Antistatic water-based polyurea coating and preparation method thereof
By using PVP modified carbon nanotubes and polyvinylpyrrolidone copolymers in polyurea coatings, the compatibility and conductivity problems of carbon nanotubes and polyurea coatings are solved, and efficient anti-static and thermal conductivity are achieved, and the efficiency of the anti-static and thermal conductivity is reduced. Acid wastewater pollution is achieved, improving the mechanical properties and environmental protection of the paint.
Patent Information
- Application Number
- CN202411277811.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-12
AI Technical Summary
In the prior art, carbon nanotubes have poor compatibility with polyurea coatings, resulting in poor conductivity and acidic wastewater pollution problems, affecting environmental protection and production efficiency.
Using PVP modified carbon nanotubes combined with polyvinylpyrrolidone copolymer, the dispersion of carbon nanotubes is improved through grinding and spray drying technology, and three-dimensional chemical crosslinking is formed with terminal isocyanate prepolymers and diamine chain extenders to improve carbon Interface compatibility between nanotubes and polyurea.
It significantly improves the electrical conductivity, thermal conductivity and mechanical properties of polyurea coatings, improves the dispersion and enhancement effect of carbon nanotubes, enhances the tensile properties and tear strength of the coatings, and reduces the generation of acidic wastewater.
Smart Images

Figure CN118978848A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurea, in particular to an antistatic water-based polyurea coating and a preparation method thereof. Background Art
[0002] Polyurea coatings have the advantages of good flexibility, fast curing speed, low curing stability, strong water resistance and waterproof performance. They are widely used in many fields such as construction, furniture and building materials, marine engineering, etc. However, in some special applications, such as electrical equipment, oil storage equipment, precision electronic instruments, aviation equipment, etc., explosions and other hazards may occur due to the accumulation of electric charges. Therefore, how to prepare an antistatic polyurea coating is an important topic.
[0003] Carbon nanotubes are a type of nanomaterial with excellent properties that can improve the electrical conductivity, antistatic properties, mechanical strength and other properties of polymer materials. However, carbon nanotubes themselves have winding characteristics, and their interfaces are not compatible with most polymer materials. Therefore, when carbon nanotubes and polymer materials are mixed, agglomeration and other uneven dispersion phenomena will occur, resulting in the need to add a large amount of carbon nanotubes to achieve conductive or antistatic effects. However, this result will make the coating fluidity worse and there will be more undispersed particles, affecting processability and appearance, and may even cause local charge accumulation, affecting safety.
[0004] Patent application No. 2021100495610 discloses an antistatic polyurea coating for use in the petroleum and petrochemical industries and a method for preparing the same; the carbon nanotubes are acid-washed and then filtered so that the carbon nanotubes can be dispersed in polymer materials such as polyisocyanates, and finally sprayed to obtain an antistatic polyurea coating. The patent improves the interface between the carbon nanotubes and the polymer substrate by treating them with hydrochloric acid and then filtering them, but this preparation process will produce more acidic wastewater, which involves environmental issues and is therefore not suitable for mass production. In summary, the development of antistatic polyurea coatings containing carbon nanotubes has become an important topic, but the following problems are currently encountered in production; 1. The problem of interface modification of carbon nanotubes. It is common to use acid washing to improve the interface between carbon nanotubes and polymer substrates, but this method will produce a large amount of acidic wastewater, which is highly polluting. 2. Carbon nanotube dispersion problem. Carbon nanotubes have a high aspect ratio, so they have high electrical conductivity. However, since carbon nanotubes are entangled with each other during production, it is difficult to distribute them evenly even if the interface is improved. As a result, a large amount of addition is usually required to obtain good electrical conductivity, which is much higher than the theoretical value. Summary of the invention
[0005] The invention solves the problem of poor compatibility between carbon nanotubes and polyurea coatings and the problem of poor electrical conductivity of polyurea coatings.
[0006] The technical solution provided by the present invention is: an antistatic water-based polyurea coating, comprising component A and component B. Component A is 100 parts by weight of terminal isocyanate prepolymer. Component B is 6.8-13.7 parts by weight of diamine chain extender, 42-60 parts by weight of polyvinyl pyrrolidone copolymer, and 1-4 parts by weight of PVP modified carbon nanotubes.
[0007] The preparation method of the polyvinyl pyrrolidone copolymer is as follows: N-vinyl pyrrolidone and a Boc-based polymerization monomer are added to N,N-dimethylformamide, heated to 70-85°C in a nitrogen atmosphere, azobisisobutyronitrile is added, the reaction is performed for 10-18 hours, petroleum ether is added to precipitate after cooling, the precipitate is added to dichloromethane after filtering, trifluoroacetic acid is added, the reaction is stirred for 5-8 hours, reduced pressure distillation is performed, the mixture is washed with a saturated sodium bicarbonate solution, and dried to obtain the polyvinyl pyrrolidone copolymer.
[0008] Preferably, the mass ratio of N-vinyl pyrrolidone, Boc-based polymerization monomer, and azobisisobutyronitrile is (5-7):(3-5):(0.07-0.08).
[0009] Preferably, the preparation method of the Boc-based polymer monomer is: adding sodium hydride to N,N-dimethylformamide under an ice bath, adding 2-bromoethyl acrylate and Boc-cysteine (CAS registration number is 20887-95-0) in a nitrogen atmosphere; the mass ratio of sodium hydride, 2-bromoethyl acrylate, and Boc-cysteine is (0.72-0.84):1:(1.3-1.4), then reacting at 20-30° C. for 18-24 hours, adding hydrochloric acid to the solution to adjust the pH to 2-3, then adding water and dichloromethane, extracting and separating, the organic phase is dried over anhydrous sodium sulfate, filtered and then distilled under reduced pressure, and the product is recrystallized from dichloromethane to obtain a Boc-based polymer monomer.
[0010] Preferably, in component A, the preparation method of the terminal isocyanate prepolymer is: mixing a dry polyether polyol and a diisocyanate compound in a molar ratio of 1:(2.2-2.4), wherein the diisocyanate compound is 2,4-toluene diisocyanate or diphenylmethane-4,4'-diisocyanate; heating to 80-90°C in a nitrogen atmosphere, reacting for 1-2h, to obtain the terminal isocyanate prepolymer.
[0011] Preferably, the diamine chain extender in component B includes 1,4-butylene diamine, meta-phenylenediamine, and diethyltoluenediamine.
[0012] Preferably, the preparation method of PVP-modified carbon nanotubes in component B is as follows: carbon nanotubes and polyvinyl pyrrolidone dispersant in a mass ratio of 1:(0.3-0.5):(16-20) and water are added into the grinding tank of a grinder, and ground with zirconium beads until the length of the carbon nanotubes is less than 10 um, and the grinding liquid is spray-dried to obtain PVP-modified carbon nanotubes.
[0013] Preferably, the preparation method of the antistatic waterborne polyurea coating is as follows: component B: diamine chain extender, polyvinyl pyrrolidone copolymer, PVP modified carbon nanotubes are added to water; after stirring, component A end isocyanate prepolymer is added to obtain the antistatic waterborne polyurea coating.
[0014] The technical effect of the present invention is that: PVP polyvinyl pyrrolidone is used as a dispersant to grind and modify carbon nanotubes to obtain PVP modified carbon nanotubes, thereby effectively improving the dispersibility of carbon nanotubes.
[0015] 2-bromoethyl acrylate and the thiol group of Boc-cysteine are used for substitution reaction to obtain a Boc-based polymerization monomer, which is then copolymerized with N-vinyl pyrrolidone. Finally, the N-Boc protecting group is removed to obtain a polyvinyl pyrrolidone copolymer with hydrophilic carboxyl and amino groups in the side chain.
[0016] The present invention uses a terminal isocyanate prepolymer as the A component of the polyurea coating; a diamine chain extender, a polyvinyl pyrrolidone copolymer, and a PVP-modified carbon nanotube as the B component of the polyurea coating. After the carbon nanotube is modified by the PVP dispersant, the dispersibility in the polyurea water-based coating is better, and a uniform conductive and thermal conductive network can be formed, which significantly improves the electrical conductivity and thermal conductivity of the coating film, and has good antistatic performance and thermal conductivity. At the same time, the mechanical properties of the polyurea are enhanced.
[0017] The polyvinyl pyrrolidone copolymer of the present invention contains hydrophilic carboxyl and amino groups, has good dispersibility in water-based polyurea coating, and has a large number of amino groups in the molecular side chain, which can react with the isocyanate group of the terminal isocyanate prepolymer to form a three-dimensional chemical crosslinking effect, which is beneficial to improving the crosslinking degree of the polyurea and improving the mechanical properties. At the same time, after the copolymer reacts with the terminal isocyanate prepolymer, the generated polyurea contains polyvinyl pyrrolidone segments, which have good interface compatibility with the polyvinyl pyrrolidone on the surface of the modified carbon nanotube, enhance the interface effect between the carbon nanotube and the polyurea, improve the compatibility between the two, make the carbon nanotube have a better reinforcement effect, and enhance the tensile properties and tear strength of the polyurea coating under the synergistic effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is the preparation reaction formula of Boc-based polymerization monomer.
[0019] Figure 2 It is the reaction formula for preparing polyvinyl pyrrolidone copolymer. DETAILED DESCRIPTION
[0020] In order to better understand the technical solution of the present invention, the above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments.
[0021] Example 1
[0022] (1) 0.5 g of carbon nanotubes, 0.2 g of polyvinyl pyrrolidone dispersant, and 8 mL of water were added to the grinding tank of a grinder, and ground with zirconium beads until the length of the carbon nanotubes was less than 10 μm. The grinding liquid was spray-dried to obtain PVP-modified carbon nanotubes.
[0023] (2) Add 2.16 g of sodium hydride to 70 mL of N,N-dimethylformamide under an ice bath, add 3 g of 2-bromoethyl acrylate and 4.1 g of Boc-cysteine under a nitrogen atmosphere, and react at 30° C. for 18 h. Add hydrochloric acid to the solution to adjust the pH to 2, then add water and dichloromethane, extract and separate, dry the organic phase over anhydrous sodium sulfate, filter and distill under reduced pressure, and recrystallize the product with dichloromethane to obtain a Boc-based polymer monomer.
[0024] (3) Add 32 g of N-vinyl pyrrolidone and 18 g of Boc-based polymerization monomer to 300 mL of N,N-dimethylformamide, heat to 70°C in a nitrogen atmosphere, add 0.35 g of azobisisobutyronitrile, react for 18 h, cool, add petroleum ether to precipitate, filter, add the precipitate to dichloromethane, add trifluoroacetic acid, stir and react for 5 h, evaporate under reduced pressure, wash with saturated sodium bicarbonate solution, and dry to obtain a polyvinyl pyrrolidone copolymer.
[0025] (4) 50 mmol of dried polyether polyol N220 and 120 mmol of diphenylmethane-4,4'-diisocyanate were mixed, heated to 90° C. in a nitrogen atmosphere, and reacted for 1 hour to obtain a terminal isocyanate prepolymer.
[0026] (5) Add 6.8 g of diethyltoluenediamine, 42 g of polyvinylpyrrolidone copolymer, and 1 g of PVP-modified carbon nanotubes to 150 mL of water; after stirring, add 100 g of terminal isocyanate prepolymer to obtain an antistatic water-based polyurea coating.
[0027] Example 2
[0028] (1) 0.5 g of carbon nanotubes, 0.25 g of polyvinyl pyrrolidone dispersant, and 10 mL of water were added to the grinding tank of a grinder, and ground with zirconium beads until the length of the carbon nanotubes was less than 10 μm. The grinding liquid was spray-dried to obtain PVP-modified carbon nanotubes.
[0029] (2) Add 2.52 g of sodium hydride to 60 mL of N,N-dimethylformamide under an ice bath, add 3 g of 2-bromoethyl acrylate and 3.9 g of Boc-cysteine under a nitrogen atmosphere, and react at 20° C. for 24 h. Add hydrochloric acid to the solution to adjust the pH to 3, then add water and dichloromethane, extract and separate, dry the organic phase over anhydrous sodium sulfate, filter and distill under reduced pressure, and recrystallize the product with dichloromethane to obtain a Boc-based polymer monomer.
[0030] (3) Add 25 g of N-vinyl pyrrolidone and 25 g of Boc-based polymerization monomer to 300 mL of N,N-dimethylformamide, heat to 80°C in a nitrogen atmosphere, add 0.4 g of azobisisobutyronitrile, react for 18 h, cool, add petroleum ether to precipitate, filter, add the precipitate to dichloromethane, add trifluoroacetic acid, stir and react for 6 h, evaporate under reduced pressure, wash with saturated sodium bicarbonate solution, and dry to obtain a polyvinyl pyrrolidone copolymer.
[0031] (4) 50 mmol of dried polyether polyol N220 and 120 mmol of 2,4-toluene diisocyanate were mixed, heated to 80° C. in a nitrogen atmosphere, and reacted for 2 h to obtain a terminal isocyanate prepolymer.
[0032] (5) Add 11.2 g of m-phenylenediamine, 48 g of polyvinyl pyrrolidone copolymer, and 2 g of PVP-modified carbon nanotubes to 150 mL of water; add 100 g of terminal isocyanate prepolymer after stirring to obtain an antistatic water-based polyurea coating.
[0033] Example 3
[0034] (1) 0.5 g of carbon nanotubes, 0.15 g of polyvinyl pyrrolidone dispersant, and 8 mL of water were added to the grinding tank of a grinder, and ground with zirconium beads until the length of the carbon nanotubes was less than 10 μm. The grinding liquid was spray-dried to obtain PVP-modified carbon nanotubes.
[0035] (2) Add 2.52 g of sodium hydride to 70 mL of N,N-dimethylformamide under an ice bath, add 3 g of 2-bromoethyl acrylate and 4.2 g of Boc-cysteine under a nitrogen atmosphere, and react at 25° C. for 18 h. Add hydrochloric acid to the solution to adjust the pH to 2, then add water and dichloromethane, extract and separate, dry the organic phase over anhydrous sodium sulfate, filter and evaporate under reduced pressure, and recrystallize the product with dichloromethane to obtain a Boc-based polymer monomer.
[0036] (3) Add 35 g of N-vinyl pyrrolidone and 15 g of Boc-based polymerization monomer to 250 mL of N,N-dimethylformamide, heat to 85° C. in a nitrogen atmosphere, add 0.35 g of azobisisobutyronitrile, react for 10 h, cool, add petroleum ether to precipitate, filter, add the precipitate to dichloromethane, add trifluoroacetic acid, stir and react for 5 h, evaporate under reduced pressure, wash with saturated sodium bicarbonate solution, and dry to obtain a polyvinyl pyrrolidone copolymer.
[0037] (4) 50 mmol of dried polyether polyol N220 and 110 mmol of 2,4-toluene diisocyanate were mixed, heated to 90° C. in a nitrogen atmosphere, and reacted for 1 hour to obtain a terminal isocyanate prepolymer.
[0038] (5) Add 6.8 g of 1,4-butanediamine, 54 g of polyvinyl pyrrolidone copolymer, and 3 g of PVP-modified carbon nanotubes to 200 mL of water; add 100 g of terminal isocyanate prepolymer after stirring to obtain an antistatic water-based polyurea coating.
[0039] Example 4
[0040] (1) 28 g of N-vinyl pyrrolidone and 22 g of Boc-based polymerization monomer (prepared according to the method of Example 1) were added to 300 mL of N,N-dimethylformamide, heated to 85° C. in a nitrogen atmosphere, added with 0.38 g of azobisisobutyronitrile, reacted for 12 h, cooled, added with petroleum ether to precipitate, filtered, added to dichloromethane, added with trifluoroacetic acid, stirred for 8 h, distilled under reduced pressure, washed with a saturated sodium bicarbonate solution, and dried to obtain a polyvinyl pyrrolidone copolymer.
[0041] (2) Add 13.7 g of diethyltoluenediamine, 60 g of polyvinylpyrrolidone copolymer, and 4 g of PVP-modified carbon nanotubes (prepared according to the method in Example 1) to 200 mL of water; after stirring, add 100 g of terminal isocyanate prepolymer (prepared according to the method in Example 1) to obtain an antistatic water-based polyurea coating.
[0042] Comparative Example 1
[0043] (1) Add 6.8 g of diethyltoluenediamine and 42 g of amino-terminated polyether D2000 to 150 mL of water; after stirring, add 100 g of terminal isocyanate prepolymer to obtain a polyurea coating.
[0044] Comparative Example 2
[0045] (1) Add 6.8 g of diethyltoluenediamine and 42 g of polyvinylpyrrolidone copolymer to 150 mL of water; after stirring, add 100 g of terminal isocyanate prepolymer to obtain a polyurea coating.
[0046] Comparative Example 3
[0047] (1) Add 6.8 g of diethyltoluenediamine, 42 g of polyvinylpyrrolidone copolymer, and 1 g of carbon nanotubes to 150 mL of water; after stirring, add 100 g of terminal isocyanate prepolymer to obtain a polyurea coating.
[0048] Comparative Example 4
[0049] (1) Add 6.8 g of diethyltoluenediamine, 42 g of polyvinylpyrrolidone, and 1 g of PVP-modified carbon nanotubes to 150 mL of water; add 100 g of terminal isocyanate prepolymer after stirring to obtain a polyurea coating.
[0050] Comparative Example 5
[0051] (1) Add 18 g of Boc-based polymerization monomer to 300 mL of N,N-dimethylformamide, heat to 70° C. in a nitrogen atmosphere, add 0.35 g of azobisisobutyronitrile, react for 18 h, cool, add petroleum ether to precipitate, filter, add the precipitate to dichloromethane, add trifluoroacetic acid, stir and react for 5 h, evaporate under reduced pressure, wash with saturated sodium bicarbonate solution, and dry to obtain an acrylate polymer.
[0052] (2) Add 6.8 g of diethyltoluenediamine, 42 g of acrylate polymer, and 1 g of PVP-modified carbon nanotubes to 150 mL of water; add 100 g of terminal isocyanate prepolymer after stirring to obtain a polyurea coating.
[0053] The antistatic waterborne polyurea coating was sprayed on the substrate surface with a spray gun, cured at room temperature for 7 days, dried, and formed into a paint film for performance testing. The conductivity of the polyurea paint film was measured with a high resistance meter. The paint film sample was a circular sample with a diameter of 20 cm and a thickness of 8 mm. The thermal conductivity of the paint film was tested with a thermal conductivity tester using the transient plane heat source method.
[0054] The polyurea coating was poured into the mold, cured at room temperature for 7 days, and dried to form a film. The tensile properties of the film were tested according to GB / T528-2009, and the tear strength was tested according to GB / T 529-2008.
[0055] The test results are shown in the table below.
[0056]
[0057] After testing, polyvinyl pyrrolidone copolymer and PVP modified carbon nanotubes were added to the polyurea coatings of Examples 1-4. After the carbon nanotubes were modified by PVP dispersant, they had better dispersibility in the polyurea water-based coatings, and could form a uniform conductive and thermal conductive network, which significantly improved the electrical and thermal conductivity of the coating film, and had good antistatic and thermal conductivity. At the same time, the mechanical properties of the polyurea were enhanced. The added polyvinyl pyrrolidone copolymer contains hydrophilic carboxyl groups and has good dispersibility in water-based polyurea coatings. The molecular side chains contain a large number of amino groups and can react with the isocyanate groups of the terminal isocyanate prepolymers to form a three-dimensional chemical crosslinking effect, which is beneficial to improving the crosslinking degree of the polyurea and improving the mechanical properties. At the same time, after the copolymer reacts with the terminal isocyanate prepolymer, the formed polyurea contains polyvinyl pyrrolidone chain segments and has good interface compatibility with the polyvinyl pyrrolidone on the surface of the modified carbon nanotubes, thereby enhancing the interface effect between the carbon nanotubes and the polyurea, improving the compatibility between the two, and making the carbon nanotubes have a better reinforcing effect. Under the synergistic effect, the tensile properties and tear strength of the polyurea coating are enhanced.
[0058] The difference between Comparative Example 1 and Example 1 is that PVP-modified carbon nanotubes are not added, and the terminal amino polyether D2000 is used instead of the polyvinyl pyrrolidone copolymer. The terminal amino polyether D2000 contains amino groups only at the terminal position, and the side chain does not contain a large number of amino groups. It is impossible to undergo a three-dimensional chemical crosslinking reaction with the terminal isocyanate prepolymer, and it is difficult to effectively improve the crosslinking degree of the polyurea. The mechanical properties of the polyurea, such as the tensile strength, are low. In addition, without the addition of PVP-modified carbon nanotubes, the thermal conductivity and electrical conductivity of the polyurea are low.
[0059] The difference between Comparative Example 2 and Example 1 is that the thermal conductivity and electrical conductivity of the polyurea are lower without adding PVP modified carbon nanotubes. And the mechanical properties such as tensile strength are lower than those of Example 1, but the polyvinyl pyrrolidone copolymer is added, and the molecular side chain contains a large number of amino groups, which can react with the isocyanate group of the terminal isocyanate prepolymer to form a three-dimensional chemical crosslinking effect, which is beneficial to improve the crosslinking degree of the polyurea and improve the mechanical properties. The tensile strength and breaking strength are higher than those of Comparative Example 1.
[0060] The difference between Comparative Example 3 and Example 1 is that unmodified carbon nanotubes are added, the dispersion of carbon nanotubes is poor, no uniform conductive and thermal conductive network is formed, and the electrical conductivity and thermal conductivity of the paint film are lower than those of Example 1. In addition, the compatibility of carbon nanotubes with polyurea is poor, the reinforcement effect is not good, and the tensile strength and breaking strength are lower than those of Example 1.
[0061] The difference between Comparative Example 4 and Example 1 is that polyvinyl pyrrolidone is used instead of polyvinyl pyrrolidone copolymer, whose side chain does not contain amino groups and cannot undergo cross-linking reaction with terminal isocyanate prepolymer, resulting in the mechanical properties of polyurea being lower than those in Example 1.
[0062] The difference between Comparative Example 5 and Example 1 is that N-vinyl pyrrolidone was not added when preparing the acrylic ester polymer. Its side chain contains a large number of amino groups, which can undergo cross-linking reactions with the terminal isocyanate prepolymer to improve the mechanical properties of the polyurea. However, the generated polyurea does not contain polyvinyl pyrrolidone segments, and the interface interaction and compatibility between it and the PVP-modified carbon nanotubes are low, resulting in a lower reinforcing effect of the carbon nanotubes than in Example 1, and lower mechanical properties such as tensile strength than in Example 1.
[0063] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. An antistatic water-based polyurea coating, characterized in that: The antistatic water-based polyurea coating comprises component A and component B; Component A is 100 parts by weight of terminal isocyanate prepolymer; Component B is 6.8-13.7 parts by weight of a diamine chain extender, 42-60 parts by weight of a polyvinyl pyrrolidone copolymer, and 1-4 parts by weight of PVP modified carbon nanotubes; The preparation method of the polyvinyl pyrrolidone copolymer is as follows: add N-vinyl pyrrolidone and Boc-based polymerization monomer to N,N-dimethylformamide, heat to 70-85° C. in a nitrogen atmosphere, add azobisisobutyronitrile, react for 10-18 hours, add petroleum ether to precipitate a precipitate after cooling, add the precipitate to dichloromethane after filtering, add trifluoroacetic acid, stir and react for 5-8 hours, distill under reduced pressure, wash with a saturated sodium bicarbonate solution, and dry to obtain the polyvinyl pyrrolidone copolymer; The structural formula of the Boc-based polymerizable monomer is:
2. The antistatic waterborne polyurea coating according to claim 1, characterized in that: The mass ratio of the N-vinyl pyrrolidone, the Boc-based polymerization monomer, and azobisisobutyronitrile is (5-7):(3-5):(0.07-0.08).
3. The antistatic waterborne polyurea coating according to claim 2, characterized in that: The preparation method of the Boc-based polymer monomer is as follows: sodium hydride is added to N,N-dimethylformamide under an ice bath, 2-bromoethyl acrylate and Boc-cysteine are added in a nitrogen atmosphere, and then the mixture is reacted at 20-30° C. for 18-24 hours, hydrochloric acid is added to the solution to adjust the pH to 2-3, and then water and dichloromethane are added for extraction and separation, the organic phase is dried over anhydrous sodium sulfate, filtered and then distilled under reduced pressure, and the product is recrystallized with dichloromethane to obtain the Boc-based polymer monomer.
4. The antistatic waterborne polyurea coating according to claim 3, characterized in that: The mass ratio of the sodium hydride, 2-bromoethyl acrylate and Boc-cysteine is (0.72-0.84):1:(1.3-1.4).
5. The antistatic waterborne polyurea coating according to claim 1, characterized in that: In the component A, the preparation method of the terminal isocyanate prepolymer is: mixing dry polyether polyol and diisocyanate compound in a molar ratio of 1:(2.2-2.4), heating to 80-90° C. in a nitrogen atmosphere, and reacting for 1-2 hours to obtain the terminal isocyanate prepolymer.
6. The antistatic waterborne polyurea coating according to claim 5, characterized in that: The diisocyanate compound is 2,4-toluene diisocyanate or diphenylmethane-4,4'-diisocyanate.
7. The antistatic waterborne polyurea coating according to claim 1, characterized in that: The diamine chain extender in the B component includes 1,4-butylene diamine, meta-phenylenediamine, and diethyltoluenediamine.
8. The antistatic waterborne polyurea coating according to claim 1, characterized in that: The preparation method of the PVP modified carbon nanotubes in the B component is: adding carbon nanotubes, polyvinyl pyrrolidone dispersant and water into the grinding tank of a grinder, grinding with zirconium beads until the length of the carbon nanotubes is less than 10um, spray drying the grinding liquid to obtain PVP modified carbon nanotubes.
9. The antistatic waterborne polyurea coating according to claim 8, characterized in that: The mass ratio of the carbon nanotubes, polyvinyl pyrrolidone and water is 1:(0.3-0.5):(16-20).
10. The method for preparing the antistatic waterborne polyurea coating according to any one of claims 1 to 9, characterized in that: The preparation method comprises: adding component B: diamine chain extender, polyvinyl pyrrolidone copolymer, and PVP modified carbon nanotubes into water; After stirring, add the terminal isocyanate prepolymer of component A to obtain an antistatic water-based polyurea coating.
Citation Information
Patent Citations
Preparation of amphoteric carbon nanotube dispersion powder
CN102275899A
Viscoelastic damping material with good conductivity and preparing method thereof
CN105384888A
Oral care composition
CN111432794A
Antistatic explosion-proof polyurea material as well as preparation method and application thereof
CN111808261A
Low-viscosity and high-conductivity carbon nanotube conductive paste and preparation method and application thereof