Silicic acid emulsified asphalt and emulsified asphalt reclaimed material mixture

By introducing silicate emulsified asphalt, glass microbeads and regenerator emulsion into the emulsified asphalt, forming a nano-scale network structure and activating old asphalt, the problem of forming speed and strength of cold regeneration mixture is solved, and rapid molding and meeting technical requirements are achieved high intensity effect.

CN118978811APending Publication Date: 2024-11-19SHANGHAI TUOPU ROAD MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411225389.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing emulsified asphalt cold regeneration mixture has a slow forming speed and a slow forming strength. The overall strength is greatly affected by the old material, making it difficult to meet the technical requirements of cracking strength and freeze-thaw strength within 1 day.

Method used

Silicic acid emulsified asphalt and glass microbeads are used to modify cold regenerated emulsified asphalt, combined with water-soluble silicate and regenerator emulsion, and by forming a nanoscale silica network structure and activating old asphalt, the forming speed and strength of the mixture are improved.

Benefits of technology

The cold regenerated mixture is rapidly formed within 1 day, meeting the technical requirements of cracking strength and freeze-thaw strength, and improving the penetration rate of new and old asphalt and the overall strength of the mixture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005024342400000031
    Figure BDA0005024342400000031
  • Figure BDA0005024342400000041
    Figure BDA0005024342400000041
  • Figure BDA0005024342400000051
    Figure BDA0005024342400000051
Patent Text Reader

Abstract

The invention discloses a silicic acid emulsified asphalt and emulsified asphalt reclaimed material mixture which comprises the following components in percentage by weight: 5-10% of water-soluble silicate, 80-90% of glass bead modified cold-recycled emulsified asphalt and 5-10% of regenerant emulsion, the water-soluble silicate is an acidic silicate solution or a neutral silicate solution; the glass bead modified cold recycled emulsified asphalt comprises the following raw materials in parts by weight: 50-65 parts of matrix asphalt, 1-4 parts of glass beads, 2.0-4.0 parts of an emulsifier, 35-45 parts of water and 0.2-1 part of inorganic acid, the glass beads are oleophylic glass beads with the particle size of more than or equal to 170 meshes, the silicon dioxide content of the glass beads is more than or equal to 67%, the forming speed of the cold-recycled mixture is increased, the strength after rapid forming is ensured, and even if coring is carried out for one day, the ratio of rupture strength to freeze-thaw strength meets the requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of emulsified asphalt, and specifically relates to a silicate emulsified asphalt and an emulsified asphalt recycled material mixture. Background Art

[0002] Asphalt pavement is widely used in China due to its many advantages. However, due to long-term load, ultraviolet rays and other factors, asphalt pavement will gradually show signs of disease and aging, and the pavement needs to be renovated, resulting in a large number of old mixtures. These old materials can be reused on the pavement using recycling technology. Among them, emulsified asphalt recycling is one of the popular directions. Due to its high proportion of old materials and environmentally friendly construction methods, it has been greatly promoted. However, the current conventional formula for cold regeneration of emulsified asphalt is to use emulsified asphalt produced by slow-cracking and slow-setting emulsifiers, combined with cement and old materials to form a cold recycled mixture through rolling; however, its molding is slow, the penetration of old asphalt is slow, and the later molding strength increases slowly, and the overall strength is greatly affected by the old materials. Summary of the invention

[0003] The purpose of the present invention is to provide a silicate emulsified asphalt and an emulsified asphalt recycled material mixture, which can improve the molding speed of the cold recycled mixture and ensure the strength after rapid molding, so that the bursting strength and freeze-thaw strength ratio can meet the requirements even if the core is taken in one day.

[0004] To achieve the above purpose, the technical solution of the present invention is as follows:

[0005] A silicate emulsified asphalt, comprising, by weight percentage: 5-10% water-soluble silicate, 80-90% glass microsphere modified cold regenerated emulsified asphalt, and 5-10% regeneration agent emulsion;

[0006] The water-soluble silicate is an acidic silicate or a neutral silicate;

[0007] The glass microsphere modified cold regenerated emulsified asphalt comprises the following raw materials in parts by weight: 50-65 parts of base asphalt, 1-4 parts of glass microspheres, 2.0-4.0 parts of emulsifier, 35-45 parts of water, and 0.2-1 part of inorganic acid; the glass microspheres are oleophilic glass microspheres with a particle size of ≥170 mesh, and the silicon dioxide content in the oleophilic glass microspheres is ≥67wt%.

[0008] Furthermore, the specific preparation steps of the regeneration agent emulsion are: adding the emulsifier to 40-60°C water, then adding inorganic acid, adjusting the pH to between 1.8-2.5 to obtain soap solution, and then adding the soap solution and the asphalt regeneration agent to the colloid mill to produce the regeneration agent emulsion.

[0009] Preferably, the emulsifier is a quaternary ammonium salt cationic emulsifier.

[0010] Preferably, the inorganic acid is hydrochloric acid.

[0011] Furthermore, the specific preparation steps of the glass bead modified cold regenerated emulsified asphalt are as follows: heating the base asphalt to 130-150°C, adding glass beads to the base asphalt and stirring and dispersing them to obtain an initial base asphalt, and then feeding the soap solution obtained by dissolving the emulsifier in water and the initial base asphalt into an emulsifier together, breaking the asphalt into tiny particles through mechanical force, and dispersing them in the soap solution to obtain glass bead modified cold regenerated emulsified asphalt.

[0012] A regenerated mixture comprising the above-mentioned silicate emulsified asphalt comprises the following raw materials in parts by weight: 3-6 parts of silicate emulsified asphalt, 60-100 parts of asphalt mixture recycled material, 1-3 parts of mineral powder, 0.5-3 parts of cement, and 1-4 parts of water.

[0013] Preferably, the recycled asphalt mixture includes 10-30 parts of recycled asphalt mixture with a particle size of 0-5 mm, 40-80 parts of recycled asphalt mixture with a particle size of 5-10 mm, and 10-20 parts of recycled asphalt mixture with a particle size of 10-18 mm.

[0014] Preferably, the cement is conventional ordinary Portland cement 425 or 325.

[0015] Preferably, the mineral powder is a mineral powder that complies with the provisions of JTG F40 "Technical Specifications for Highway Asphalt Pavement Construction", preferably limestone mineral powder.

[0016] The recycled mixture includes the following raw materials by weight: 3-6 parts of silicate emulsified asphalt, 60-100 parts of asphalt mixture recycled material, 1-3 parts of mineral powder, 0.5-3 parts of cement, and 1-4 parts of water. Cement in the recycled mixture has a great influence on the strength, but too much cement will cause uneven mixing of the cold recycled mixture, so it cannot be added too much.

[0017] In order to obtain higher strength, the present invention introduces water-soluble silicate (acidic silicon solution or neutral solution). After the water-soluble silicon solution is formed, it has a nano-scale silicon dioxide network structure, which improves the adhesion and strength of the cold recycled mixture.

[0018] In the glass microsphere-modified cold regenerated emulsified asphalt of the present invention, lipophilic glass microspheres are added to the emulsified asphalt. Since the glass microspheres themselves have high strength and low density, they can be effectively dispersed in the emulsified asphalt to enhance the strength of the mixture. At the same time, the oxides contained in the glass microspheres can help the emulsified asphalt to demulsify and accelerate the formation of the mixture.

[0019] Glass beads and water-soluble silicates can effectively help emulsified cold recycling molding. Water-soluble silicates form a network structure after dehydration, which helps the road surface to form strength and quickly form and coring. Even coring in one day can make the fracture strength and freeze-thaw strength ratio meet the requirements. The coring of traditional emulsified cold recycled mixtures takes 7 days.

[0020] The introduction of regeneration agent emulsion can help activate old asphalt. Since old asphalt is relatively hard, it will become soft after introduction, increasing the speed of mutual penetration between new and old asphalt, so that the porosity will become smaller during the final inspection, which can more effectively prevent water seepage in the road surface.

[0021] Beneficial effects of the present invention:

[0022] The present invention improves the molding speed of cold recycled mixture by adding glass microspheres and water-soluble silicates at the same time, and ensures the strength after rapid molding, so that the fracture strength and freeze-thaw strength ratio meet the requirements even if the coring is done in one day, while the traditional cold recycled mixture coring takes 7 days.

[0023] At the same time, if the original technology is formed too quickly, the new and old asphalt will not be well integrated, there may be uneven strength, and the freeze-thaw strength ratio cannot pass. The introduction of glass beads is used as filler reinforcement, and the introduction of regeneration agent activates the old asphalt, so that the old asphalt and the new asphalt can be better integrated to ensure strength. DETAILED DESCRIPTION

[0024] The present invention will be further described below in conjunction with the embodiments.

[0025] The composition of the silicate emulsified asphalt of the present invention is shown in Table 1, the specific components of the glass bead modified cold regenerated emulsified asphalt are shown in Table 2, and the components of the regenerated mixture of the silicate emulsified asphalt are shown in Table 3.

[0026] Table 1 Unit: Weight percentage

[0027]

[0028]

[0029] Table 2 Unit: parts

[0030] Base asphalt Glass beads Emulsifier water Inorganic acid Example 1 50 1 3 35 0.2 Example 2 55 3 2 38 0.6 Example 3 60 4 2.5 45 0.8 Example 4 65 2 4 40 1 Comparative Example 1 60 2 3 1 2 Comparative Example 2 60 2 3 1 2 Comparative Example 3 60 - 3 1 2 Comparative Example 4 60 - 3 1 2

[0031] Table 3 Unit:

[0032] Silicate emulsified asphalt Recycling of old materials Mineral powder cement water Example 1 3.5 91 3 0.5 2 Example 2 4.5 98 2 1 3 Example 3 6.0 80 1 2 2 Example 4 5.0 60 3 3 4 Comparative Example 1 4.5 90 3 1 2 Comparative Example 2 4.5 90 3 1 2 Comparative Example 3 4.5 90 3 1 2 Comparative Example 4 4.5 90 3 1 2

[0033] The performance indicators of the embodiments of the present invention and the comparative examples are shown in Table 4.

[0034] Table 4

[0035]

[0036] The cold regeneration coring experiment is a method to determine the molding of the mixture. If the mixture has been molded and has strength, the core sample can be completely taken out. The general construction coring time is 7-14 days. From the results in Table 4, it can be seen that the embodiments of the present invention can all be cored within 1 day, proving that the molding speed of the mixture is extremely fast. The porosity, splitting strength, and freeze-thaw splitting strength ratio of the embodiments of the present invention all meet the technical index requirements of JTG / T5521-2019 for emulsified asphalt cold recycled mixtures, among which the splitting strength reaches the requirements of heavy load and above traffic load level surface layer ≥0.6, and the freeze-thaw splitting strength reaches the requirements of heavy load and above traffic load level ≥80%.

[0037] In Comparative Example 1, no regeneration agent emulsion is added, and the old asphalt cannot be quickly activated and combined with the new asphalt. The overall asphalt mixture is too hard, resulting in the freeze-thaw splitting strength failing to meet the minimum technical requirements.

[0038] In Comparative Example 2, no aqueous silicate was added, and the coring time was 3 days. At the same time, the splitting strength could not meet the requirements of the heavy-load traffic surface layer, and could only meet the technical requirements of the heavy-load traffic base layer and the layers below ≥0.5.

[0039] In Comparative Example 3, cold recycled emulsified asphalt modified with glass beads is not used, and the coring time is 4d. At the same time, the splitting strength cannot meet the requirements of the heavy-load traffic surface layer, and can only meet the technical requirements of the heavy-load traffic base layer and the layers below ≥0.5.

[0040] In Comparative Example 4, the emulsified asphalt modified with no water-based silicate and glass beads, i.e., normal emulsified asphalt cold recycled mixture, has a coring time of 7 days and a splitting strength that cannot meet the requirements of the heavy-load traffic surface layer and can only meet the technical requirements of the heavy-load traffic base layer and the layers below ≥0.5.

Claims

1. A silicate emulsified asphalt, characterized in that: The composition comprises, by weight percentage: 5-10% water-soluble silicate, 80-90% glass microsphere modified cold regenerated emulsified asphalt, and 5-10% regeneration agent emulsion; The water-soluble silicate is an acidic silicate or a neutral silicate; The glass microsphere modified cold regenerated emulsified asphalt comprises the following raw materials in parts by weight: 50-65 parts of base asphalt, 1-4 parts of glass microspheres, 2.0-4.0 parts of emulsifier, 35-45 parts of water, and 0.2-1 part of inorganic acid; the glass microspheres are oleophilic glass microspheres with a particle size of ≥170 mesh, and the silicon dioxide content in the oleophilic glass microspheres is ≥67wt%.

2. The silicate emulsified asphalt according to claim 1, characterized in that The specific preparation steps of the regeneration agent emulsion are: adding an emulsifier to 40-60°C water, then adding an inorganic acid, adjusting the pH to between 1.8-2.5 to obtain a soap solution, and then adding the soap solution and the asphalt regeneration agent to a colloid mill to produce the regeneration agent emulsion.

3. The silicate emulsified asphalt according to claim 1 or 2, characterized in that: The emulsifier is a quaternary ammonium salt cationic emulsifier.

4. The silicate emulsified asphalt according to claim 1 or 2, characterized in that: The inorganic acid is hydrochloric acid.

5. The silicate emulsified asphalt according to claim 1, characterized in that The specific preparation steps of the glass bead modified cold regenerated emulsified asphalt are as follows: heating the base asphalt to 130-150° C., adding glass beads to the base asphalt and stirring and dispersing it to obtain an initial base asphalt, and then feeding the soap solution obtained by dissolving the emulsifier in water and the initial base asphalt into an emulsifier together, breaking the asphalt into tiny particles through mechanical force, and dispersing them in the soap solution to obtain glass bead modified cold regenerated emulsified asphalt.

6. A recycled mixture comprising the silicate emulsified asphalt according to any one of claims 1 to 5, characterized in that: The method comprises the following raw materials in parts by weight: 3-6 parts of silicate emulsified asphalt, 60-100 parts of asphalt mixture recycled material, 1-3 parts of mineral powder, 0.5-3 parts of cement and 1-4 parts of water.

7. The recycled mixed material according to claim 6, characterized in that: The asphalt mixture recycled material includes 10-30 parts of asphalt mixture recycled material with a particle size of 0-5 mm, 40-80 parts of asphalt mixture recycled material with a particle size of 5-10 mm, and 10-20 parts of asphalt mixture recycled material with a particle size of 10-18 mm.

8. The recycled mixed material according to claim 6, characterized in that: The cement is conventional ordinary Portland cement 425 or 325.

9. The recycled mixed material according to claim 6, characterized in that: The mineral powder is a mineral powder that complies with the provisions of JTG F40 "Technical Specifications for Highway Asphalt Pavement Construction", and is preferably limestone mineral powder.