Road marking paint for high-humidity environment and preparation method of road marking paint
Through the combination of nanocil modified acrylic polyurethane and modified diisopropyl peroxide curing agent, a multi-layer structural coating was prepared, which solved the stability and wear resistance of road marking coatings in the prior art under high humidity environments in the prior art The problem has significantly improved the performance of the paint.
Patent Information
- Application Number
- CN202411456750.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing two-component road marking coatings show problems such as long drying time, poor adhesion, poor stain resistance, discoloration and wear resistance in high humidity environments, especially in high humidity environments in southern regions. More prominent.
By modifying acrylic polyurethane with nanoclays and preparing nanosilica microcapsules, combined with modified diisopropyl peroxide curing agent, a multi-layer structural coating is formed to enhance the barrier properties of the coating and under high humidity environments. stability.
It significantly improves the stability and wear resistance of road marking coatings in high humidity environments, enhances stain resistance and UV resistance, and extends the service life of the coating.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coating preparation, and in particular to a road marking coating for a high-humidity environment and a preparation method thereof. Background Art
[0002] With the development of transportation construction, transportation and traffic safety are becoming more and more important. As an important part of transportation and traffic safety, road markings are widely used in highways and airports of all levels. Compared with other coatings, road markings need to withstand harsh environmental tests, especially for road markings in southern regions, which have to face the test of harsh environments such as high temperature, high humidity, and strong ultraviolet rays. Due to the particularity of the application environment of traffic markings, the particularity of the materials used to prepare road markings is determined.
[0003] The two-component road marking paints commonly found on the market are usually polyurethane, epoxy, polyurea, and MA (methyl methacrylate monomer) types. These common two-component road marking paints have the characteristics of long solid drying time, poor adhesion, poor anti-fouling, and prominent discoloration problems. And the impact of high humidity is more prominent in the southern region, especially in the annual return of the south wind in the southern region. Due to excessive humidity, it is easy to condense and form water beads on the surface of the road markings. In this high humidity environment, the road markings will be more prone to aging, and the coating will be prone to cracking and the wear resistance will be reduced. The two-component road marking paints currently on the market cannot cope well with high humidity environments. There is an urgent need for a road marking paint with high humidity resistance on the market. Summary of the invention
[0004] The present invention aims to provide a road marking paint for high humidity environment and a preparation method thereof, so as to solve the disadvantage that the road marking paint in the prior art is not resistant to high humidity environment.
[0005] The present invention is achieved by the following technical scheme. A method for preparing a road marking paint for a high humidity environment comprises the following steps: S100, firstly, using nano clay to modify acrylic polyurethane to prepare nano clay modified acrylic polyurethane, mixing deionized water, a dispersant and titanium dioxide and stirring evenly, grinding the mixture to a fineness of ≤50 μm, adding the nano clay modified acrylic polyurethane, stirring evenly to obtain a first coating; wherein, in parts by weight, the deionized water is 100 parts, the dispersant is 2 to 5 parts, and the titanium dioxide is 10 to 10 parts. 20 parts, S200, using a polymer chain to modify dicumyl peroxide to prepare a modified curing agent; S300, modifying nano-silica, and encapsulating the modified nano-silica with polylactic acid-glycolic acid copolymer and gelatin to prepare microcapsules; S400, mixing the modified curing agent and the microcapsules in a weight fraction ratio of 1:0.2, adding deionized water and titanium dioxide, and stirring to obtain a second coating; mixing the first coating and the second coating in a weight fraction ratio of 1:0.5 to obtain a road marking coating.
[0006] Further, the nanoclay-modified acrylic polyurethane is prepared by the following method: S110, adding 1 part of an organic silane coupling agent by weight to 99 parts of an ethanol solvent and using ultrasonic dispersion to prepare an organic silane coupling solvent, wherein the ultrasonic dispersion frequency is 80-90 KHz and the dispersion time is 30-35 min; S120, then adding 100 parts of nanoclay by weight to the organic silane coupling solvent, stirring evenly and heating to react, wherein the heating temperature is 80-90° C. and the heating time is 0.5-1 h; S130, adding 20 parts of high-hydroxyl acrylic polyurethane by weight to 80 parts of ethyl acetate, stirring until the high-hydroxyl acrylic polyurethane is completely dissolved, wherein the stirring temperature is 40-50° C., to prepare an acrylic solution; S140, mixing the nanoclay mixed solution and the acrylic solution, heating to 40° C., using ultrasonic stirring for 40-60 min, and the ultrasonic frequency is 90-110 KHz, to prepare nanoclay-modified acrylic polyurethane.
[0007] Furthermore, the modified curing agent is prepared by the following steps: S210, methyl methacrylate and 2-hydroxyethyl methacrylate are mixed in a weight ratio of 9:1; S220, azobisisobutyronitrile is added to the mixture as an initiator under nitrogen protection, the mixture is heated to 70°C, and maintained for 2-4 hours until the methyl methacrylate and 2-hydroxyethyl methacrylate monomers are converted into polymers; S230, dicumyl peroxide is added to ethyl acetate solvent and mixed, and the synthesized polymer is added to the solvent under nitrogen protection and mixed evenly; S240, the mixed solvent is heated to 45-55°C and maintained for 1-2 hours to promote the grafting reaction of dicumyl peroxide with the polymer chain; S250, after the reaction is completed, the mixed solution is cooled to room temperature and filtered to obtain a filter cake, and the filter cake is washed 5 times with deionized water to remove unreacted dicumyl peroxide, polymer and initiator; S260, the washed polymer is dried in a vacuum drying oven to obtain a modified curing agent.
[0008] Further, the microcapsules are prepared by the following steps: S310, modifying the nano-silica to enhance its hydrophobic properties, and then uniformly dispersing the modified nano-silica in anhydrous ethanol by stirring to prepare a nano-silica solution, wherein the stirring speed is 1200-1500 rpm and the time is 20-35 min; S320, dissolving polylactic acid-glycolic acid copolymer in dichloromethane to prepare a dichloromethane mixed solution; S330, placing the dichloromethane mixed solution on a hot plate, heating the mixed solution to 45° C. and maintaining it, and slowly adding the modified nano-silica solution to the mixed solution, stirring Mix the solutions until they are evenly mixed to obtain a first coating solution; S340, dissolve gelatin in deionized water to prepare an aqueous solution, add glutaraldehyde for cross-linking treatment, and stir evenly to obtain a second coating solution; S350, dropwise add the first coating solution into the second coating solution, and stir with a high-speed stirrer to form a double emulsion; S360, place the double emulsion in a rotary evaporator, slowly evaporate dichloromethane under low pressure, solidify the polylactic acid-glycolic acid copolymer, and form an inner shell; S370, then stand at room temperature for 6 hours to wait for the outer layer of gelatin to coagulate, and use a centrifugal method to separate to obtain microcapsules coated with modified nano-silica.
[0009] Further, the modification of nano-silicon dioxide includes the following steps: S311, first pre-treating the nano-silicon dioxide, dispersing 100 parts of nano-silicon dioxide by weight in deionized water, and using 90-110KHz ultrasonic cleaning for 30 minutes to remove surface impurities; S312, dissolving 2-5 parts of hexadecyltrichlorosilane by weight in 500 ml of anhydrous ethanol, stirring evenly to prepare a modified solution; S313, adding 100 parts of dry nano-silicon dioxide to the modified solution, and using 90-110KHz ultrasonic dispersion for 30-45 minutes. ; S314. After the nano-silica is completely dispersed in the modified solution, 5 ml of 0.1M hydrochloric acid is added to the modified solution as a catalyst, and the reaction is carried out under stirring. The stirring reaction is continued for 12 hours to ensure that the hexadecyltrichlorosilane fully reacts with the surface of the nano-silica; S315. After the reaction is completed, the reaction mixture is filtered through filter paper to obtain a modified nano-silica filter cake, and the filter cake is washed alternately with anhydrous ethanol and deionized water for 3 times to remove unreacted hexadecyltrichlorosilane and by-products; S316. The washed nano-silica is dried in a vacuum drying oven at 60°C for 12 hours to prepare modified nano-silica.
[0010] Further, the nanoclay may include montmorillonite nanoclay, kaolinite nanoclay and halloysite nanoclay.
[0011] In another aspect, the present invention provides a road marking paint for use in a high humidity environment. The paint is prepared according to the preparation method described above.
[0012] Another aspect of the present invention provides a composite coating for road marking in a high humidity environment, comprising an acrylic polyurethane primer layer sprayed on cement and a dicumyl peroxide topcoat layer.
[0013] Furthermore, the dicumyl peroxide topcoat layer contains microcapsules. When the ambient humidity is greater than 95%, the microcapsules rupture and release the encapsulated modified nano-silicon dioxide slurry.
[0014] Furthermore, the thickness of the dicumyl peroxide topcoat layer is 0.5-1 mm; the thickness of the acrylic polyurethane primer layer is 0.7-1.7 mm.
[0015] Compared with the prior art, the present invention has the following beneficial effects:
[0016] 1. The present invention uses nanoclay to modify acrylic polyurethane. The sheet structure of nanoclay can effectively hinder the penetration of gas and liquid, improve the barrier property of the material, and thus effectively improve the stability of acrylic polyurethane coating in a high humidity environment.
[0017] 2. The present invention adds a multi-layer structure microcapsule designed and prepared in the curing agent, and realizes the response to the high humidity environment stimulus through the carefully planned layer design, thereby accurately controlling the release of the contained substances. In a high humidity environment, through the synergistic effect of the outer layer and the middle layer, the rupture of the microcapsule and the release of the core substance can be effectively controlled, thereby improving the high humidity resistance of the entire road marking in a high humidity environment. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment, and the illustrative embodiments of the present invention and its description are only used to explain the present invention, and are not used as limitation of the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper limit and the lower limit of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper limit and lower limit of these smaller ranges can be independently included or excluded in the scope.
[0019] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0020] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0021] The terms "include", "comprising", "having", "containing", etc. used in this document are open-ended terms, which mean including but not limited to. In addition, the terms "first", "second", etc. are only used to distinguish descriptions and cannot be understood as indicating or implying relative importance.
[0022] Embodiment 1:
[0023] This embodiment provides a method for preparing a road marking coating for a high humidity environment. The parts mentioned in this embodiment are all in parts by weight. The preparation method comprises the following steps:
[0024] Step 1: Prepare the custom acrylic polyurethane.
[0025] Specifically, the preparation of the tailor-made acrylic polyurethane may include the following sub-steps:
[0026] First, the nanoclay is pretreated, and 1 part of the organosilane coupling agent is added to 99 parts of the ethanol solvent and dispersed by ultrasonic wave to prepare the organosilane coupling solvent, wherein the ultrasonic dispersion frequency is 80 KHz and the dispersion time is 30 min. It should be noted that the nanoclay used in this embodiment is montmorillonite nanoclay.
[0027] Then, 100 parts of montmorillonite nanoclay were added into the organosilane coupling solvent, stirred evenly and heated for reaction; wherein, the heating temperature was 80° C. and the heating time was 0.5 h.
[0028] Deionized water, dispersant and titanium dioxide are mixed and stirred evenly, and the mixture is ground to a fineness of ≤50 μm, and added to the montmorillonite nanoclay solution after the reaction is completed to prepare a montmorillonite nanoclay mixed solution.
[0029] Among them, deionized water is 100 parts, dispersant is 2 parts, and titanium dioxide is 10 parts.
[0030] 20 parts of high-hydroxyl acrylic polyurethane were added into 80 parts of ethyl acetate, and stirred until the high-hydroxyl acrylic polyurethane was completely dissolved, wherein the stirring temperature was 40° C., to prepare an acrylic polyurethane solution.
[0031] The nanoclay mixed solution and the acrylic acid solution were mixed, heated to 40° C., and stirred with ultrasound for 40 minutes at an ultrasonic frequency of 90 KHz to prepare montmorillonite nanoclay modified acrylic polyurethane.
[0032] It should be noted that the high aspect ratio and large surface area of nanoclay enable it to form a good interface bond within the polymer matrix. The use of nanoclay to modify acrylic polyurethane can effectively enhance the tensile strength of acrylic polyurethane, making the material perform better when subjected to tensile stress. At the same time, nanoclay has good thermal stability, and its distribution in the polymer matrix can hinder the heat conduction path, which means that the modified acrylic polyurethane can maintain its performance at higher temperatures. Most importantly, the lamellar structure of nanoclay can effectively hinder the penetration of gases and liquids, thereby improving the barrier properties of the material and effectively improving the stability of acrylic polyurethane coatings in high humidity environments. And nanoclay itself is a natural material, and its addition can reduce the use of certain chemical additives, making the modified acrylic polyurethane material more environmentally friendly.
[0033] Step 2, preparing a modified dicumyl peroxide curing agent, specifically comprising the following steps;
[0034] Methyl methacrylate (MMA) and 2-hydroxyethyl methacrylate (HEMA) were mixed in a weight ratio of MMA: HEMA = 9:1. A small amount of azobisisobutyronitrile (AIBN) was added to the mixture as an initiator under nitrogen protection. The mixture was heated to 70°C and maintained for 2 hours until the monomer was completely converted into a polymer.
[0035] The synthesized polymer and a certain amount of dicumyl peroxide are added to an ethyl acetate solvent and mixed, and the mixed solvent is heated to 45° C. and maintained for 1 hour under nitrogen protection to promote the grafting reaction of dicumyl peroxide with the polymer chain.
[0036] After the reaction is completed, the mixed solution is cooled to room temperature and filtered to obtain a filter cake, and the filter cake is washed 5 times with deionized water to remove unreacted dicumyl peroxide, polymer and initiator. The washed polymer is dried in a vacuum drying oven to obtain modified dicumyl peroxide.
[0037] Step 3: preparing nano-silicon dioxide microcapsules.
[0038] Specifically, the following sub-steps may be included:
[0039] First, nanosilica needs to be modified to further enhance its hydrophobic properties.
[0040] Specifically, the process includes the following steps: first, pre-treating the nano-silicon dioxide, dispersing 100 parts of the nano-silicon dioxide in deionized water, and using 90KHz ultrasonic cleaning for 30 minutes to remove surface impurities. The nano-silicon dioxide that has been ultrasonically cleaned is dried at 60°C for 6 hours to ensure that it is completely dry.
[0041] Dissolve 2 parts of hexadecyltrichlorosilane in 500 ml of anhydrous ethanol and stir evenly to prepare a modified solution.
[0042] 100 parts of dry nano-silicon dioxide were added to the modified solution and dispersed using 90 KHz ultrasound for 30 minutes.
[0043] After the nano-silica is completely dispersed in the modified solution, 5 ml of 0.1M hydrochloric acid is added to the modified solution as a catalyst, and the reaction is carried out under stirring. The stirring reaction is continued for 12 hours to ensure that the hexadecyltrichlorosilane fully reacts with the surface of the nano-silica. During the reaction, the room temperature (25°C) is maintained or slightly heated to 40°C to accelerate the reaction rate.
[0044] After the reaction is completed, the reaction mixture is filtered through filter paper to obtain a modified nano-silica filter cake, which is washed three times alternately with anhydrous ethanol and deionized water to remove unreacted hexadecyltrichlorosilane and by-products;
[0045] The washed nano-silica was dried in a vacuum drying oven at 60° C. for 12 h to prepare modified nano-silica.
[0046] It should be noted that the modification of nano-silica by hexadecyltrichlorosilane can effectively enhance the hydrophobic properties of silica, and can make the modified silica show better dispersibility and stability in water and other polar solvents, which is suitable for application scenarios that require hydrophobic properties. And according to the subsequent microcapsule preparation process, it was found that the hexadecyltrichlorosilane modification can effectively reduce the surface energy of nano-silica, making it easier to disperse in a medium with low surface energy, avoiding sedimentation and agglomeration, which has a good effect on the subsequent preparation of microcapsules. The nano-silica modified by hexadecyltrichlorosilane has better dispersibility in organic solvents and polymer matrices, and is easier to form a microcapsule structure. After analysis, it is believed that this may be because the long-chain alkyl can reduce the van der Waals force and hydrogen bonding between nanoparticles, reduce agglomeration, thereby improving the uniformity and performance of the material, so that the preparation of microcapsules is more convenient.
[0047] At the same time, subsequent experiments have found that the modified nano-silica microcapsules can be broken in a high humidity environment to release the modified nano-silica, which can repair the road markings and enhance the overall scratch resistance and wear resistance of the road markings in a high humidity environment.
[0048] After the modified nano-silicon dioxide is prepared, the nano-silicon dioxide is uniformly dispersed in anhydrous ethanol by stirring to prepare a modified nano-silicon dioxide solution, wherein the stirring speed is 1200 rpm and the stirring time is 20 minutes.
[0049] Poly(lactic-co-glycolic acid) (PLGA) was dissolved in dichloromethane (DCM) to prepare a mixed solution.
[0050] The mixed solution is placed on a hot plate, heated to 45° C. and maintained at this temperature, and the modified nano-silica solution is slowly added to the mixed solution, and the mixed solution is stirred until the two are evenly mixed to obtain a first encapsulation solution.
[0051] Gelatin is dissolved in deionized water to prepare an aqueous solution, and glutaraldehyde is added for cross-linking treatment, and stirred evenly to prepare a second coating solution. The purpose of adding glutaraldehyde is to allow glutaraldehyde and gelatin to cross-link to control the sensitivity of gelatin to humidity changes.
[0052] The first coating solution was added dropwise into the second coating solution while being stirred by a high-speed stirrer to form a water-in-oil-in-water (W / O / W) double emulsion.
[0053] The double emulsion is placed in a rotary evaporator to slowly evaporate dichloromethane under low pressure to solidify the polylactic acid-co-glycolic acid (PLGA) to form an inner shell.
[0054] Then the mixture was allowed to stand at room temperature for 6 hours to allow the outer layer of gelatin to coagulate, and the microcapsules encapsulating the modified nano-silica were separated by centrifugation.
[0055] Step 4: Add the prepared modified diisopropylbenzene peroxide curing agent and nano-silicon dioxide microcapsules in a weight ratio of 1:0.2, deionized water and titanium dioxide, and mix and stir to obtain a cured coating.
[0056] When in use, the cured coating is added to the prepared special acrylic polyurethane coating, and corresponding glass microbeads are added to the coating according to national standards to obtain a road marking coating for a high humidity environment.
[0057] Embodiment 2,
[0058] This embodiment provides a method for preparing a road marking coating for a high humidity environment. The parts mentioned in this embodiment are all in parts by weight. The preparation method comprises the following steps:
[0059] Step 1: Prepare the custom acrylic polyurethane.
[0060] Specifically, the preparation of the tailor-made acrylic polyurethane may include the following sub-steps:
[0061] First, the nanoclay was pretreated, and 1 part of the organosilane coupling agent was added to 99 parts of the ethanol solvent and dispersed by ultrasonic wave to prepare the organosilane coupling solvent, wherein the ultrasonic dispersion frequency was 85 KHz and the dispersion time was 32 min. It should be noted that the nanoclay used in this embodiment is kaolinite nanoclay.
[0062] Then, 100 parts of kaolinite nanoclay were added into the organosilane coupling solvent, stirred evenly and heated for reaction; wherein, the heating temperature was 85° C. and the heating time was 45 min.
[0063] Deionized water, dispersant and titanium dioxide are mixed and stirred evenly, and the mixture is ground to a fineness of ≤50 μm, and added to the kaolinite nanoclay solution after the reaction is completed to prepare a kaolinite nanoclay mixed solution, wherein the deionized water is 100 parts, the dispersant is 3 parts, and the titanium dioxide is 15 parts.
[0064] 20 parts of high-hydroxyl acrylic polyurethane were added into 80 parts of ethyl acetate, and stirred until the high-hydroxyl acrylic polyurethane was completely dissolved, wherein the stirring temperature was 45° C., to prepare an acrylic acid solution.
[0065] The kaolinite nanoclay mixed solution and the acrylic acid solution were mixed, heated to 40° C., and stirred with ultrasound for 50 minutes at an ultrasonic frequency of 100 KHz to prepare kaolinite nanoclay modified acrylic polyurethane.
[0066] Step 2: In this embodiment, the dicumyl peroxide curing agent used is a commercially available dicumyl peroxide curing agent, and a modification operation is performed on it.
[0067] Step 3: preparing nano-silicon dioxide microcapsules.
[0068] Specifically, the following sub-steps may be included:
[0069] First, nanosilica needs to be modified to further enhance its hydrophobic properties.
[0070] Specifically, the process includes the following steps: first, pre-treating the nano-silicon dioxide, dispersing 100 parts of the nano-silicon dioxide in deionized water, and using 100KHz ultrasonic cleaning for 30 minutes to remove surface impurities. The nano-silicon dioxide that has been ultrasonically cleaned is dried at 60°C for 6 hours to ensure that it is completely dry.
[0071] Dissolve 2-5 parts of hexadecyltrichlorosilane in 500 ml of anhydrous ethanol and stir evenly to prepare a modified solution.
[0072] 100 parts of dry nano-silicon dioxide were added to the modified solution and dispersed using 90-110 KHz ultrasound for 35 min.
[0073] After the nano-silica is completely dispersed in the modified solution, 5 ml of 0.1M hydrochloric acid is added to the modified solution as a catalyst, and the reaction is carried out under stirring. The stirring reaction is continued for 12 hours to ensure that the hexadecyltrichlorosilane fully reacts with the surface of the nano-silica. During the reaction, the room temperature (25°C) is maintained or slightly heated to 40°C to accelerate the reaction rate.
[0074] After the reaction is completed, the reaction mixture is filtered through filter paper to obtain a modified nano-silica filter cake, which is washed three times alternately with anhydrous ethanol and deionized water to remove unreacted hexadecyltrichlorosilane and by-products;
[0075] The washed nano-silica was dried in a vacuum drying oven at 60° C. for 12 h to prepare modified nano-silica.
[0076] After the modified nano-silicon dioxide is prepared, the nano-silicon dioxide is uniformly dispersed in anhydrous ethanol by stirring to prepare a modified nano-silicon dioxide solution, wherein the stirring speed is 1350 rpm and the stirring time is 30 minutes.
[0077] Poly(lactic-co-glycolic acid) (PLGA) was dissolved in dichloromethane (DCM) to prepare a mixed solution.
[0078] The mixed solution is placed on a hot plate, heated to 45° C. and maintained at this temperature, and the modified nano-silica solution is slowly added to the mixed solution, and the mixed solution is stirred until the two are evenly mixed to obtain a first encapsulation solution.
[0079] Gelatin is dissolved in deionized water to prepare an aqueous phase solution, glutaraldehyde is added for cross-linking treatment, and the solution is stirred evenly to prepare a second coating solution.
[0080] The first coating solution was added dropwise into the second coating solution while being stirred by a high-speed stirrer to form a water-in-oil-in-water (W / O / W) double emulsion.
[0081] The double emulsion is placed in a rotary evaporator to slowly evaporate dichloromethane under low pressure to solidify the polylactic acid-co-glycolic acid (PLGA) to form an inner shell.
[0082] Then the mixture was allowed to stand at room temperature for 6 hours to allow the outer layer of gelatin to coagulate, and the microcapsules encapsulating the modified nano-silica were separated by centrifugation.
[0083] Step 4: Add the prepared modified diisopropylbenzene peroxide curing agent and nano-silica microcapsules in a weight ratio of 1:0.2, deionized water and titanium dioxide, and mix and stir to obtain a cured coating.
[0084] When in use, the cured coating is added to the prepared special acrylic polyurethane coating, and corresponding glass microbeads are added to the coating according to national standards to obtain a road marking coating for a high humidity environment.
[0085] Embodiment 3,
[0086] This embodiment provides a method for preparing a road marking coating for a high humidity environment. The parts mentioned in this embodiment are all in parts by weight. The preparation method comprises the following steps:
[0087] Step 1: Prepare the custom acrylic polyurethane.
[0088] Specifically, the preparation of the tailor-made acrylic polyurethane may include the following sub-steps:
[0089] First, the nanoclay is pretreated, and 1 part of the organosilane coupling agent is added to 99 parts of the ethanol solvent and dispersed by ultrasonic wave to prepare the organosilane coupling solvent, wherein the ultrasonic dispersion frequency is 90 KHz and the dispersion time is 35 min. It should be noted that the nanoclay used in this embodiment is halloysite nanoclay (natural halloysite nanotube).
[0090] Then, 100 parts of halloysite nanoclay were added into the organosilane coupling solvent, stirred evenly and heated for reaction; wherein the heating temperature was 90° C. and the heating time was 1 hour.
[0091] Deionized water, dispersant and titanium dioxide are mixed and stirred evenly, and the mixture is ground to a fineness of ≤50 μm, and added to the halloysite nanoclay solution after the reaction is completed to prepare a halloysite nanoclay mixed solution, wherein the deionized water is 100 parts, the dispersant is 5 parts, and the titanium dioxide is 20 parts.
[0092] 20 parts of high-hydroxyl acrylic polyurethane were added into 80 parts of ethyl acetate, and stirred until the high-hydroxyl acrylic polyurethane was completely dissolved, wherein the stirring temperature was 50° C., to prepare an acrylic solution.
[0093] The halloysite nanoclay mixed solution and the acrylic acid solution were mixed, heated to 40° C., and ultrasonically stirred for 60 minutes at an ultrasonic frequency of 110 KHz to prepare halloysite nanoclay modified acrylic polyurethane.
[0094] Step 2, preparing a modified dicumyl peroxide curing agent, specifically comprising the following steps;
[0095] Methyl methacrylate (MMA) and 2-hydroxyethyl methacrylate (HEMA) were mixed in a weight ratio of MMA: HEMA = 9:1. A small amount of azobisisobutyronitrile (AIBN) was added to the mixture as an initiator under nitrogen protection. The mixture was heated to 70°C and maintained for 4 hours until the monomer was completely converted into a polymer.
[0096] The synthesized polymer and a certain amount of dicumyl peroxide were added to an ethyl acetate solvent and mixed, and under nitrogen protection, the mixed solvent was heated to 55° C. and maintained for 2 hours to promote the grafting reaction of dicumyl peroxide with the polymer chain.
[0097] After the reaction is completed, the mixed solution is cooled to room temperature and filtered to obtain a filter cake, and the filter cake is washed 5 times with deionized water to remove unreacted dicumyl peroxide, polymer and initiator. The washed polymer is dried in a vacuum drying oven to obtain modified dicumyl peroxide.
[0098] Step 3: preparing nano-silicon dioxide microcapsules.
[0099] Specifically, the following sub-steps may be included:
[0100] First, nanosilica needs to be modified to further enhance its hydrophobic properties.
[0101] Specifically, the process includes the following steps: first, pre-treating the nano-silicon dioxide, dispersing 100 parts of the nano-silicon dioxide in deionized water, and using 110KHz ultrasonic cleaning for 30 minutes to remove surface impurities. The nano-silicon dioxide that has been ultrasonically cleaned is dried at 60°C for 6 hours to ensure that it is completely dry.
[0102] Dissolve 5 parts of hexadecyltrichlorosilane in 500 ml of anhydrous ethanol and stir evenly to obtain a modified solution.
[0103] 100 parts of dry nano-silicon dioxide were added to the modified solution and dispersed using 110 KHz ultrasound for 45 minutes.
[0104] After the nano-silica is completely dispersed in the modified solution, 5 ml of 0.1M hydrochloric acid is added to the modified solution as a catalyst, and the reaction is carried out under stirring. The stirring reaction is continued for 12 hours to ensure that the hexadecyltrichlorosilane fully reacts with the surface of the nano-silica. During the reaction, the room temperature (25°C) is maintained or slightly heated to 40°C to accelerate the reaction rate.
[0105] After the reaction is completed, the reaction mixture is filtered through filter paper to obtain a modified nano-silica filter cake, which is washed three times alternately with anhydrous ethanol and deionized water to remove unreacted hexadecyltrichlorosilane and by-products;
[0106] The washed nano-silica was dried in a vacuum drying oven at 60° C. for 12 h to prepare modified nano-silica.
[0107] At the same time, subsequent experiments have found that the modified nano-silica microcapsules can be broken in a high humidity environment to release the modified nano-silica, which can repair the road markings and enhance the overall scratch resistance and wear resistance of the road markings in a high humidity environment.
[0108] After the modified nano-silicon dioxide is prepared, the nano-silicon dioxide is uniformly dispersed in anhydrous ethanol by stirring to prepare a modified nano-silicon dioxide solution, wherein the stirring speed is 1500 rpm and the stirring time is 35 minutes.
[0109] Poly(lactic-co-glycolic acid) (PLGA) was dissolved in dichloromethane (DCM) to prepare a mixed solution.
[0110] The mixed solution is placed on a hot plate, heated to 45° C. and maintained at this temperature, and the modified nano-silica solution is slowly added to the mixed solution, and the mixed solution is stirred until the two are evenly mixed to obtain a first encapsulation solution.
[0111] Gelatin is dissolved in deionized water to prepare an aqueous phase solution, glutaraldehyde is added for cross-linking treatment, and the solution is stirred evenly to prepare a second coating solution.
[0112] The first coating solution was added dropwise into the second coating solution while being stirred by a high-speed stirrer to form a water-in-oil-in-water (W / O / W) double emulsion.
[0113] The double emulsion is placed in a rotary evaporator to slowly evaporate dichloromethane under low pressure to solidify the polylactic acid-co-glycolic acid (PLGA) to form an inner shell.
[0114] Then the mixture was allowed to stand at room temperature for 6 hours to allow the outer layer of gelatin to coagulate, and the microcapsules encapsulating the modified nano-silica were separated by centrifugation.
[0115] Step 4: Add the prepared modified diisopropylbenzene peroxide curing agent and nano-silicon dioxide microcapsules in a weight ratio of 1:0.2, deionized water and titanium dioxide, and mix and stir to obtain a cured coating.
[0116] When in use, the cured coating is added to the prepared special acrylic polyurethane coating, and corresponding glass microbeads are added to the coating according to national standards to obtain a road marking coating for a high humidity environment.
[0117] Embodiment 4,
[0118] The difference between this embodiment and embodiment 1 is that the steps of preparing nano-silicon dioxide microcapsules and preparing modified dicumyl peroxide are deleted. Specifically, the following contents are included:
[0119] Step 1: Prepare the custom acrylic polyurethane.
[0120] Specifically, the preparation of the tailor-made acrylic polyurethane may include the following sub-steps:
[0121] First, the nanoclay is pretreated, and 1 part of the organosilane coupling agent is added to 99 parts of the ethanol solvent and dispersed by ultrasonic wave to prepare the organosilane coupling solvent, wherein the ultrasonic dispersion frequency is 80 KHz and the dispersion time is 30 min. It should be noted that the nanoclay used in this embodiment is montmorillonite nanoclay.
[0122] Then, 100 parts of montmorillonite nanoclay were added into the organosilane coupling solvent, stirred evenly and heated for reaction; wherein, the heating temperature was 80° C. and the heating time was 0.5 h.
[0123] Deionized water, dispersant and titanium dioxide are mixed and stirred evenly, and the mixture is ground to a fineness of ≤50 μm, and added to the montmorillonite nanoclay solution after the reaction is completed to prepare a montmorillonite nanoclay mixed solution.
[0124] Among them, deionized water is 100 parts, dispersant is 2 parts, and titanium dioxide is 10 parts.
[0125] 20 parts of high-hydroxyl acrylic polyurethane were added into 80 parts of ethyl acetate, and stirred until the high-hydroxyl acrylic polyurethane was completely dissolved, wherein the stirring temperature was 40° C., to prepare an acrylic solution.
[0126] The nanoclay mixed solution and the acrylic acid solution were mixed, heated to 40° C., and stirred with ultrasound for 40 minutes at an ultrasonic frequency of 90 KHz to prepare montmorillonite nanoclay modified acrylic polyurethane.
[0127] Step 2: The dicumyl peroxide curing agent in this embodiment is a commercially available dicumyl peroxide curing agent (produced by Suzhou Senfida Chemical).
[0128] Step 3: Add deionized water and titanium dioxide to the commercially available diisopropylbenzene peroxide curing agent, and mix and stir to obtain a cured coating.
[0129] When in use, the cured coating is added to the prepared special acrylic polyurethane coating, and corresponding glass microbeads are added to the coating according to national standards to obtain a road marking coating for a high humidity environment.
[0130] Embodiment 5,
[0131] The difference between this embodiment and embodiment 1 is that nano clay is not used to modify the modified acrylic polyurethane. The remaining steps are the same as those in embodiment 1.
[0132] Comparative Example 1
[0133] Compared with Example 2, the special acrylic polyurethane is replaced by ordinary commercially available acrylic resin (produced by Suzhou Senfida Chemical), and the modified diisopropylbenzene peroxide curing agent is replaced by ordinary commercially available diisopropylbenzene peroxide curing agent, and no homemade nano-silica microcapsules are added.
[0134] Comparative Example 2
[0135] Compared with Example 2, this comparative example replaces the specially prepared acrylic polyurethane with common commercially available polyurethane resin.
[0136] Comparative Example 3
[0137] Compared with Example 2, this comparative example replaces the modified dicumyl peroxide curing agent with a commercially available dicumyl peroxide curing agent, and does not add the homemade nano-silica microcapsules.
[0138] Experimental example:
[0139] The products prepared by the above five embodiments and three comparative examples and the commercially available two-component water-based road marking paint were coated on the cement surface, so that the thickness of the coating in all experimental examples was 3mm±0.5mm, wherein the exposed area of each coating sample was 100 cm². The prepared experimental objects were sent to the aging laboratory, the humidity in the laboratory was adjusted to 95%, the temperature was adjusted to 45°C, and a xenon lamp was used to simulate the intensity of sunlight, the illumination intensity of the xenon lamp was 1000 W / m², and the aging time was 10 days. Table 1 shows the results after 10 days of aging experiment.
[0140] Table 1. Comparison of 10-day aging test results:
[0141] ;
[0142] Each sample was subjected to salt spray corrosion resistance test, acid and alkali resistance test and weather resistance test.
[0143] Among them, a salt spray test box with model LP / YWX-150 was used to conduct salt spray test on the samples. For alkali resistance test, a sodium hydroxide solution with pH=10 was first prepared, and the prepared sodium hydroxide solution was applied to the surface of the sample, and observations were made at regular intervals and records were made. For weather resistance test, a box-type ultraviolet light aging test box with model HT-UV3 was used to conduct ultraviolet aging weather resistance test. The coating was placed in an ultraviolet aging box with ultraviolet radiation (310nm, 1.5 kw) and continuously irradiated. At regular intervals, the degree of coating aging was observed and recorded. The results are shown in Table 2
[0144] Table 2 Related performance test results:
[0145] ;
[0146] According to the experimental method for two-component coatings in standard JT / T 280-2022 "Road Marking Paints", the wear resistance and coating adhesion tests were completed. The results are shown in Table 3.
[0147] Table 3. Abrasion resistance and adhesion test results:
[0148] ;
[0149] According to the above experimental results, it can be seen that the road marking paint prepared by the present invention has good anti-aging performance in the aging experiment under high humidity environment. At the same time, the paint prepared according to the preparation method described in this embodiment 1 has excellent performance in various tests, indicating that the road marking paint prepared by the modification operation in embodiment 1 has good tolerance to high humidity environment and good performance in other tests.
[0150] The diisopropylbenzene peroxide curing agent in Example 2 is a commercially available diisopropylbenzene peroxide curing agent, which has not been modified. It can be seen that there is not much difference in the effect of the basic ten-day aging test from that in Example 1, and there are only slight differences in the specific details test thereafter from the coating in Example 1. That is to say, in general construction, construction personnel can select a suitable curing agent according to the specific environmental conditions, and do not necessarily need to use the modified curing agent in Example 1, which can also make the road marking have good high humidity performance. At the same time, it can be seen from Table 2 that the adhesion of Example 2, Example 4, Comparative Example 1 and Comparative Example 3 are all lower than that of other experimental samples. Through analysis, we believe that the difference is caused by the diisopropylbenzene peroxide curing agent. The samples with lower adhesion all use the commercially available diisopropylbenzene peroxide curing agent, which has not been modified. We believe that by grafting with methyl methacrylate (MMA) and 2-hydroxyethyl methacrylate (HEMA) monomers, the modified dicumyl peroxide curing agent effectively improves the adhesion between the curing agent and the substrate, so that the final road marking paint has better adhesion performance than the commercially available unmodified dicumyl peroxide curing agent, which can effectively prevent the paint from falling off.
[0151] And through the above experiments, we also found that the coating of the present invention has good anti-ultraviolet ability. It is speculated that the improvement of the anti-ultraviolet ability of the present invention is mainly due to the following two reasons:
[0152] 1. The addition of nanoclay, the particle size of which is at the nanometer scale, can make the modified acrylic polyurethane perform better in terms of optical properties while maintaining its basic properties. This is reflected in the improved UV resistance of the entire material, and it has excellent performance in the UV weathering performance test. 2. The modified nano-silica microcapsules are broken in a high humidity environment to release the modified nano-silica contained therein, and the UV resistance of the modified nano-silica is also improved.
[0153] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
[0154] The invention discloses a method for preparing a road marking paint for a high humidity environment, which belongs to the field of paint preparation, including modifying acrylic polyurethane with nano clay to prepare nano clay modified acrylic polyurethane, mixing deionized water, a dispersant and titanium dioxide and stirring evenly to obtain a first paint; modifying dicumyl peroxide with a polymer chain to prepare a modified curing agent; modifying nano silicon dioxide, and encapsulating the modified nano silicon dioxide with polylactic acid-glycolic acid copolymer and gelatin to prepare microcapsules; mixing the curing agent and the microcapsules at a weight fraction ratio of 1:0.2, adding deionized water and titanium dioxide and stirring to obtain a second paint; mixing the first paint and the second paint at a weight fraction ratio of 1:0.5 to obtain a road marking paint. The invention improves the stability of the road marking paint in a high humidity environment.
Claims
1. A method for preparing a road marking paint for use in a high humidity environment, It is characterized in that The preparation method comprises the following steps: S100, first modifying acrylic polyurethane with nanoclay to prepare nanoclay-modified acrylic polyurethane, mixing deionized water, a dispersant and titanium dioxide and stirring evenly, grinding the mixture to a fineness of ≤50 μm, adding the nanoclay-modified acrylic polyurethane, and stirring evenly to obtain a first coating; Wherein, by weight, deionized water is 100 parts, dispersant is 2-5 parts, titanium dioxide is 10-20 parts, S200, modifying dicumyl peroxide using a polymer chain to prepare a modified curing agent; S300, modifying nano-silica using an organic silane coupling agent, and encapsulating the modified nano-silica with polylactic acid-glycolic acid copolymer and gelatin to prepare microcapsules; S400, adding deionized water and titanium dioxide to the modified curing agent and the microcapsule in a weight fraction ratio of 1:0.2 to obtain a second coating; The first coating and the second coating are mixed in a weight fraction ratio of 1:0.5 to obtain a road marking coating.
2. The method for preparing a road marking paint for a high humidity environment according to claim 1, It is characterized in that The nano-clay modified acrylic polyurethane is prepared by the following method: S110, adding 1 part of an organic silane coupling agent by weight to 99 parts of an ethanol solvent and dispersing the mixture by ultrasonic wave to prepare an organic silane coupling solvent, wherein the ultrasonic wave dispersion frequency is 80 to 90 kHz and the dispersion time is 30 to 35 min; S120, then adding 100 parts by weight of nanoclay to the organosilane coupling solvent, stirring evenly and heating to react, wherein the heating temperature is 80-90° C. and the heating time is 0.5-1 h; S130, adding 20 parts by weight of high-hydroxyl acrylic polyurethane to 80 parts of ethyl acetate, stirring until the high-hydroxyl acrylic polyurethane is completely dissolved, wherein the stirring temperature is 40-50° C., to prepare an acrylic acid solution; S140, mixing the nanoclay mixed solution and the acrylic acid solution, heating the mixture to 40° C., stirring the mixture with ultrasound for 40 to 60 minutes at an ultrasound frequency of 90 to 110 KHz, and preparing nanoclay-modified acrylic polyurethane.
3. The method for preparing a road marking paint for a high humidity environment according to claim 1, It is characterized in that The modified curing agent is prepared by the following steps: S210, mixing methyl methacrylate and 2-hydroxyethyl methacrylate in a weight ratio of 9:1; S220, under nitrogen protection, adding azobisisobutyronitrile as an initiator to the mixture, heating the mixture to 70° C., and maintaining for 2-4 hours until the methyl methacrylate and 2-hydroxyethyl methacrylate monomers are converted into polymers; S230, adding dicumyl peroxide to ethyl acetate solvent and mixing, and adding the synthesized polymer and the solvent under nitrogen protection and mixing evenly; S240, heating the mixed solvent to 45-55° C. and maintaining the temperature for 1-2 hours to promote the grafting reaction between dicumyl peroxide and the polymer chain; S250, after the reaction is completed, the mixed solution is cooled to room temperature and filtered to obtain a filter cake, and the filter cake is washed 5 times with deionized water to remove unreacted dicumyl peroxide, polymer and initiator; S260, drying the washed polymer in a vacuum drying oven to obtain a modified curing agent.
4. The method for preparing a road marking paint for a high humidity environment according to claim 1, It is characterized in that The microcapsules are prepared by the following steps: S310, modifying the nano-silicon dioxide to enhance its hydrophobicity, and then uniformly dispersing the modified nano-silicon dioxide in anhydrous ethanol by stirring to prepare a nano-silicon dioxide solution, wherein the stirring speed is 1200-1500 rpm and the time is 20-35 min; S320, dissolving the polylactic acid-glycolic acid copolymer in dichloromethane to prepare a dichloromethane mixed solution; S330, placing the dichloromethane mixed solution on a hot plate, heating the mixed solution to 45° C. and maintaining the temperature, while slowly adding the modified nano-silica solution to the mixed solution, stirring the mixed solution until the two are evenly mixed to obtain a first encapsulation solution; S340, dissolving gelatin in deionized water to prepare an aqueous solution, adding glutaraldehyde for cross-linking treatment, and stirring to obtain a second coating solution; S350, adding the first encapsulation solution dropwise into the second encapsulation solution, and stirring with a high-speed stirrer to form a double emulsion; S360, placing the double emulsion in a rotary evaporator, slowly volatilizing dichloromethane under low pressure, so that the polylactic acid-glycolic acid copolymer is solidified to form an inner shell; S370, then standing at room temperature for 6 hours to wait for the outer layer of gelatin to coagulate, and using a centrifugal method to separate and obtain microcapsules encapsulating modified nano-silica.
5. The method for preparing a road marking paint for a high humidity environment according to claim 4, It is characterized in that The modification of nano silicon dioxide comprises the following steps: S311, first pre-treating the nano-silicon dioxide, dispersing 100 parts by weight of the nano-silicon dioxide in deionized water, and using 90-110KHz ultrasonic cleaning for 30 minutes to remove surface impurities; S312, dissolving 2 to 5 parts by weight of hexadecyltrichlorosilane in 500 ml of anhydrous ethanol, and stirring to obtain a modified solution; S313, adding 100 parts by weight of dry nano-silicon dioxide to the modified solution, and dispersing it using 90-110 KHz ultrasound for 30-45 min; S314, after the nano-silica is completely dispersed in the modified solution, 5 ml of 0.1 M hydrochloric acid is added to the modified solution as a catalyst, and the mixture is reacted under stirring. The stirring reaction is continued for 12 hours to ensure that the hexadecyltrichlorosilane fully reacts with the surface of the nano-silica; S315, after the reaction is completed, the reaction mixture is filtered through filter paper to obtain a modified nano-silica filter cake, and the filter cake is washed alternately with anhydrous ethanol and deionized water for 3 times to remove unreacted hexadecyltrichlorosilane and by-products; S316. Dry the washed nano-silica in a vacuum drying oven at 60° C. for 12 hours to prepare modified nano-silica.
6. The method for preparing a road marking paint for a high humidity environment according to claim 1, It is characterized in that The nanoclay includes montmorillonite nanoclay, kaolinite nanoclay and halloysite nanoclay.
7. A road marking paint for high humidity environments, It is characterized in that Prepared according to any one of the preparation methods of claims 1 to 6.
8. A composite coating for road marking in high humidity environments. It is characterized in that The road marking paint prepared by any one of the preparation methods of claims 1 to 6 is sprayed sequentially on a cement or asphalt pavement with an acrylic polyurethane primer layer and a dicumyl peroxide topcoat layer.
9. The composite coating for road marking in high humidity environment according to claim 8, It is characterized in that The dicumyl peroxide topcoat layer contains microcapsules. When the ambient humidity is greater than 95%, the microcapsules rupture to release the wrapped modified nano-silicon dioxide slurry.
10. The composite coating for road marking in high humidity environment according to claim 8, It is characterized in that The thickness of the dicumyl peroxide topcoat layer is 0.5-1 mm; the thickness of the acrylic polyurethane primer layer is 0.7-1.7 mm.
Citation Information
Patent Citations
Absorbable magnesium alloy stent of anticorrosion and drug release composite coating and preparation method thereof
CN101721266A
Orange reflective traffic marking coating as well as preparation method and application thereof
CN113265183A
Environment-friendly high-solid-content waterborne polyurethane acrylate composite emulsion as well as preparation method and application thereof
CN114045107A
A method for manufacturing a concrete block in which cement mortar is sprayed on a surface
KR1020210022208A