Asphalt dry-process direct-feeding modifier capable of being quickly melted and preparation method thereof
By using butadiene-styrene-butadiene block copolymer and rubber powder in dry asphalt modifiers, combining stabilizers and surfactants, the uneven dispersion of dry modifiers and the uneven dispersion of dry modifiers is solved. The problem of slow melting speed achieves rapid melting and efficient modification, significantly improving the performance and service life of asphalt pavement.
Patent Information
- Application Number
- CN202411283365.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-19
AI Technical Summary
The existing dry asphalt modifiers have problems such as uneven dispersion, slow melting speed and low modification efficiency, resulting in poor performance of the asphalt mixture, long construction time and high energy consumption.
The butadiene-styrene-butadiene block copolymer and rubber powder are used as the modification body. Through the action of stabilizers and coupling agents, the compatibility and molecular linkage of the modifier are enhanced, and the surfactant and Plasticizer achieves rapid melting and uniform dispersion, and optimizes the component content and preparation process of the modifier.
It significantly improves the melting rate and modification efficiency of asphalt modifiers, reduces production energy consumption and material costs, extends the service life of asphalt pavement, and improves water damage resistance and pavement performance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to a novel asphalt polymer modifier, in particular to a fast-melting asphalt dry-process direct-throw modifier and a preparation method thereof. Background Art
[0002] In some hot and rainy areas and in the construction of high-grade asphalt pavements, ordinary base asphalt can no longer meet the pavement requirements, and modified asphalt is needed to meet the high-temperature rutting resistance, low-temperature cracking resistance and other properties. The development of asphalt modification technology has significantly improved the performance of asphalt pavements in various environments.
[0003] With the improvement of road performance requirements and the advancement of industrial technology, new materials and new technologies have been applied more and more on the basis of traditional asphalt modification technology in recent years, and composite modification and functional modification technologies have also emerged. At present, asphalt modification mainly adopts two technologies: wet method and dry method. Although wet modification technology can effectively improve the performance of asphalt, its production process is complicated, the cost is high, and special equipment is required for high-temperature mixing, which limits its wide application. In contrast, dry modification technology has the advantages of simple operation and low cost. By directly adding solid modifiers to asphalt mixtures, the modifier and asphalt are mixed. However, existing dry modifiers have problems such as uneven dispersion, insufficient bonding with asphalt, and slow melting speed, all of which will affect the performance of the final asphalt mixture.
[0004] In view of these deficiencies in the prior art, the present invention proposes a fast-melting asphalt dry-cast modifier. The modifier is designed with special materials and processing technology, which can quickly melt and evenly disperse in the asphalt and aggregate under the temperature and pressure conditions of conventional asphalt paving, thereby significantly improving the efficiency of the asphalt modifier. The modifier can also provide better resistance to water damage and extend the service life of asphalt pavement, with significant economic benefits and social value. Compared with the existing road dry-cast polymer modifier technology, the fast-melting asphalt dry-cast modifier requires a short preparation time and a low preparation temperature, which shortens the construction time and reduces construction energy consumption. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide a fast-melting asphalt dry direct-addition modifier and a preparation method thereof, so as to improve the problems of complex preparation procedures, long time consumption, high energy consumption, uneven mixing with asphalt mixture during use, and low modification efficiency of the modifier in ordinary asphalt dry direct-addition modifiers.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A fast-melting asphalt dry-process direct-injection modifier, the raw materials of which include the following components in parts by weight:
[0008]
[0009] The present invention uses two common modified materials, butadiene-styrene-butadiene block copolymer and rubber powder, as the modified main body. In order to achieve the purpose of rapid melting and rapid dispersion in asphalt mixture, it is necessary to improve the compatibility between the two modified materials and reduce the overall surface activity of the direct-cast modifier, so that the modified particles can be dispersed in a short time when in contact with the asphalt mixture during use and produce a similar "self-leveling" effect on the stone or asphalt surface. At the same time, it is also necessary to be highly compatible with the matrix asphalt and undergo a cross-linking reaction at a normal stirring temperature and a short stirring time to maximize the modification effect.
[0010] In order to achieve the above modification effect, the present invention selects butadiene-styrene-butadiene block copolymer materials with suitable molecular weight and rubber powder particles with moderate particle size as the modification main body, and enhances the molecular link between the two types of polymer modifiers, as well as the compatibility and dispersibility between the modifier and the matrix asphalt through the joint action of the stabilizer and the coupling agent. Under the action of the preferred surfactant and other additives, micro mutual repulsion will be generated between the particles, preventing agglomeration on the surface of the asphalt mixture, and achieving the effect of rapid melting and effective modification, improving the shortcomings of uneven dispersion of the modifier, slow melting speed, and low modification efficiency of the traditional dry direct casting modifier.
[0011] The content of each component of the fast-melting asphalt dry direct-throw modifier in the present invention should be within the range mentioned in the technical scheme. The range requirements of the content of each component in the technical scheme are based on experimental results. If the content ratio of the stabilizer and coupling agent to the modified main additive is too low, the two types of modified main additives will not be able to produce stable crosslinking, causing part of the butadiene-styrene-butadiene block copolymer and the rubber powder particles to become independent units, which not only wastes the modifier material, but also easily causes the solid modifier to agglomerate in the asphalt mixture; if the content ratio of the stabilizer and coupling agent to the modified main additive is too high, it will cause excessive crosslinking between the modifier bodies, which will also cause the agglomeration effect of the modifier particles. The use of the component content requirements of this scheme can maximize the melting rate and modification efficiency of the modifier and the asphalt mixture, while reducing the production energy consumption of the modifier, reducing the material cost, and achieving the unity of the melting rate, modification efficiency and economy of the dry direct-throw polymer modifier.
[0012] The butadiene-styrene-butadiene block copolymer is a star-shaped SBS with a molecular weight of 150,000 to 200,000.
[0013] The particle size of the rubber powder is 150-200 meshes.
[0014] There are two types of stabilizers, namely, sulfur stabilizer and nano cerium oxide.
[0015] The plasticizer is diisooctyl sebacate.
[0016] The surfactant is polyglyceryl-6 stearate.
[0017] The present invention also provides a method for preparing a fast-melting asphalt dry direct-injection modifier, comprising the following steps:
[0018] (1) subjecting the butadiene-styrene-butadiene block copolymer to high-speed shearing for standby use;
[0019] (2) adding rubber powder and diisooctyl sebacate to the butadiene-styrene-butadiene block copolymer obtained in step (1), and mixing them uniformly;
[0020] (3) heating the mixture, adding a plasticizer, and performing high-temperature plasticizing;
[0021] (4) adding a stabilizer, a coupling agent and a surfactant to the material obtained in step (3) and mixing them;
[0022] (5) The product obtained in step (4) is granulated by high-temperature melt extrusion through a single-screw extruder, and the granular product is ground to obtain the asphalt dry direct injection modifier that can be melted quickly.
[0023] In step (1), the rotation speed of the high-speed shearing machine is 3000-4000 rpm; the shearing treatment time is 20-40 minutes;
[0024] In the step (3), the temperature of mixing and heating the butadiene-styrene-butadiene block copolymer, rubber powder and diisooctyl sebacate is 180-200°C, and then polyglycerol-6 stearate is added. The plasticizing temperature is 120°C-150°C, and the plasticizing time is 3-8 minutes;
[0025] In the step (4), the mixing temperature is 80° C.-100° C., and the mixing time is 2-5 minutes.
[0026] The step (5) is specifically as follows: preparing a granular product with a particle size of less than 2 mm by high-temperature melt extrusion granulation using a single screw extruder. Finally, the granular product is ground to obtain a dry direct injection modifier with a particle size of less than 20 microns.
[0027] Preferably, the selected butadiene-styrene-butadiene block copolymer is a star-shaped SBS with a molecular weight of 160,000;
[0028] The particle size of the selected rubber powder is 180 mesh;
[0029] The polymer grafted or copolymerized with maleic anhydride is a maleic anhydride grafted polymer;
[0030] In step (1), the rotation speed of the high-speed shearing machine is 4000 rpm; the shearing treatment time is 40 minutes;
[0031] In step (3), the temperature at which the butadiene-styrene-butadiene block copolymer, rubber powder and diisooctyl sebacate are mixed and heated is 180°C. After the temperature drops to 120°C, polyglycerol-6 stearate is added, the plasticizing temperature is 120°C, and the plasticizing time is 4 minutes;
[0032] In step (4), the mixing temperature is 100° C. and the mixing time is 3 minutes.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] (1) The selected butadiene-styrene-butadiene block copolymer is a star-shaped SBS with a molecular weight of 150,000 to 200,000. Compared with linear SBS, the use of star-shaped SBS for modification can enhance the viscosity and elastic properties of asphalt to a greater extent. The molecular weight should not be too large or too small, because it is necessary to simultaneously meet the modification effect and the dispersion effect of the modifier in the asphalt mixture.
[0035] (2) The mesh size of the selected rubber powder is 150-200 meshes. The rubber powder with fine meshes has a larger surface area. Under the action of coupling agent and other additives, it can more fully cross-link with butadiene-styrene-butadiene block copolymer. In addition to being able to form a network structure similar to butadiene-styrene-butadiene block copolymer, the refined rubber powder microparticles can act as reinforcing nodes in the network structure, enhancing the elasticity and toughness of the structure. At the same time, smaller microparticles are also more conducive to the dispersion of dry modifiers in the direct modification process.
[0036] (3) The selected stabilizers are sulfur stabilizer and nano-cerium oxide. Sulfur is a commonly used stabilizer for butadiene-styrene-butadiene block copolymers, and its stabilizing effect has been proven by many years of practice. Nano-cerium oxide has good crystal form, good dispersibility and transparency, and good compatibility with polymers. Nano-cerium oxide is an effective inorganic active agent and vulcanization accelerator for rubber materials. It can greatly improve the cross-linking of rubber and butadiene-styrene-butadiene block copolymers, improve density, and ensure the stability of the two without causing segregation and agglomeration problems.
[0037] (4) Using the plasticizer diisooctyl sebacate, this material has high plasticizing efficiency, low volatility, excellent cold resistance, and good heat resistance. When diisooctyl sebacate molecules are added to the polymer, they will be inserted between the polymer molecular chains and between them and the rubber microparticles, weakening the stress between the polymer molecular chains, increasing the mobility of the molecular chains, and reducing their crystallinity, thereby effectively improving plasticity.
[0038] (5) The polymer grafted or copolymerized with maleic anhydride has both polar group aldehyde group and olefin non-polar segment. In the present invention, chemical bonding can be carried out between the polymer and the filler under the action of melting or screw shearing, and a generalized dehydration reaction occurs with the polar group, thereby chemically coupling the incompatible polar and non-polar substances to achieve a combination of strength and toughness. The cost and dosage of the polymer grafted or copolymerized with maleic anhydride are extremely low, and it also has a toughening effect. After mixing with the raw materials, it does not need to undergo a long swelling process and can take effect in a short time.
[0039] (6) The addition of surfactant polyglycerol-6 stearate reduces the surface activity of the dry direct injection modifier in the molten state, allowing it to disperse and stabilize in the asphalt mixture as quickly as possible. At the same time, it reduces the interaction between the star-shaped SBS molecules and the interaction between the star-shaped SBS molecules and the rubber powder, preventing the modifier from agglomerating.
[0040] (7) In the preparation method of the fast-melting asphalt dry direct-injection modifier provided by the present invention, the temperature and time of plasticizing and mixing are the optimal solutions after multiple experiments. If the temperature is too high or the time is too long, it will cause the degradation of butadiene-styrene-butadiene block copolymer and rubber powder, affect the formation of the network structure, and greatly increase the production energy consumption and cost; if the temperature of plasticizing and mixing is too low or the time is too short, it will lead to incomplete plasticizing and mixing, reducing the modification efficiency. DETAILED DESCRIPTION
[0041] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0042] Comparative Example 1
[0043] This comparative example is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 90 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 0.5 parts of a sulfur stabilizer; 0.5 parts of nano-cerium oxide; 3 parts of diisooctyl sebacate; 3 parts of a maleic anhydride grafted polymer; and 3 parts of polyglycerol-6 stearate.
[0044] The preparation method is as follows:
[0045] The butadiene-styrene-butadiene block copolymer is sheared at a high speed of 4000 rpm for 40 minutes, and mixed with diisooctyl sebacate at 180°C. After uniform mixing, polyglycerol-6 stearate is added, and high-temperature plasticization is performed at 120°C for 4 minutes to obtain an intermediate product. Sulfur stabilizer, nano-cerium oxide, maleic anhydride grafted polymer and polyglycerol-6 stearate are added to the intermediate product, and after mixing at 100°C for 3 minutes, a granular product with a particle size of less than 2 mm is prepared by high-temperature melt extrusion granulation with a single screw extruder. Finally, the granular product is ground to obtain a dry direct injection modifier with a particle size of less than 20 microns.
[0046] Comparative Example 2
[0047] This comparative example is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 50 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 40 parts of 180-mesh rubber powder; 1 part of a sulfur stabilizer; 2 parts of diisooctyl sebacate; 3 parts of a maleic anhydride grafted polymer; and 4 parts of polyglycerol-6 stearate.
[0048] The preparation method is as follows:
[0049] The butadiene-styrene-butadiene block copolymer is sheared at a high speed of 4000 rpm for 40 minutes, and mixed with rubber powder and diisooctyl sebacate at 180°C. After uniform mixing, polyglycerol-6 stearate is added, and high-temperature plasticization is performed at 120°C for 4 minutes to obtain an intermediate product. Sulfur stabilizer, maleic anhydride grafted polymer and polyglycerol-6 stearate are added to the intermediate product, and after mixing at 100°C for 3 minutes, a granular product with a particle size of less than 2 mm is prepared by high-temperature melt extrusion granulation with a single screw extruder. Finally, the granular product is ground to obtain a dry direct injection modifier with a particle size of less than 20 microns.
[0050] Comparative Example 3
[0051] This comparative example is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 45 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 45 parts of 180-mesh rubber powder; 1 part of a sulfur stabilizer; 0.5 parts of nano-cerium oxide; 3.5 parts of diisooctyl sebacate; and 5 parts of polyglycerol-6 stearate.
[0052] The preparation method is as follows:
[0053] The butadiene-styrene-butadiene block copolymer is sheared at a high speed of 4000 rpm for 40 minutes, and mixed with rubber powder and diisooctyl sebacate at 180°C. After uniform mixing, polyglycerol-6 stearate is added, and high-temperature plasticization is performed at 120°C for 4 minutes to obtain an intermediate product. Sulfur stabilizer, nano-cerium oxide and polyglycerol-6 stearate are added to the intermediate product, and after mixing at 100°C for 3 minutes, a granular product with a particle size of less than 2 mm is prepared by high-temperature melt extrusion granulation with a single screw extruder. Finally, the granular product is ground to obtain a dry direct injection modifier with a particle size of less than 20 microns.
[0054] Comparative Example 4
[0055] This comparative example is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 50 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 40 parts of 180-mesh rubber powder; 0.5 parts of a sulfur stabilizer; 0.5 parts of nano-cerium oxide; 4 parts of diisooctyl sebacate; 2 parts of a maleic anhydride grafted polymer; and 3 parts of polyglycerol-6 stearate.
[0056] The preparation method is as follows:
[0057] The butadiene-styrene-butadiene block copolymer is sheared at a high speed of 4000 rpm for 20 minutes, and mixed with rubber powder and diisooctyl sebacate at 150°C. After uniform mixing, polyglycerol-6 stearate is added, and high-temperature plasticization is performed at 100°C for 15 minutes to obtain an intermediate product. Sulfur stabilizer, nano-cerium oxide, maleic anhydride grafted polymer and polyglycerol-6 stearate are added to the intermediate product, and after mixing at 60°C for 10 minutes, a granular product with a particle size of less than 2 mm is prepared by high-temperature melt extrusion granulation with a single screw extruder. Finally, the granular product is ground to obtain a dry direct injection modifier with a particle size of less than 20 microns.
[0058] Comparative Example 5
[0059] This comparative example is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 50 parts of a linear butadiene-styrene-butadiene block copolymer with a molecular weight of 80,000; 40 parts of 60-mesh rubber powder; 0.5 parts of a sulfur stabilizer; 0.5 parts of nano-cerium oxide; 4 parts of diisooctyl sebacate; 2 parts of a maleic anhydride grafted polymer; and 3 parts of polyglycerol-6 stearate.
[0060] The preparation method is as follows:
[0061] The butadiene-styrene-butadiene block copolymer is sheared at a high speed of 4000 rpm for 40 minutes, and mixed with rubber powder and diisooctyl sebacate at 180°C. After uniform mixing, polyglycerol-6 stearate is added, and high-temperature plasticization is performed at 120°C for 4 minutes to obtain an intermediate product. Sulfur stabilizer, nano-cerium oxide, maleic anhydride grafted polymer and polyglycerol-6 stearate are added to the intermediate product, and after mixing at 100°C for 3 minutes, a granular product with a particle size of less than 2 mm is prepared by high-temperature melt extrusion granulation with a single screw extruder. Finally, the granular product is ground to obtain a dry direct injection modifier with a particle size of about 40 microns.
[0062] Comparative Example 6
[0063] This comparative example is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 50 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 40 parts of 180-mesh rubber powder; 0.5 parts of a sulfur stabilizer; 0.5 parts of nano-cerium oxide; 4 parts of diisooctyl sebacate; 2 parts of a maleic anhydride grafted polymer; and 3 parts of polyglycerol-6 stearate.
[0064] The preparation method is as follows:
[0065] The butadiene-styrene-butadiene block copolymer is sheared at a high speed of 2000 rpm for 15 minutes, and mixed with rubber powder and diisooctyl sebacate at 180°C. After uniform mixing, polyglycerol-6 stearate is added, and high-temperature plasticization is performed at 120°C for 4 minutes to obtain an intermediate product. Sulfur stabilizer, nano-cerium oxide, maleic anhydride grafted polymer and polyglycerol-6 stearate are added to the intermediate product, and after mixing at 100°C for 3 minutes, a granular product with a particle size of less than 2 mm is prepared by high-temperature melt extrusion granulation with a single screw extruder. Finally, the granular product is ground to obtain a dry direct injection modifier with a particle size of less than 20 microns.
[0066] Comparative Example 7
[0067] This comparative example is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 47 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 40 parts of 150-200 mesh rubber powder; 0.5 parts of a sulfur stabilizer; 0.5 parts of nano-cerium oxide; 3 parts of diisooctyl sebacate; 6 parts of a maleic anhydride grafted polymer; and 3 parts of polyglycerol-6 stearate.
[0068] The preparation method is as follows:
[0069] The butadiene-styrene-butadiene block copolymer is sheared at a high speed of 2000 rpm for 15 minutes, and mixed with rubber powder and diisooctyl sebacate at 150°C. After uniform mixing, polyglycerol-6 stearate is added, and high-temperature plasticization is performed at 100°C for 15 minutes to obtain an intermediate product. Sulfur stabilizer, nano-cerium oxide, maleic anhydride grafted polymer and polyglycerol-6 stearate are added to the intermediate product, and after mixing at 60°C for 10 minutes, a granular product with a particle size of less than 2 mm is prepared by high-temperature melt extrusion granulation with a single screw extruder. Finally, the granular product is ground to obtain a dry direct injection modifier with a particle size of less than 20 microns.
[0070] Example 1
[0071] The present embodiment is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 45 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 40.5 parts of 180-mesh rubber powder; 1 part of a sulfur stabilizer; 0.5 parts of nano-cerium oxide; 4 parts of diisooctyl sebacate; 4 parts of a maleic anhydride grafted polymer; and 5 parts of polyglycerol-6 stearate.
[0072] The preparation method is as follows:
[0073] The butadiene-styrene-butadiene block copolymer is sheared at a high speed of 4000 rpm for 40 minutes, and mixed with rubber powder and diisooctyl sebacate at 180°C. After uniform mixing, polyglycerol-6 stearate is added, and high-temperature plasticization is performed at 120°C for 4 minutes to obtain an intermediate product. Sulfur stabilizer, nano-cerium oxide, maleic anhydride grafted polymer and polyglycerol-6 stearate are added to the intermediate product, and after mixing at 100°C for 3 minutes, a granular product with a particle size of less than 2 mm is prepared by high-temperature melt extrusion granulation with a single screw extruder. Finally, the granular product is ground to obtain a dry direct injection modifier with a particle size of less than 20 microns.
[0074] Example 2
[0075] The present embodiment is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 50 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 40 parts of 180-mesh rubber powder; 1 part of a sulfur stabilizer; 0.5 parts of nano-cerium oxide; 2 parts of diisooctyl sebacate; 2 parts of a maleic anhydride grafted polymer; and 4.5 parts of polyglycerol-6 stearate.
[0076] The preparation method is as follows:
[0077] The preparation method of the fast-melting asphalt dry direct-injection modifier is the same as the preparation method in Example 1.
[0078] Example 3
[0079] The present embodiment is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 45 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 45 parts of 180-mesh rubber powder; 1 part of a sulfur stabilizer; 0.5 parts of nano-cerium oxide; 2 parts of diisooctyl sebacate; 2 parts of a maleic anhydride grafted polymer; and 4.5 parts of polyglycerol-6 stearate.
[0080] The preparation method is as follows:
[0081] The preparation method of the fast-melting asphalt dry direct-injection modifier is the same as the preparation method in Example 1.
[0082] Example 4
[0083] The present embodiment is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 47.7 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 45 parts of 180-mesh rubber powder; 0.2 parts of a sulfur stabilizer; 0.1 parts of nano-cerium oxide; 2 parts of diisooctyl sebacate; 2 parts of a maleic anhydride grafted polymer; and 3 parts of polyglycerol-6 stearate.
[0084] The preparation method is as follows:
[0085] The preparation method of the fast-melting asphalt dry direct-injection modifier is the same as the preparation method in Example 1.
[0086] Example 5
[0087] The present embodiment is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 45 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 40.5 parts of 180-mesh rubber powder; 1 part of a sulfur stabilizer; 0.5 parts of nano-cerium oxide; 4 parts of diisooctyl sebacate; 4 parts of a maleic anhydride grafted polymer; and 5 parts of polyglycerol-6 stearate.
[0088] The preparation method is as follows:
[0089] The butadiene-styrene-butadiene block copolymer is sheared at a high speed of 3000 rpm for 20 minutes, and mixed with rubber powder and diisooctyl sebacate at 180°C. After uniform mixing, polyglycerol-6 stearate is added, and high-temperature plasticization is performed at 120°C for 4 minutes to obtain an intermediate product. Sulfur stabilizer, nano-cerium oxide, maleic anhydride grafted polymer and polyglycerol-6 stearate are added to the intermediate product, and after mixing at 100°C for 3 minutes, a granular product with a particle size of less than 2 mm is prepared by high-temperature melt extrusion granulation with a single screw extruder. Finally, the granular product is ground to obtain a dry direct injection modifier with a particle size of less than 20 microns.
[0090] Example 6
[0091] The present embodiment is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 45 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 40.5 parts of 180-mesh rubber powder; 1 part of a sulfur stabilizer; 0.5 parts of nano-cerium oxide; 4 parts of diisooctyl sebacate; 4 parts of a maleic anhydride grafted polymer; and 5 parts of polyglycerol-6 stearate.
[0092] The preparation method is as follows:
[0093] The butadiene-styrene-butadiene block copolymer is sheared at a high speed of 4000 rpm for 40 minutes, and mixed with rubber powder and diisooctyl sebacate at 180°C. After uniform mixing, polyglycerol-6 stearate is added, and high-temperature plasticization is performed at 150°C for 8 minutes to obtain an intermediate product. Sulfur stabilizer, nano-cerium oxide, maleic anhydride grafted polymer and polyglycerol-6 stearate are added to the intermediate product, and after mixing at 100°C for 3 minutes, a granular product with a particle size of less than 2 mm is prepared by high-temperature melt extrusion granulation with a single screw extruder. Finally, the granular product is ground to obtain a dry direct injection modifier with a particle size of less than 20 microns.
[0094] Example 7
[0095] The present embodiment is a fast-melting asphalt dry direct-injection modifier, which is prepared from the following raw materials in parts by weight: 45 parts of a star-shaped butadiene-styrene-butadiene block copolymer with a molecular weight of 160,000; 40.5 parts of 180-mesh rubber powder; 1 part of a sulfur stabilizer; 0.5 parts of nano-cerium oxide; 4 parts of diisooctyl sebacate; 4 parts of a maleic anhydride grafted polymer; and 5 parts of polyglycerol-6 stearate.
[0096] The preparation method is as follows:
[0097] The butadiene-styrene-butadiene block copolymer is sheared at a high speed of 4000 rpm for 40 minutes, and mixed with rubber powder and diisooctyl sebacate at 180°C. After uniform mixing, polyglycerol-6 stearate is added, and high-temperature plasticization is performed at 120°C for 4 minutes to obtain an intermediate product. Sulfur stabilizer, nano-cerium oxide, maleic anhydride grafted polymer and polyglycerol-6 stearate are added to the intermediate product, and after mixing at 80°C for 2 minutes, a granular product with a particle size of less than 2 mm is prepared by high-temperature melt extrusion granulation with a single screw extruder. Finally, the granular product is ground to obtain a dry direct injection modifier with a particle size of less than 20 microns.
[0098] The performance of the asphalt dry direct injection modifier obtained in Comparative Examples 1 to 7 and Examples 1 to 7 was tested. The difference between Examples 1 to 4 is that the dosage of butadiene-styrene-butadiene block copolymer, rubber powder, stabilizer, plasticizer, polymer grafted or copolymerized with maleic anhydride and surfactant is different. The difference of Example 5 is that a lower shearing speed is used to shear the butadiene-styrene-butadiene block copolymer; the difference of Example 6 is that a higher plasticizing temperature and a longer plasticizing time are used; the difference of Example 7 is that a lower mixing temperature and a shorter mixing time are used.
[0099] Comparative Example 1 is a star-shaped butadiene-styrene-butadiene block copolymer direct-cast modifier without rubber powder; Comparative Example 2 is compared with the direct-cast modifier of the present invention, without adding nano cerium oxide; Comparative Example 3 is compared with the direct-cast modifier of the present invention; in Comparative Example 4, the temperature and time conditions of the plasticizing and mixing steps are different from the protection scope of the present invention; in Comparative Example 5, the particle size of the rubber powder raw material, the type of butadiene-styrene-butadiene block copolymer and the particle size of the microparticles produced by grinding during the production process are not within the protection scope of the present invention; in Comparative Example 6, the shear rate and shear time in the high-speed shearing step of butadiene-styrene-butadiene block copolymer are not within the protection scope of the present invention; in Comparative Example 7, the dosage of the maleic anhydride grafted polymer is not within the protection scope of the present invention.
[0100] Detection methods include:
[0101] (1) The melting index of the fast-melting asphalt dry-casting modifiers of the examples and comparative examples was tested using a melting index tester to evaluate the melting rate of the asphalt dry-casting modifiers. The melting index tester was MFI-2322S, the test temperature was 190°C, and the weight was 2.16 kg. The test results are shown in Table 1.
[0102] (2) The melting and dispersibility of the fast-melting asphalt dry direct-addition modifiers of the examples and comparative examples in mixing and stirring with stone were tested using an indoor asphalt mixture mixing pot. The direct-addition temperature was 180°C, the stone particle size was 4.75-9.5 mm, and the mixing time was 1 min. The test results are shown in Table 1.
[0103] (3) According to the standards of the test procedures for asphalt and asphalt mixtures for highway engineering, such as solubility, Brookfield rotation viscosity, penetration, softening point, ductility, and modified asphalt segregation test, the asphalt modified by the fast-melting asphalt dry-cast modifier of the embodiment and the comparative example was tested. The dosage of the fast-melting asphalt dry-cast modifier was 5% of the base asphalt. The test results are shown in Table 2.
[0104] (4) The road performance of the asphalt mixture modified by the fast-melting asphalt dry-cast modifier of the embodiment and the comparative example was tested. The corresponding tests were carried out according to the relevant test specifications of the "Technical Guide for Highway Dry SBS Modified Asphalt Pavement" T / CHTS20003-2018 and the "Test Procedure for Highway Engineering Asphalt and Asphalt Mixture" JTGE20-2011. The commonly used SMA-13 asphalt mixture was used, with an oil-stone ratio of 5.0%, and the dosage of the fast-melting asphalt dry-cast modifier was 5% of the base asphalt. The road performance was compared with that of the wet-modified asphalt SMA-13, with the wet-modified oil-stone ratio of 5.0%. The test results are shown in Table 3.
[0105] Table 1 Comparison of melt index and dispersion performance test results of Examples 1 to 7 and Comparative Examples 1 to 7
[0106]
[0107]
[0108] Table 2 Comparison of performance test results of fast-melting asphalt dry direct-cast modified asphalt of Examples 1 to 7 and Comparative Examples 1 to 7
[0109]
[0110]
[0111] Table 3 Comparison of performance test results of fast-melting asphalt dry direct-cast modified asphalt mixtures of Examples 1 to 7 and Comparative Examples 1 to 7
[0112]
[0113]
[0114] As can be seen from Table 1, the fast-melting asphalt dry-casting modifier obtained in the present invention has a significantly faster melting rate than the ordinary dry-casting SBS modifier and rubber powder modifier, and has excellent dispersibility after dry mixing with stone, and can reach a completely molten state. Comparing the experimental data of the examples and comparative examples, it can be seen that the formula and ratio of the fast-melting asphalt dry-casting modifier in the comparative example are not within the protection scope of the present invention, and show a lower melting rate and poorer stone dry mixing dispersibility than the examples.
[0115] The data in Table 2 show that the asphalt modified by the fast-melting asphalt dry-casting modifier of the present invention has a viscosity 2 to 3 times higher than that of the asphalt modified by the common dry-casting SBS modifier and rubber powder modifier, a lower penetration, a higher softening point and ductility. At the same time, it also has significantly better storage stability. This shows that the fast-melting asphalt dry-casting modifier of the present invention can significantly improve the viscosity, modulus, tensile strength, heat resistance and storage stability of asphalt.
[0116] The data in Table 3 show that the asphalt mixture modified by the fast-melting asphalt dry-cast modifier of the present invention has a significantly improved freeze-thaw splitting ratio, a substantially doubled Marshall stability, a 40% to 53% reduction in scattering loss, a 12% to 25% increase in pavement water permeability coefficient, and a nearly doubled improvement in 60°C stability index compared to the asphalt mixture modified by the ordinary dry-cast SBS modifier and rubber powder modifier. The road performance of the wet-process star-shaped SBS modified asphalt mixture is also significantly improved. It can be seen that the fast-melting asphalt dry-cast modifier of the present invention can significantly improve the road performance of asphalt pavement under dry application conditions, improve pavement strength, improve crack resistance, bonding performance and rutting resistance, and greatly improve the water permeability of asphalt pavement, and is suitable for large-pore drainage pavement applications.
[0117] In summary, the fast-melting asphalt dry-cast modifier prepared by the technology of the present invention has the advantages of fast melting, excellent dispersibility with stone, short preparation process, low required processing temperature, etc., compared with the ordinary dry-cast SBS modifier, and good construction and workability. It can greatly improve the viscosity, elasticity and other basic asphalt indexes of asphalt while meeting the general road use standards, and significantly improve the drainage, crack resistance, rutting resistance and bonding performance of asphalt mixture, and is very suitable for drainage pavement and thin layer paving applications.
Claims
1. A fast-melting asphalt dry-process direct-injection modifier, characterized in that: The raw materials include the following components in parts by weight:
2. The fast-melting asphalt dry-process direct-injection modifier according to claim 2 is characterized in that: The butadiene-styrene-butadiene block copolymer is a star-shaped SBS with a molecular weight of 150,000 to 200,000.
3. The fast-melting asphalt dry-process direct-injection modifier according to claim 1 is characterized in that: The particle size of the rubber powder is 150-200 meshes.
4. The fast-melting asphalt dry-process direct-injection modifier according to claim 1, characterized in that: The stabilizer is one of a sulfur stabilizer and nano-cerium oxide or a combination of the two in any proportion.
5. The fast-melting asphalt dry-process direct-injection modifier according to claim 1 is characterized in that: The plasticizer is diisooctyl sebacate.
6. The fast-melting asphalt dry direct-injection modifier according to claim 1, characterized in that: The surfactant is polyglyceryl-6 stearate.
7. A method for preparing a fast-melting asphalt dry direct-injection modifier, characterized in that: The following steps are involved: (1) subjecting the butadiene-styrene-butadiene block copolymer to high-speed shearing for standby use; (2) adding rubber powder and diisooctyl sebacate to the butadiene-styrene-butadiene block copolymer obtained in step (1), and mixing them uniformly; (3) heating the mixture, adding a plasticizer, and performing high-temperature plasticizing; (4) adding a stabilizer, a coupling agent and a surfactant to the material obtained in step (3) and mixing them; (5) The product obtained in step (4) is granulated by high-temperature melt extrusion through a single-screw extruder, and the granular product is ground to obtain the asphalt dry direct injection modifier that can be melted quickly.
8. The method for preparing a fast-melting asphalt dry direct-injection modifier according to claim 7, characterized in that: In the step (1), the rotation speed of the high-speed shearing machine is 3000-4000 rpm; and the shearing treatment time is 20-40 minutes.
9. The method for preparing a fast-melting asphalt dry direct-injection modifier according to claim 7, characterized in that: In the step (3), the temperature for mixing and heating the butadiene-styrene-butadiene block copolymer, rubber powder and diisooctyl sebacate is 180-200° C., and then polyglycerol-6 stearate is added. The plasticizing temperature is 120° C.-150° C. and the plasticizing time is 3-8 minutes.
10. The method for preparing a fast-melting asphalt dry direct-injection modifier according to claim 7, characterized in that: In the step (4), the mixing temperature is 80° C.-100° C., and the mixing time is 2-5 minutes.
11. The method for preparing a fast-melting asphalt dry direct-injection modifier according to claim 7, characterized in that: The step (5) is specifically as follows: preparing a granular product with a particle size of less than 2 mm by high-temperature melt extrusion granulation using a single screw extruder, and finally grinding the granular product to obtain a dry direct injection modifier with a particle size of less than 20 microns.
Citation Information
Cited By
Additive for dry-mix modified asphalt and method for preparing the same, and modified asphalt mixture using the additive and method for preparing the same