent method, etc. Alkali lignin is mainly extracted by hydrolyzing fiber raw materials under the action of alkali, which increases the solubility of lignin. This method produces a large amount of alkaline wastewater, which needs to be neutralized with acid, increasing the application cost; another lignin sulfonate is a by-product of the sulfite pulping process. The active functional groups of lignin are seriously lost and the introduction of sulfur elements leads to a narrower scope of subsequent use. It is generally used as a water-coal slurry dispersant, concrete water reducer, rubber wear agent and other low-end products; CN115216027A discloses a method for preparing lignin with a high phenolic hydroxyl content, using kraft lignin extracted from pulping black liquor as a raw material, and adding choline chloride 1,4-butanediol and urea in turn to react, followed by dialysis treatment to obtain lignin with a high phenolic hydroxyl content, but its maximum hydroxyl content is only 1.13mmol.g -1 , and the process is relatively complicated.
[0005] The organic solvent method is considered to be the best technology for separating lignin because the separated lignin has high activity and good solubility. CN 106633099A discloses a method for producing highly active lignin, which comprises: crushing the plant fiber raw material by a crusher to obtain wood powder that passes a 30-mesh standard sieve, first pre-treating it with an organic solvent, then using an organic acid aqueous solution as a cooking solvent, adding a catalyst to cook the pre-treated raw material, and extracting lignin from the cooking liquid after solid-liquid separation. This method has a relatively high lignin extraction rate and high purity, but crushing by a crusher is not suitable for large-scale production and has high energy consumption. The use of organic acid increases the corrosion resistance requirements of the equipment. The use of organic solvents such as benzene is highly toxic and not easy for large-scale production. Summary of the invention
[0006] Purpose of the invention: To address the deficiencies of the prior art, the purpose of the present invention is to provide a method for extracting lignin, which degrades the β-O-4 bonds in the raw material lignin in a step-by-step and direction manner, and increases the specific surface area of the fiber raw material by mechanical extrusion, and synergizes with an organic solvent to degrade and extract lignin. No additional chemical reagents such as acids and alkalis are added during the extraction process, and the only organic alcohol solvent used can be recycled. In addition, the use of a large-scale produced twin-screw extruder during the mechanical diameter reduction process is conducive to its industrial application.
[0007] In order to solve the above technical problems, the present invention discloses a method for preparing lignin with a high phenolic hydroxyl content, comprising the following steps:
[0008] (1) After measuring the moisture content of the raw wood, the raw wood is sent to a high temperature and high pressure resistant digester, the solid-liquid ratio is adjusted, and then a high temperature hydrothermal treatment is performed. After the reaction is completed, the hydrolyzate is filtered to obtain a pretreated material;
[0009] (2) The pretreated material obtained in step (1) is fed into a twin-screw extruder having screws running in opposite directions to process the material into filaments; specifically, fine filaments are formed under the combined action of the "extrusion-loosening" treatment and the shear force and friction force generated by the forward and reverse screws, and the purpose of quickly feeding the filaments into the twin-screw extruder is to remove the pseudo-lignin formed in the first hydrothermal process and reduce the obstacles to the extraction of lignin by organic solvents, and the amount of extrusion liquid is relatively small;
[0010] (3) The material obtained in step (2) is added to an organic solvent for lignin extraction, stirred and kept warm; after the reaction is completed, a Buchner funnel with a filter cloth is used for suction filtration, and then washed with an organic solvent, the washing liquid and the filtrate are combined and rotary evaporated to 40-50 mL, slowly poured into 800-1000 mL of deionized water, centrifuged to retain the solid part, and freeze-dried to obtain lignin with a polyphenolic hydroxyl content. Preferably, 100-150 mL of an organic solvent is used for washing three times, the washing liquid and the filtrate are combined and rotary evaporated to 40-50 mL, slowly poured into 800-1000 mL of deionized water, centrifuged to retain the solid part, and freeze-dried to obtain lignin with a polyphenolic hydroxyl content.
[0011] The raw material is broadleaf wood chips, and the size of the wood chips is 3-5 cm*3-5 cm*1 mm. In a specific embodiment, eucalyptus, poplar and other wood chips can be selected.
[0012] In step (1), the solid-liquid mass ratio is adjusted to 1:4 to 1:6.
[0013] Specifically, the conditions of high-temperature hydrothermal pretreatment are: heating to 160-180° C. and keeping warm for 30-120 minutes.
[0014] Preferably, in step (2), the twin-screw extruder with counter-rotating screws has an extrusion zone I and an extrusion zone II, wherein the spiral gap of the extrusion zone I is 40 mm, and the spiral gap of the extrusion zone II is 24 mm. After extrusion, the material is processed into filaments with a size of 0.18 mm to 0.425 mm in particle size and a moisture content of about 60%.
[0015] In step (3), the organic solvent is ethanol or propanol; the mass fraction of the organic solvent is 60% to 90%, and the absolutely dry material and the organic solvent are treated according to a solid-liquid mass ratio of 1:8 to 1:15.
[0016] Preferably, in step (3), the stirring speed is 100-300 r / min, the insulation temperature is 180-220° C., and the insulation time is 60-120 min.
[0017] Preferably, a Buchner funnel with filter cloth is used for suction filtration.
[0018] Further preferably, the filter cloth is a 400 mesh filter cloth.
[0019] Preferably, the hydrolyzate obtained in step (1) is used to extract xylooligosaccharides, thereby realizing resource utilization of fiber raw materials.
[0020] The principle of the present invention is as follows: firstly, hemicellulose is extracted by hydrothermal pretreatment, which can break the dense structure of the cell wall and form nanopores, which is conducive to the subsequent reaction; on the other hand, the fiber can be swollen and softened, which is conducive to reducing the energy consumption in the next step of "extrusion-loosening" mechanical pretreatment (twin-screw extruder); at the same time, by adjusting the hydrothermal treatment intensity factor, the β-O-4 bond of lignin in the fiber raw material is broken and the condensation of lignin is controlled as much as possible. This process can not only increase the phenolic hydroxyl content of lignin, but also help to increase the breaking of more β-O-4 bonds when extracting lignin with organic solvents, thereby increasing the phenolic hydroxyl content of the extracted lignin. After the steam release of the material after hydrothermal pretreatment is completed, the solid part is put into a twin-screw extruder while hot ("extrusion-loosening" process) for extrusion. Under the combined action of shear force, extrusion force and friction force, the particle size of the biomass raw material is reduced, its specific surface area is increased, and its reaction performance is improved; the lignin droplets ("pseudo-lignin") produced on the fiber surface by high-temperature hydrothermal pretreatment can be removed during the extrusion process, which is conducive to eliminating the obstruction of "pseudo-lignin" to organic solvents; finally, lignin is extracted with an alcohol-water solution, and the macromolecular lignin is depolymerized and the ether bond is broken under the action of autocatalytic ethanol to produce a large amount of lignin containing phenolic hydroxyl groups. The synergistic effect of hydrothermal and twin-screw extrusion can not only improve the lignin extraction rate, but also increase the phenolic hydroxyl content of lignin.
[0021] Beneficial effects: The present invention uses hydrothermal-mechanical extrusion-organic solvent to extract lignin from fiber raw materials. In the process, except for recyclable organic solvents such as ethanol, no additional chemicals are added, the pollution is small, and the corrosion resistance of the equipment is low. In this combined process, the hydrolyzate recovered by high-temperature hydrothermal pretreatment can extract by-products such as oligoxylose to realize the utilization of hemicellulose; at the same time, it can also reduce the energy consumption in the extrusion process. In addition, because the lignin of the present application is extracted with an organic solvent, it can be dissolved in most organic solvents, the extraction rate of lignin is improved, the purity of the extracted lignin is high, and the uniformity is good. The processes of hydrothermal treatment, mechanical extrusion treatment, and organic solvent extraction of lignin can be used with the help of existing mature pulping equipment and process flow to achieve large-scale production. This process flow is simple, the phenolic hydroxyl content of the obtained lignin is greatly improved, it has good organic solvent solubility and antioxidant properties, etc., and has broad market prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is the solid phase yield at different temperatures and holding times in the examples;
[0023] Figure 2 is the cellulose retention rate at different temperatures and holding times in the examples;
[0024] Figure 3 is the hemicellulose extraction rate at different temperatures and holding times in the examples;
[0025] Figure 4 is the lignin dissolution rate at different temperatures and holding times in the examples;
[0026] Figure 5 is the solid phase yield at different temperatures and holding times in Example 2;
[0027] Figure 6 is the cellulose retention rate at different temperatures and holding times in Example 2;
[0028] Figure 7 is the hemicellulose extraction rate at different temperatures and holding times in Example 2;
[0029] Figure 8 is the lignin dissolution rate at the same temperature and holding time in Example 2;
[0030] Fig. 9 Schematic diagram of the operation of a twin-screw extruder with counter-rotating screws. DETAILED DESCRIPTION
[0031] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.
[0032] High-temperature hydrothermal pretreatment has a great influence on the subsequent organic solvent extraction of lignin. In order to illustrate the importance of the hydrothermal conditions of the present invention, this paper uses the same ethanol extraction conditions to verify the influence of hydrothermal conditions on the extraction of lignin.
[0033] Example 1
[0034] The poplar wood is processed into wood chips of about 3cm*4cm*1mm in size, and sent to a high-temperature cooking pot. An appropriate amount of deionized water is added to adjust the solid-liquid mass ratio to 1:4, and the temperature is raised to different insulation temperatures (150, 160, 170, 180℃), and the temperature is kept at this temperature for different times (30, 60, 90, 120min). After the reaction is completed, the hydrolyzate is filtered (the hydrolyzate can be further used to extract oligoxylose). The hydrothermally treated wood chips are extruded in a twin-screw extruder with reverse-running screws while hot. Fine filaments are formed under the combined action of the "extrusion-loosening" treatment and the shear force and friction generated by the forward and reverse spirals, such as Fig. 9As shown, the twin-screw extruder with counter-rotating screws has an extrusion area I and an extrusion area II, the spiral gap of the extrusion area I is 40 mm, and the spiral gap of the extrusion area II is 24 mm. After extrusion, the material is processed into filaments with a size of 0.18 mm to 0.425 mm particles. The moisture content of the material after extrusion is measured, and the moisture content is about 60%. Then, ethanol is used to extract lignin. The effects of different hydrothermal treatment conditions on the dissolution rate of hemicellulose, the dissolution rate of lignin and the retention rate of cellulose are analyzed (see Figure 1-Figure 4 ); extract the ground wood lignin of the raw material and the materials after hydrothermal treatment under different conditions, and analyze the effect of hydrothermal treatment on the structure of raw material lignin (see Table 2).
[0035] The ethanol extraction method is: 10 grams of absolute dry solid (raw material and material after hydrothermal treatment), 50% ethanol mass fraction, solid-liquid ratio 1:10, stirring speed 200r / min, insulation temperature 200°C, insulation time 120min. After the reaction is completed, use a Buchner funnel with a 400-mesh filter cloth for suction filtration, wash with 150mL of 50% ethanol solution three times, combine the washing liquid and the filtrate and evaporate to 50mL, slowly pour into 1000mL of deionized water, centrifuge to retain the solid part, and freeze-dry to obtain poplar lignin EPE.
[0036] From the perspective of effective utilization of the three major components of biomass resources, the more hemicellulose is dissolved during the hydrothermal treatment, the more beneficial it is for the extraction and utilization of hemicellulose, and the more lignin and cellulose are retained, the higher the extraction rate can be when the next component is extracted and utilized. According to the hydrothermal optimization results, the dissolution rate of hemicellulose is basically the same when the treatment conditions of 170℃ for 60min and 180℃ for 90min are treated, achieving the highest hemicellulose extraction rate, but the retention rates of lignin and cellulose are significantly different. Therefore, we believe that for this hardwood, 170℃ for 60min is a more suitable hydrothermal treatment condition.
[0037] After the materials were treated under different hydrothermal treatment conditions, the ground wood lignin was extracted and its molecular weight and connecting bonds were analyzed (see Table 1). It can be seen that the degree of β-O-4 bond breaking was different under different intensity treatment conditions. With the increase of temperature, not only the β-O-4 bond was broken, but also the polymerization reaction of lignin molecules increased, and the degree of condensation increased, which is also the main reason for the increase of lignin molecular weight. The condensed lignin is not conducive to the extraction of lignin and the increase of phenolic hydroxyl content, so the condensation of lignin should be avoided as much as possible.
[0038] Table 1 Effects of different hydrothermal treatment conditions on lignin structure of poplar
[0039]
[0040]
[0041] In order to verify the effectiveness of the combination, three control group experiments were conducted:
[0042] Control experiment 1: The poplar wood chips were not treated in any way, and lignin was directly extracted using the above-mentioned ethanol extraction conditions. The obtained lignin was labeled as PC;
[0043] Control experiment 2: After the above hydrothermal pretreatment, the poplar wood chips were washed with deionized water, and the hydrothermal pretreated wood chips were subjected to lignin extraction according to the above ethanol lignin extraction conditions, and the obtained lignin was labeled as PP (the lignin extracted under different hydrothermal treatment conditions were labeled as PP150, PP160, PP170, and PP180 respectively);
[0044] Control experiment 3: Poplar wood chips were directly extruded into a twin-screw extruder to obtain extruded wood fibers. Lignin was extracted according to the above lignin extraction conditions, and the obtained lignin was labeled as PE.
[0045] The properties of the above lignin were measured, and the results are shown in Table 2 and Table 3.
[0046] Determination of phenolic hydroxyl content: 20 mg of unacetylated lignin was dissolved in 0.5 mL of anhydrous pyridine-d5 / CDCl3 (1.6 / 1, v / v) solution, and then 100 μL of cyclohexanol (11.02 mg / mL, internal standard) and 100 μL of acetylacetonate chromium (III) (5 mg / mL, relaxant) prepared using anhydrous pyridine-d5 / CDCl3 solution were mixed with the lignin solution, and then 60 μL of phosphating reagent (2-chloro-4,4,5,5-tetramethyl-1,2,3-dioxaphosphine) was added. After shaking at room temperature for 30 minutes, the mixture was immediately analyzed on a BrukerAVANCE 600 MHz (Switzerland) spectrometer.
[0047] Molecular weight determination: The lignin samples were dissolved in tetrahydrofuran (THF, HPLC grade) at a concentration of 1 mg / mL and the molecular weight of lignin was determined by LC-20A GPC (Shimadzu Corporation, Japan) using an organic exclusion chromatography column (KF-804, 300 mm×8 mm id, 7 μm). The detection column temperature was operated at 40°C and calibrated with polystyrene standards (peak average molecular weight (Mw) of 43600, 30000, 10000, 4050 and 2400 g / mol), eluted with chromatography grade furan at a flow rate of 1 mL / min.
[0048] Specific surface area determination: the raw materials, raw materials after hydrothermal treatment, and raw materials after extrusion are crushed into 40-60 mesh wood powder by a pulverizer and then tested. The raw materials after hydrothermal coupling mechanical extrusion are directly tested. About 100 mg of powder is weighed and placed in an American Mack specific surface area meter (model: ASAP 2020) at 120°C for degassing (degassing time: 18h), then cooled and tested in a nitrogen atmosphere.
[0049] Table 2 Pore size, pore volume and specific surface area of different pretreated fibers
[0050]
[0051]
[0052] Table 3 Analysis of lignin structure extracted from poplar wood under different pretreatment conditions
[0053]
[0054] It can be seen from Table 2 that the specific surface area of the poplar wood chips can be increased after different treatments. The specific surface area and pore size increase the most after hydrothermal coupling mechanical extrusion pretreatment, which is conducive to the penetration of the liquid medicine and the reaction. This is also the main reason for the subsequent increase in extraction rate (see Table 3).
[0055] From the control experiment 2 in Table 3, it can be seen that the phenolic hydroxyl content of lignin extracted by ethanol is different after hydrothermal treatment at different temperatures and times. It can be seen from Table 1 that there is a certain correlation with the degree of breakage of β-O-4 bond of lignin during hydrothermal treatment. After hydrothermal coupled mechanical extrusion pretreatment, the phenolic hydroxyl content of lignin extracted by ethanol increased the most (170℃, 60min).
[0056] Example 2
[0057] The eucalyptus wood was processed into wood chips of about 3cm*4cm*1mm in size, and sent to a high-temperature cooking pot. An appropriate amount of deionized water was added to adjust the solid-liquid mass ratio to 1:6, and the temperature was raised to different insulation temperatures (150, 160, 170, 180°C), and the temperature was kept at this temperature for different times (30, 60, 90, 120min). After the reaction, the hydrolyzate was filtered (the hydrolyzate can be further used to extract oligoxylose). The hydrothermally treated wood chips were extruded in a twin-screw extruder with reverse-running screws while hot. Fine filaments were formed under the combined action of the shear force and friction generated by the "extrusion-loosening" treatment and the forward and reverse spirals. The moisture content of the material after extrusion was measured, and lignin was extracted using ethanol. The effects of different hydrothermal treatment conditions on the hemicellulose dissolution rate, lignin dissolution rate and cellulose retention rate were analyzed (see Figure 5-8); extract the ground wood lignin of the raw material and the materials after hydrothermal treatment under different conditions, and analyze the effect of hydrothermal treatment on the structure of raw material lignin (see Table 3).
[0058] Specifically, 10 grams of absolute dry solid, 80% ethanol mass fraction, solid-liquid ratio 1:15, stirring speed 200r / min, insulation temperature 200°C, insulation time 120min. After the reaction is completed, use a Buchner funnel with a 400-mesh filter cloth for suction filtration, wash with 150mL of 80% ethanol solution three times, combine the washing liquid and the filtrate and evaporate to 50mL, slowly pour into 1000mL of deionized water, centrifuge to retain the solid part, and freeze-dry to obtain poplar lignin EPE.
[0059] According to the hydrothermal optimization results, it can be seen that ( Figure 5-8 ), eucalyptus and poplar raw materials showed similar properties. The dissolution rates of hemicellulose were basically the same when treated at 170℃ for 60min and 180℃ for 90min, achieving the highest hemicellulose extraction rate, but the retention rates of lignin and cellulose were significantly different. Therefore, we believe that for hardwood, 170℃ for 60min is a more suitable hydrothermal treatment condition.
[0060] After the materials were treated under different hydrothermal treatment conditions, their ground wood lignin was extracted and their molecular weight and connecting bonds were analyzed (see Table 4). It can be seen that the performance properties are similar to those of poplar wood mentioned above. The degree of β-O-4 bond breaking is different under different strength conditions. With the increase of temperature, not only the β-O-4 bond breaks, but also the polymerization reaction of lignin molecules increases, and the degree of shrinkage increases. This is also the main reason for the increase in lignin molecular weight.
[0061] Table 4 Effects of different hydrothermal pretreatments of eucalyptus on lignin structure
[0062]
[0063] In order to verify the effectiveness of the combination, three control group experiments were conducted:
[0064] Control experiment 1: The eucalyptus chips were not treated in any way, and lignin was directly extracted using the above-mentioned ethanol extraction conditions. The obtained lignin was labeled as EC;
[0065] Control experiment 2: After the above hydrothermal pretreatment, the poplar wood chips were washed with deionized water, and the hydrothermal pretreated wood chips were subjected to lignin extraction according to the lignin extraction conditions, and the obtained lignin was labeled as EP (the lignin extracted under different hydrothermal treatment conditions were labeled as EP150, EP160, EP170, and EP180, respectively);
[0066] Control experiment 3: Poplar wood chips were directly extruded into a twin-screw extruder to obtain extruded wood fibers. Lignin was extracted according to the above lignin extraction conditions, and the obtained lignin was marked as EE.
[0067] The results of the above experiment are shown in Table 6.
[0068] Table 5 Pore size, pore volume and specific surface area of different pretreated fibers
[0069]
[0070] Table 6 Analysis of lignin structure extracted from eucalyptus under different pretreatment conditions
[0071]
[0072] It can be seen from Table 5 that the specific surface area of the eucalyptus wood chips can be increased by different pretreatments. The specific surface area and pore size increase the most after hydrothermal coupling mechanical extrusion pretreatment, which is conducive to the penetration of the liquid medicine and the reaction. This is also the main reason for the subsequent increase in extraction rate (see Table 6).
[0073] From the control experiment 2 in Table 6, it can be seen that after hydrothermal treatment at different temperatures and different times, the phenolic hydroxyl content of lignin extracted by ethanol is also different. From Table 4, it can be seen that the degree of lignin β-O-4 bond breakage is similar to that of poplar wood when eucalyptus is hydrothermally treated. After hydrothermal coupled mechanical extrusion pretreatment, the phenolic hydroxyl content of lignin extracted by ethanol increases the most (170℃, 60min).
[0074] The present invention provides a preparation idea and method of lignin with high phenolic hydroxyl content. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.
Claims
1. A method for preparing lignin with high phenolic hydroxyl content, characterized in that: The steps include: (1) After the moisture content of the raw wood is measured, it is sent to a high temperature and high pressure resistant digester, the solid-liquid ratio is adjusted, and then a high temperature hydrothermal treatment is performed. After the reaction is completed, the hydrolyzate is filtered to obtain a pretreated material; (2) The pretreated material obtained in step (1) is fed into a twin-screw extruder having screws running in opposite directions to process the material into granular filaments; (3) The material obtained in step (2) is added to an organic solvent for lignin extraction, stirred and kept warm; after the reaction is completed, the mixture is filtered using a Buchner funnel with filter cloth, then washed with an organic solvent, the washing liquid and the filtrate are combined and rotary evaporated to 40-50 mL, slowly poured into 800-1000 mL of deionized water, centrifuged to retain the solid part, and freeze-dried to obtain lignin with a polyphenol hydroxyl content.
2. The preparation method according to claim 1, characterized in that: The raw material is broadleaf wood chips with a size of 3~5cm*3~5cm*1mm.
3. The preparation method according to claim 1, characterized in that: In step (1), the solid-liquid ratio is adjusted to 1:4-1:
6.
4. The preparation method according to claim 1, characterized in that: The conditions of high-temperature hydrothermal pretreatment are: heating to 160~180℃ and keeping warm for 30~120min.
5. The preparation method according to claim 1, characterized in that: In step (2), the twin-screw extruder with counter-rotating screws has an extrusion area I and an extrusion area II, wherein the spiral gap of the extrusion area I is 40 mm, and the spiral gap of the extrusion area II is 24 mm. After extrusion, the material is processed into granular filaments with a size of 0.18 mm to 0.425 mm.
6. The preparation method according to claim 1, characterized in that: In step (3), the organic solvent is ethanol or propanol; the mass fraction of the organic solvent is 60% to 90%, and the absolutely dry material and the organic solvent are treated according to a solid-liquid mass ratio of 1:8 to 1:
15.
7. The preparation method according to claim 1, characterized in that: In step (3), the stirring speed is 100-300 r / min, the insulation temperature is 180-220°C, and the insulation time is 60-120 min.
8. The preparation method according to claim 4, characterized in that: Use a Buchner funnel and filter cloth for suction filtration, the filter cloth is 400 mesh filter cloth.
9. The preparation method according to claim 1, characterized in that: The hydrolyzate obtained in step (1) is used to extract xylo-oligosaccharides.
Citation Information
Patent Citations
Production method for high-activity lignin
CN106633099A
Preparation method of lignin with high phenolic hydroxyl content
CN115216027A