Preparation method and construction method of stone-like coating
By adding cellulose and silicone acrylic emulsion to imitation stone paint and adding granulation glue solution to the color point for shearing treatment, the problem of insufficient adhesion strength of existing imitation stone paint is solved, and the construction steps and shortening are achieved. Effect of construction time.
Patent Information
- Application Number
- CN202411046280.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing imitation stone paint lacks adhesion, which leads to the need to scrape the putty twice during the construction process, extending the construction cycle.
By adding cellulose and silicon acrylic emulsion to the texture, spraying the texture through flat spray and spraying floating point, increasing the adhesion force; adding granulation glue solution to the color point and shear it. The surface of the color point particles is wrapped with granulation glue, and the screen is divided and cut through the screen to improve the adhesion force; the stirring device is used to achieve the integration of stirring, shearing and sieving.
It realizes that the bonding strength of the texture coating can be satisfied by just scraping the putty once, shortening the construction time and improving construction efficiency.
Smart Images

Figure CN118978839A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of exterior wall coatings, in particular to a stone-like coating and a construction method thereof. Background Art
[0002] Imitation stone paint is a decorative architectural paint that imitates the texture and appearance of natural stone through special production formula, process and coating method, so as to replace or reduce the use of natural stone. Imitation stone paint has the characteristics of rich colors, realistic texture, wear resistance, weather resistance, easy maintenance, etc. Its main properties include mechanical properties, physical properties, durability, appearance properties, production and construction properties, etc. It is widely used in construction, decoration, gardening and other fields.
[0003] The existing imitation stone paint coating process requires two coats of putty after basic treatment. The reason is that the first coat of putty is for repairing and leveling and strengthening the tightness of the wall. Since the existing imitation stone paint has insufficient adhesion, the second coat of putty is required for delicate leveling to make the imitation stone paint more stable. The interval between the two coats of putty cannot be too short. The second coat of putty must be applied after the first coat of putty is dry, which prolongs the construction period. Summary of the invention
[0004] The purpose of the invention is to provide a stone-like paint, which has the effect of improving the adhesion of the paint.
[0005] The above technical objectives of the present invention are achieved through the following technical solutions: a stone-like paint, including a textured mid-coat and a litchi stone color dot paint, characterized in that: the textured mid-coat includes, by weight, 10-15 parts of water, 0.2-0.5 parts of cellulose, 60-70 parts of fillers, 15-18 parts of silicone acrylic emulsion, and 3-14 parts of a mid-coat additive;
[0006] The litchi stone color point paint comprises 625-635 color points, 195-205 parts of granulation rubber solution and 165-175 parts of continuous phase solution by mass; the color points are composed of color paste and basic paint, and the color paste accounts for 0.1%-3% of the mass fraction of the color points.
[0007] The base paint comprises, by mass, 35-40 parts of water, 0.8-1 parts of cellulose, 40-50 parts of filler, 15-18 parts of silicone-acrylic emulsion, 0.6-0.9 parts of hollow microspheres, and 4-5 parts of pregel;
[0008] The continuous phase solution comprises 330-340 parts of water, 590-610 parts of silicone-acrylic emulsion and 62-68 parts of continuous phase auxiliary agent by mass.
[0009] By adopting the above technical scheme, cellulose and silicone acrylic emulsion are added to the textured mid-coat to improve the adhesion between the textured mid-coat and putty. At the same time, the textured mid-coat is sprayed by atomized flat spraying and floating point spraying, which further improves the adhesion with the putty.
[0010] The present invention is further configured as follows: the continuous phase additive includes, by mass, 5.3-5.7 parts of thickener, 24-26 parts of ethylene glycol, 6.8-7.2 parts of preservative, 23-25 parts of film-forming additive, 0.8-1.2 parts of defoamer, 1.3-1.7 parts of anti-settling agent and 0.6-0.8 parts of multifunctional additive.
[0011] The present invention is further configured as follows: the middle coating additive includes, by mass, 0.8-1.2 parts of a defoamer, 0.8-1.2 parts of a dispersant, 2.8-3.2 parts of a bactericide, 0.5-0.9 parts of a multifunctional additive, and 3.3-3.7 parts of a film-forming additive.
[0012] The present invention is further configured as follows: the preparation method of the litchi stone color dot paint comprises the following steps:
[0013] S1 color point preparation: mix the color paste and the base paint in proportion;
[0014] S2 color point cutting: add granulation rubber solution into the color point according to the components and shear;
[0015] S3 color point screening: the sheared color points are screened and cut through the sieve;
[0016] S4 color point mixing: Mix the sieved color points with the continuous phase solution in proportion.
[0017] By adopting the above technical solution, a granulating rubber solution is added to the color dots and sheared, so that the granulating rubber solution is wrapped on the surface of the sheared color dot particles, and the sheared color dot particles are sieved and cut through a sieve, so that the diameter of the sieved color dot particles meets the requirements.
[0018] The present invention is further configured as follows: the stirring speed of the mixing and stirring in step S1 is 600 rpm, and the duration is 2-3 min; the stirring speed of the mixing and stirring in step S4 is 100 rpm, and the duration is 2-3 min.
[0019] The present invention is further configured as follows: the granulated rubber solution includes water and rubber powder, and the rubber powder in the granulated rubber solution accounts for 4% of the total mass of the granulated rubber solution; the pregel includes water and rubber powder, and the rubber powder in the pregel accounts for 10% of the total mass of the pregel.
[0020] The present invention is further configured as follows: the emulsion is an acrylic resin emulsion, and the filler is quartz sand with a mesh size of 120-180.
[0021] The present invention also provides a construction method of stone-like paint, which is characterized by comprising the following steps:
[0022] Step 1: Scrape the anti-cracking mortar on the wall and lay the fiber mesh;
[0023] Step 2: Scrape and level the rough putty on the fiber mesh;
[0024] Step 3: Polishing, flushing and maintenance;
[0025] Step 4: Spray or roll the exterior wall alkali-resistant primer;
[0026] Step 5: Draw lines, divide grids, and paste color separation paper;
[0027] Step 6: Atomized flat spray texture mid-coat;
[0028] Step 7: Spray floating texture mid-coat;
[0029] Step 8: Sand the textured midcoat with 100-grit sandpaper;
[0030] Step 9: Spray the litchi rock color paint all over;
[0031] Step 10: Spray or roll on the topcoat:.
[0032] The present invention is further configured as follows: it also includes a stirring device for implementing stirring and shearing, the stirring device includes a stirring barrel and a bracket fixedly connected above the stirring barrel, the bracket is fixedly connected to a driving motor, the bracket is fixedly connected to an internal gear, the end of the rotating shaft of the driving motor is fixedly connected to a driving rotating shaft, the driving rotating shaft is connected to a driving gear located inside the internal gear, a transmission shaft located between the internal gear and the driving gear is slidably connected to the bracket, the transmission shaft is connected to a transmission gear, the internal gear and the driving gear are respectively meshed with the transmission gear, a stirring blade is fixedly connected to the end of the transmission shaft, a shearing blade is fixedly connected to the end of the driving rotating shaft, a discharge outlet is provided at the bottom of the stirring barrel, the axis of the driving rotating shaft passes through the discharge outlet, and a filter screen is connected to the discharge outlet.
[0033] The present invention is further configured as follows: a pushing auger is fixedly connected to the driving shaft, a reflux pipe is connected to the discharge port, the end of the reflux pipe extends out of the upper port of the mixing barrel, a reflux pump and a control valve are connected to the reflux pipe, a one-way bearing located between the driving shaft and the driving gear is sleeved on the driving shaft, when the driving shaft rotates synchronously with the driving gear through the one-way bearing, the conveying direction of the pushing auger is upward along the driving shaft, and when the driving shaft rotates relative to the driving gear through the one-way bearing, the conveying direction of the pushing auger is upward along the driving shaft.
[0034] By adopting the above technical solution, when the stirring device is used to mix the litchi stone color point paint, the color paste and the base paint are introduced into the stirring barrel, the driving motor drives the driving shaft to rotate forward, the driving shaft rotates synchronously with the driving gear through the one-way bearing, the transmission gear is meshed with the internal gear and the driving gear respectively, and the transmission gear drives the stirring blade to rotate on the bracket and revolve around the driving shaft as a planetary gear, so as to complete the mixing and stirring of the color paste and the base paint, and at the same time, the auger is driven to drive the mixed fluid to flow upward, thereby improving the stirring effect; the control valve is connected to the discharge port, after the stirring is completed, the driving motor drives the driving shaft to rotate in the opposite direction, the driving gear and the driving shaft rotate relative to each other through the one-way bearing, the driving gear is stationary, the control valve and the reflux pump are opened, the auger is driven to push the fluid downward to contact with the rotating shear blade for shearing and discharge from the discharge port and pass through the filter screen, the reflux pump re-pumps the sieved color points into the stirring barrel, after a period of time, the reflux pump and the control valve are closed, the continuous phase solution is added to the stirring barrel, and the driving motor drives the driving device to rotate forward, thereby driving the color points and the continuous phase solution to stir and mix.
[0035] The beneficial effects of the present invention are:
[0036] 1. Adding cellulose and silicone acrylic emulsion to the textured mid-coat improves the bonding strength between the textured mid-coat and putty. At the same time, spraying the textured mid-coat by atomized flat spraying and floating spraying further improves the bonding strength with putty, so that only one scraping of putty is needed to meet the bonding strength of the textured mid-coat, shortening the construction time and improving the construction efficiency;
[0037] 2. Add granulation glue solution to the color point and shear it, so that the granulation glue solution is wrapped on the surface of the sheared color point particles, and the sheared color point particles are screened and cut through the screen to make the color point particles more uniform.
[0038] 3. The stirring device is used to realize the integration of stirring, mixing, shearing and screening functions of litchi stone color dot paint in the same device. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0040] Figure 1 Schematic diagram of the structure of the stirring device of this embodiment.
[0041] In the figure, 1. mixing barrel; 11. discharge port; 12. filter screen; 2. bracket; 21. guide ring; 3. internal gear; 4. drive motor; 41. drive shaft; 42. drive gear; 43. shear blade; 44. push auger; 5. transmission shaft; 51. limit convex part; 52. transmission gear; 53. mixing blade; 6. one-way bearing; 7. control valve; 8. reflux pump; 9. reflux pipe. DETAILED DESCRIPTION
[0042] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0043] Embodiment 1 A stone-like paint, comprising a textured mid-coat and a litchi stone color dot paint;
[0044] The texture includes 10 parts of water, 0.2 parts of hydroxyethyl cellulose, 60 parts of texture filler, 15 parts of silicone acrylic emulsion, and 3 parts of mid-coat additive by mass;
[0045] The texture filler includes, by mass, 3.4 parts of bentonite, 1.9 parts of titanium dioxide, 120 parts of 40-80 mesh quartz sand, 340 parts of 80-120 mesh quartz sand, and 240 parts of 120-180 mesh quartz sand;
[0046] The middle coating additives include 0.8 parts of defoamer, 0.8 parts of dispersant, 2.8 parts of fungicide, 0.5 parts of multifunctional additive, and 3.3 parts of film-forming additive by mass;
[0047] The litchi stone color point paint includes 625 parts of color points, 195 parts of granulation rubber solution, and 165 parts of continuous phase solution by mass;
[0048] The granulating rubber solution includes water and rubber powder, and the rubber powder in the granulating rubber solution accounts for 4% of the total mass of the granulating rubber solution;
[0049] The color point includes color paste and base paint, and the color paste accounts for 0.1% of the color point mass fraction;
[0050] The base paint includes, by mass, 35 parts of water, 0.8 parts of hydroxyethyl cellulose, 40 parts of base paint filler, 15 parts of silicone acrylic emulsion, 0.6 parts of hollow microspheres, 4 parts of pregel, and 1.4 parts of base paint additives;
[0051] The pregel comprises water and rubber powder, wherein the rubber powder in the pregel accounts for 10% of the total mass of the pregel;
[0052] The base paint filler includes 73 parts of 80-180 mesh quartz sand, 8 parts of kaolin and 4 parts of titanium dioxide by mass;
[0053] The base paint additives include, by mass, 1.8 parts of defoamer, 0.8 parts of dispersant, 4.3 parts of preservative, 1.8 parts of ethylene glycol, 1.3 parts of multifunctional additive, and 2.8 parts of film-forming additive;
[0054] The continuous phase solution includes 330 parts of water, 590 parts of silicone-acrylic emulsion and 62 parts of continuous phase additive by mass;
[0055] The continuous phase additives include, by mass, 5.3 parts of thickener, 24 parts of ethylene glycol, 6.8 parts of preservative, 23 parts of film-forming additive, 0.8 parts of defoamer, 1.3 parts of anti-settling agent and 0.6 parts of multifunctional additive;
[0056] Embodiment 2 A stone-like paint, comprising a textured mid-coat and a litchi stone color dot paint;
[0057] The texture includes 15 parts of water, 0.5 parts of hydroxyethyl cellulose, 70 parts of texture filler, 18 parts of silicone acrylic emulsion, and 14 parts of mid-coat additive by mass;
[0058] The texture filler includes, by mass, 3.6 parts of bentonite, 2.1 parts of titanium dioxide, 130 parts of 40-80 mesh quartz sand, 360 parts of 80-120 mesh quartz sand, and 260 parts of 120-180 mesh quartz sand;
[0059] The middle coating additives include 1.2 parts of defoamer, 1.2 parts of dispersant, 3.2 parts of fungicide, 0.9 parts of multifunctional additive, and 3.7 parts of film-forming additive by mass;
[0060] The litchi stone color point paint includes 635 parts of color points, 205 parts of granulation rubber solution, and 175 parts of continuous phase solution by mass;
[0061] The granulating rubber solution includes water and rubber powder, and the rubber powder in the granulating rubber solution accounts for 4% of the total mass of the granulating rubber solution;
[0062] The color point includes color paste and base paint, and the color paste accounts for 3% of the color point mass fraction;
[0063] The base paint includes, by mass, 40 parts of water, 1 part of hydroxyethyl cellulose, 50 parts of base paint filler, 18 parts of silicone acrylic emulsion, 0.9 parts of hollow microspheres, 5 parts of pregel, and 4.6 parts of base paint additives;
[0064] The pregel comprises water and rubber powder, wherein the rubber powder in the pregel accounts for 10% of the total mass of the pregel;
[0065] The base paint filler includes 77 parts of 80-180 mesh quartz sand, 12 parts of kaolin and 6 parts of titanium dioxide by mass;
[0066] The base paint additives include, by mass, 2.2 parts of defoamer, 1.2 parts of dispersant, 4.7 parts of preservative, 2.2 parts of ethylene glycol, 1.7 parts of multifunctional additive, and 3.2 parts of film-forming additive;
[0067] The continuous phase solution includes 340 parts of water, 610 parts of silicone-acrylic emulsion and 68 parts of continuous phase additive by mass;
[0068] The continuous phase additives include, by mass, 5.7 parts of thickener, 26 parts of ethylene glycol, 7.2 parts of preservative, 25 parts of film-forming additive, 1.2 parts of defoamer, 1.7 parts of anti-settling agent and 0.8 parts of multifunctional additive;
[0069] Embodiment 3 A stone-like paint, comprising a textured mid-coat and a litchi stone color dot paint;
[0070] The texture includes 13 parts of water, 0.35 parts of hydroxyethyl cellulose, 65 parts of texture filler, 16.7 parts of silicone acrylic emulsion, and 7.5 parts of mid-coat additive by mass;
[0071] The texture filler includes, by mass, 3.5 parts of bentonite, 2 parts of titanium dioxide, 125 parts of 40-80 mesh quartz sand, 350 parts of 80-120 mesh quartz sand, and 250 parts of 120-180 mesh quartz sand;
[0072] The middle coating additives include 1 part of defoamer, 1 part of dispersant, 3 parts of fungicide, 0.7 parts of multifunctional additive, and 3.5 parts of film-forming additive by mass;
[0073] The litchi stone color point paint includes 630 parts of color points, 200 parts of granulation rubber solution, and 170 parts of continuous phase solution by mass;
[0074] The granulating rubber solution includes water and rubber powder, and the rubber powder in the granulating rubber solution accounts for 4% of the total mass of the granulating rubber solution;
[0075] The color point includes color paste and base paint, and the color paste accounts for 1.5% of the color point mass fraction;
[0076] The base paint includes, by mass, 37 parts of water, 0.9 parts of hydroxyethyl cellulose, 45 parts of base paint filler, 16.5 parts of silicone acrylic emulsion, 0.7 parts of hollow microspheres, 4.5 parts of pregel, and 3 parts of base paint additives;
[0077] The pregel comprises water and rubber powder, wherein the rubber powder in the pregel accounts for 10% of the total mass of the pregel;
[0078] The base paint filler includes 75 parts of 80-180 mesh quartz sand, 10 parts of kaolin and 5 parts of titanium dioxide by mass;
[0079] The base paint additives include, by mass, 2 parts of defoamer, 1 part of dispersant, 4.5 parts of preservative, 2 parts of ethylene glycol, 1.5 parts of multifunctional additive, and 3 parts of film-forming additive;
[0080] The continuous phase solution includes 335 parts of water, 600 parts of silicone-acrylic emulsion and 65 parts of continuous phase additive by mass;
[0081] The continuous phase additives include, by mass, 5.5 parts of thickener, 25 parts of ethylene glycol, 7 parts of preservative, 24 parts of film-forming additive, 1 part of defoamer, 1.5 parts of anti-settling agent and 0.7 parts of multifunctional additive;
[0082] The preparation method of the textured mid-coat in Examples 1-3 comprises the following steps:
[0083] Step 1: Mix water, cellulose and bentonite at a stirring speed of 400-450rpm for 5-6min;
[0084] Step 2: Add defoamer, dispersant, titanium dioxide and multifunctional additives and mix and stir at a speed of 500-550rpm for 5-8min;
[0085] Step 3: Add silicone acrylic emulsion, film-forming aid, fungicide and thickener and mix at a stirring speed of 500-550rpm for 5-6min;
[0086] Step 4: Add quartz sand and mix with stirring at a speed of 600-650 rpm for 5-6 min. The preparation method of litchi stone color dot paint in Example 1-3 comprises the following steps:
[0087] S1 color point preparation: Mix the color paste and the base paint in proportion, stirring at a speed of 600 rpm for 2-3 minutes;
[0088] S2 color point cutting: add granulation rubber solution into the color point according to the components and shear;
[0089] S3 color point screening: the sheared color points are screened and cut through the sieve;
[0090] S4 color point mixing: Mix the sieved color points with the continuous phase solution in proportion, with a stirring speed of 100 rpm and a duration of 2-3 minutes.
[0091] The construction application performance and key performance index parameters of conventional imitation stone coatings in the imitation stone coating market are compared in each embodiment.
[0092] Detection method:
[0093] Performance parameters: Use the special primer for imitation stone paint in each embodiment and the conventional primer on the market to match the scraping type texture paint construction, test the key performance indicators such as primer adhesion and matching texture scraping construction, consumption, sand drop rate, surface effect and bonding strength (bonding strength is tested with reference to the relevant requirements in JG / T24-2018 standard)
[0094]
[0095] The construction method of the imitation stone coating, as shown in the figure, includes the following steps:
[0096] Step 1: Scrape the anti-cracking mortar on the wall and lay the fiber mesh;
[0097] Step 2: Scrape and level the rough putty on the fiber mesh;
[0098] Step 3: Polishing, flushing and maintenance;
[0099] Step 4: Spray or roll the exterior wall alkali-resistant primer;
[0100] Step 5: Draw lines, divide grids, and paste color separation paper;
[0101] Step 6: Atomized flat spray texture mid-coat;
[0102] Step 7: Spray floating texture mid-coat;
[0103] Step 8: Sand the textured midcoat with 100-grit sandpaper;
[0104] Step 9: Spray the litchi rock color paint all over;
[0105] Step 10: Spray or roll on the topcoat.
[0106] A stirring device for implementing stirring and shearing, as shown in the figure, comprises a stirring barrel 1 and a bracket 2 fixedly connected above the stirring barrel 1, a driving motor 4 is fixedly connected to the bracket 2, an internal gear 3 is fixedly connected to the bracket 2, a driving shaft end of the driving motor 4 is fixedly connected to a driving shaft 41, a driving shaft 41 is connected to a driving gear 42 located inside the internal gear 3, a transmission shaft 5 located between the internal gear 3 and the driving gear 42 is slidably connected to the bracket 2, a guide ring 21 is provided on the bracket 2, an end of the transmission shaft 5 extends into the guide ring 21, a section of the transmission shaft 5 extending into the guide ring 21 is fixedly connected to a limited position convex portion 51, a transmission gear 52 is connected to the transmission shaft 5, the internal gear 3 and the driving gear 42 are respectively meshed with the transmission gear 52, a stirring blade 53 is fixedly connected to the end of the transmission shaft 5, a shearing blade 43 is fixedly connected to the end of the driving shaft 41, a discharge port 11 is provided at the bottom of the stirring barrel 1, the axis of the driving shaft 41 passes through the discharge port 11, and a filter screen 12 is connected to the discharge port 11. A pushing auger 44 is fixedly connected to the driving shaft 41, and a reflux pipe 9 is connected to the discharge port 11. The end of the reflux pipe 9 extends out of the upper port of the mixing barrel 1. The reflux pipe 9 is connected to a reflux pump 8 and a control valve 7. A one-way bearing 6 is sleeved on the driving shaft 41 and is located between the driving shaft 41 and the driving gear 42. When the driving shaft 41 rotates synchronously with the driving gear 42 through the one-way bearing 6, the conveying direction of the pushing auger 44 is upward along the driving shaft 41. When the driving shaft 41 rotates relative to the driving gear 42 through the one-way bearing 6, the conveying direction of the pushing auger 44 is upward along the driving shaft 41.
[0107] When the stirring device is used, the color paste and the base paint are introduced into the stirring barrel 1, the driving motor 4 drives the driving shaft 41 to rotate in the positive direction, the driving shaft 41 rotates synchronously with the driving gear 42 through the one-way bearing 6, the transmission gear 52 is respectively meshed with the internal gear 3 and the driving gear 42, and the transmission gear 52 drives the stirring blade 53 on the bracket 2 to rotate in the horizontal plane and revolve around the driving shaft 41 to complete the mixing and stirring of the color paste and the base paint, and at the same time, the auger 44 is driven to drive the mixed fluid to flow upward, thereby improving the stirring effect; the control valve 7 is connected to the discharge port 11, and after the stirring is completed, the driving The motor 4 drives the driving shaft 41 to rotate in the opposite direction, and drives the gear 42 to rotate relative to the driving shaft 41 through the one-way bearing 6. The driving gear 42 is stationary, and the control valve 7 and the reflux pump 8 are opened to push the auger 44 to push the fluid to move downward and contact with the rotating shear blade 43 for shearing and discharge from the discharge port 11 and pass through the filter screen 12. The reflux pump 8 pumps the sieved color points back into the mixing barrel 1. After a period of time, the reflux pump 8 and the control valve 7 are closed, and the continuous phase solution is added into the mixing barrel 1. The driving motor 4 drives the driving device to rotate forward, thereby driving the color points and the continuous phase solution to be stirred and mixed.
Claims
1. A stone-like paint, comprising a textured mid-coat and a litchi stone color dot paint, characterized in that: The textured mid-coat comprises, by weight, 10-15 parts of water, 0.2-0.5 parts of cellulose, 60-70 parts of texture filler, 15-18 parts of silicone-acrylic emulsion, and 3-14 parts of mid-coat additive; the texture filler comprises, by weight, 3.4-3.6 parts of bentonite, 1.9-2.1 parts of titanium dioxide, and 700-750 parts of quartz sand of 40-180 meshes; The litchi stone color point paint comprises 625-635 color points, 195-205 parts of granulation rubber solution and 165-175 parts of continuous phase solution by mass; the color point is composed of color paste and base paint, and the color paste accounts for 0.1%-3% of the mass fraction of the color point; The base paint comprises, by mass, 35-40 parts of water, 0.8-1 parts of cellulose, 40-50 parts of base paint filler, 15-18 parts of silicone-acrylic emulsion, 0.6-0.9 parts of hollow microspheres, 4-5 parts of pregel, and 1.4-4.6 parts of base paint additives; the base paint filler comprises, by mass, 73-77 parts of 80-180 mesh quartz sand, 8-12 parts of kaolin, and 4-6 parts of titanium dioxide; The continuous phase solution comprises 330-340 parts of water, 590-610 parts of silicone acrylic emulsion and 62-68 parts of continuous phase auxiliary agent by mass.
2. The stone-like paint according to claim 1, characterized in that: The continuous phase auxiliary agent comprises, by weight, 5.3-5.7 parts of thickener, 24-26 parts of ethylene glycol, 6.8-7.2 parts of preservative, 23-25 parts of film-forming auxiliary, 0.8-1.2 parts of defoaming agent, 1.3-1.7 parts of anti-settling agent and 0.6-0.8 parts of multifunctional auxiliary.
3. The stone-like paint according to claim 1, characterized in that: The middle coating additive comprises, by mass, 0.8-1.2 parts of a defoamer, 0.8-1.2 parts of a dispersant, 2.8-3.2 parts of a bactericide, 0.5-0.9 parts of a multifunctional additive, and 3.3-3.7 parts of a film-forming additive.
4. The stone-like paint according to claim 1, characterized in that: The base paint additives include, by mass, 1.8-2.2 parts of a defoamer, 0.8-1.2 parts of a dispersant, 4.3-4.7 parts of a preservative, 1.8-2.2 parts of ethylene glycol, 1.3-1.7 parts of a multifunctional additive, and 2.8-3.2 parts of a film-forming additive.
5. A stone-like paint according to any one of claims 1 to 4, characterized in that: The preparation method of the litchi rock color dot paint comprises the following steps: S1 color point preparation: Mix the color paste and the base paint in proportion, stirring at a speed of 600 rpm for 2-3 minutes; S2 color point cutting: add granulation rubber solution into the color point according to the components and shear; S3 color point screening: the sheared color points are screened and cut through the sieve; S4 color point mixing: Mix the sieved color points with the continuous phase solution in proportion and stir at a speed of 100 rpm for 2-3 minutes.
6. The stone-like paint according to claim 1, characterized in that: The granulated rubber solution comprises water and rubber powder, wherein the rubber powder in the granulated rubber solution accounts for 4% of the total mass of the granulated rubber solution; the pregel comprises water and rubber powder, wherein the rubber powder in the pregel accounts for 10% of the total mass of the pregel.
7. A stone-like paint according to any one of claims 1 to 4, characterized in that: The preparation method of the textured mid-coat comprises the following steps: Step 1: Mix water, cellulose and bentonite at a stirring speed of 400-450 rpm for 5-6 minutes; Step 2: Add defoamer, dispersant, titanium dioxide and multifunctional additives and mix and stir at a speed of 500-550rpm for 5-8min; Step 3: Add silicone acrylic emulsion, film-forming aid, fungicide and thickener and mix at a stirring speed of 500-550rpm for 5-6min; Step 4: Add quartz sand and mix at a speed of 600-650rpm for 5-6min.
8. A construction method of a stone-like coating, characterized in that: The following steps are involved: Step 1: Scrape the anti-cracking mortar on the wall and lay the fiber mesh; Step 2: Scrape and level the rough putty on the fiber mesh; Step 3: Polishing, flushing and maintenance; Step 4: Spray or roll the exterior wall alkali-resistant primer; Step 5: Draw lines, divide grids, and paste color separation paper; Step 6: Atomized flat spray texture mid-coat; Step 7: Spray floating texture mid-coat; Step 8: Sand the textured midcoat with 100-grit sandpaper; Step 9: Spray the litchi rock color paint all over; Step 10: Spray or roll on the topcoat.
9. The stone-like paint according to claim 5, characterized in that: The invention also comprises a stirring device for implementing stirring and shearing, the stirring device comprising a stirring barrel (1) and a bracket (2) fixedly connected to the top of the stirring barrel (1), the bracket (2) being fixedly connected to a driving motor (4), the bracket (2) being fixedly connected to an internal gear (3), the rotating shaft end of the driving motor (4) being fixedly connected to a driving shaft (41), the driving shaft (41) being connected to a driving gear (42) located inside the internal gear (3), the bracket (2) being slidably connected to a gear (42) located inside the internal gear (3), and the internal gear (3) being fixedly connected to a driving shaft (41) at the end of the rotating shaft of the driving motor (4). A transmission shaft (5) is provided between the gear (3) and the driving gear (42), the transmission shaft (5) being connected to a transmission gear (52), the internal gear (3) and the driving gear (42) respectively meshing with the transmission gear (52), a stirring blade (53) being fixedly connected to the end of the transmission shaft (5), a shearing blade (43) being fixedly connected to the end of the driving shaft (41), an axis of the driving shaft (41) passing through the discharge port (11), and a filtering screen (12) being connected to the discharge port (11).
10. The stone-like paint according to claim 9, characterized in that: The driving shaft (41) is fixedly connected with a pushing auger (44); the discharge port (11) is connected with a return pipe (9); the end of the return pipe (9) extends out of the upper port of the mixing barrel (1); the return pipe (9) is connected with a return pump (8) and a control valve (7); the driving shaft (41) is sleeved with a one-way bearing (6) located between the driving shaft (41) and the driving gear (42); when the driving shaft (41) rotates synchronously with the driving gear (42) through the one-way bearing (6), the conveying direction of the pushing auger (44) is upward along the driving shaft (41); when the driving shaft (41) rotates relative to the driving gear (42) through the one-way bearing (6), the conveying direction of the pushing auger (44) is upward along the driving shaft (41).
Citation Information
Patent Citations
Construction method for acquiring coating with colorful texture
CN105484455A
Paint producing equipment
CN106474951A
Waterborne sand-in-water colorful paint color point pelletizer and pelletizing method thereof
CN108144552A
Construction method of environment-friendly stone-like coating exterior wall with heat insulation and reflection functions
CN108930374A
Production equipment and production method of real stone paint
CN114887541A