Micro-network heat conduction enhanced nano-carbon-based molten salt composite material as well as preparation method and application thereof

By generating nanocarbon micronetwork structures in situ in phase change materials, the problems of low thermal conductivity and nanocarbon aggregation of phase change materials are solved, and efficient heat transfer and heat storage performance are achieved.

CN118978893APending Publication Date: 2024-11-19NANJING JINHE ENERGY MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411040896.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The thermal conductivity of existing phase change heat storage materials is low, which is difficult to meet the needs of efficient heat storage and release in practical applications. Moreover, the high surface energy of nano-carbon-based materials leads to uneven aggregation and dispersion, affecting thermal conductivity.

Method used

By in situ generating nanocarbon micronetwork structures in molten salt phase change materials, using expanded graphite as a carbon precursor, in situ peeling method is used to form nanocarbon sheets, and combining silicon carbide nanowires to form nanosheet-wire interwoven structures to increase heat Bridge effect to avoid uneven material aggregation and dispersion.

Benefits of technology

It significantly improves the thermal conductivity of composite materials, realizes rapid charging and exothermic of heat storage materials, and promotes the construction and application of high-efficiency heat storage systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978893A_ABST
    Figure CN118978893A_ABST
Patent Text Reader

Abstract

The invention discloses a micro-network heat conduction enhanced nano-carbon-based fused salt composite material and a preparation method and application thereof, the fused salt composite material comprises a fused salt phase change material, a nano-carbon micro-network structure is distributed in the fused salt phase change material, and the nano-carbon micro-network structure comprises a nano-carbon sheet layer. The preparation method comprises the following steps: carrying out heat treatment on a mixture containing the fused salt phase change material and expanded graphite, so that the expanded graphite is stripped in situ to form the nano carbon sheet layer. The micro-network nano-carbon-based molten salt composite heat storage material with the xylem-imitating structure is prepared in one step by taking expanded graphite as a carbon precursor and silicon carbide nanowires as a microstructure modifier through an in-situ exfoliation method and utilizing the inherent advantage of ion exfoliation of a molten salt phase-change material by adopting the in-situ exfoliation method. The heat storage material has high heat storage capacity and good heat conductivity, and can quickly store a large amount of heat.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of phase change heat storage materials, and in particular to a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material and a preparation method and application thereof. Background Art

[0002] The phase change heat storage system is used in solar thermal power generation, building energy conservation, waste heat recovery and other fields due to its advantages of efficient energy storage, stable temperature, small footprint and flexible heat release. By efficiently storing and releasing heat energy, it achieves optimal management and utilization of energy and improves energy efficiency and system stability.

[0003] However, due to the low thermal conductivity of the phase change material itself, it is difficult to meet the needs of efficient heat storage and release in practical applications, so the thermal conductivity of the device itself is improved by adding thermal conductivity enhancers. Nanocarbon-based materials are widely used as thermal conductivity enhancers due to their light weight, high thermal conductivity and chemical stability, and are often used to improve the thermal conductivity of phase change materials. However, the high surface energy of nanocarbon-based materials can easily lead to their aggregation, increase the thermal resistance of the composite material interface, and thus reduce the thermal conductivity.

[0004] To solve this problem, the interaction between nanocarbons is often adjusted through surface modification and functional group grafting to reduce aggregation. However, the traditional preparation method still cannot avoid the problem of non-uniform dispersion of high-content nanocarbon-based materials. At the same time, surface treatment inevitably introduces defects, increases phonon scattering, and affects its thermal conductivity. Therefore, it is urgent to optimize the structural design and preparation process of thermally conductive enhanced phase change composite materials to further improve thermal conductivity.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material and a preparation method and application thereof, so as to improve the above-mentioned technical problems.

[0007] The present invention is achieved in that:

[0008] In a first aspect, the present invention provides a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which includes a molten salt phase change material, wherein a nano-carbon micro-network structure is distributed inside the molten salt phase change material, and the nano-carbon micro-network structure includes nano-carbon sheets.

[0009] Optionally, the above-mentioned nanocarbon micronetwork structure also includes silicon carbide nanowires (SiCnw), and the nanocarbon micronetwork structure is a nanosheet-wire interwoven structure. Preferably, the mass ratio of the nanocarbon sheet layer to the silicon carbide nanowire is (12-1):1, and more preferably (8-2):1.

[0010] Optionally, the mass percentage of the nano-carbon network structure in the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material is 0.5% to 6%, preferably 1% to 4%.

[0011] Optionally, the molten salt phase change material is a multi-component molten salt, preferably a ternary eutectic molten salt, and more preferably, the ternary eutectic molten salt is composed of a lithium-based fluoride salt, a chloride salt and a nitrate salt.

[0012] In a second aspect, the present invention also provides a method for preparing the above-mentioned micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which comprises: heat-treating a mixture containing a molten salt phase change material and expanded graphite so that the expanded graphite is in situ exfoliated to form the nano-carbon sheet layer.

[0013] Optionally, the heat treatment is to raise the temperature to 320° C. to 400° C. and keep the temperature for 1 hour to 4 hours.

[0014] Optionally, the heating rate is 4°C / min to 6°C / min.

[0015] Optionally, the mixture containing molten salt phase change material and expanded graphite is obtained by the following steps: placing the molten salt phase change material and expanded graphite in a ball mill for ball milling; when containing silicon carbide nanowires, placing the molten salt phase change material, expanded graphite and silicon carbide nanowires in a ball mill for ball milling.

[0016] Optionally, the molten salt phase change material is dried prior to ball milling.

[0017] Optionally, the expanded graphite is obtained by rapidly heating flake graphite from room temperature in a muffle furnace and then cooling it down.

[0018] Optionally, the mass content of the expanded graphite in the mixture is 0.5% to 6%, preferably 1% to 4%; when the mixture also contains silicon carbide nanowires, the total mass of the expanded graphite and the silicon carbide nanowires in the mixture is 0.5% to 6%, preferably 1% to 4%, and the mass ratio of the expanded graphite to the silicon carbide nanowires is (12 to 1):1, preferably (8 to 2):1.

[0019] Optionally, before the above heat treatment, an inert gas is introduced at room temperature to remove impurity atmosphere.

[0020] In a third aspect, the present invention also provides the application of the above-mentioned micro-network thermal conductivity enhanced nano-carbon-based molten salt composite material in solar water heaters, solar thermal power generation systems, building exterior walls, waste heat recovery systems, electronic equipment cooling systems or cold chain transportation devices.

[0021] The present invention has the following beneficial effects: by using expanded graphite as a carbon precursor, adopting an in-situ exfoliation method, and utilizing the mild melting reaction conditions of molten salt, a nano-carbon micro-network structure is generated in-situ inside the molten salt phase change material, thereby avoiding the problem of material aggregation and uneven dispersion caused by directly adding nano-carbon-based materials. Nano-carbon is distributed in the molten salt phase change material in the form of a nano-carbon micro-network structure containing nano-sheet layers, which can effectively form a thermal bridge, increase the heat transfer rate in the system, and thus improve the thermal conductivity of the composite phase change material. Furthermore, the construction of the nano-carbon micro-network structure improves the current problem of large defects in nano-carbon-based materials and the inability to be evenly dispersed in the phase change material, which is conducive to realizing the rapid charging and discharging of heat storage materials, thereby promoting the construction and application of high-efficiency heat storage systems. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0023] Figure 1 is a SEM image of the nanocarbon micronetwork sample of Example 1 of the present invention;

[0024] Figure 2 is a SEM image of the nanocarbon micronetwork sample of Example 2 of the present invention;

[0025] Figure 3 is a SEM image of the nanocarbon micronetwork sample of Example 3 of the present invention;

[0026] Figure 4 is a SEM image of the nanocarbon micronetwork sample of Example 4 of the present invention;

[0027] Figure 5 is a SEM image of the nanocarbon micronetwork sample of Example 5 of the present invention;

[0028] Figure 6 is a SEM image of the nanocarbon micronetwork sample of Example 6 of the present invention;

[0029] Figure 7 is a SEM image of the nanocarbon micronetwork sample of Example 7 of the present invention;

[0030] Figure 8 is a SEM image of the nanocarbon micronetwork sample of Example 8 of the present invention;

[0031] Fig. 9 is a SEM image of the nanocarbon micronetwork sample of Example 9 of the present invention;

[0032] Fig.10 is a SEM image of the nanocarbon micronetwork sample of Example 10 of the present invention;

[0033] Fig.11 It is a comparison diagram of thermal conductivity of molten salt and micro-network thermally conductive enhanced nano-carbon-based molten salt composite materials of Examples 1 to 10 of the present invention;

[0034] Fig.12 DSC curve diagram of the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material according to Example 1 of the present invention;

[0035] Fig.13 DSC curve diagram of the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material according to Example 2 of the present invention;

[0036] Fig.14 DSC curve diagram of the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material of Example 3 of the present invention;

[0037] Fig.15 DSC curve diagram of the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material of Example 4 of the present invention;

[0038] Fig.16 DSC curve diagram of the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material of Example 5 of the present invention;

[0039] Fig.17 DSC curve diagram of the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material of Example 6 of the present invention;

[0040] Fig.18 DSC curve diagram of the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material of Example 7 of the present invention;

[0041] Fig.19 DSC curve diagram of the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material of Example 8 of the present invention;

[0042] Fig. 20 DSC curve diagram of the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material of Example 9 of the present invention;

[0043] Fig.21 DSC curve of the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material of Example 10 of the present invention. DETAILED DESCRIPTION

[0044] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0045] The following is a detailed description of a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material provided by the present invention, as well as its preparation method and application.

[0046] Some embodiments of the present invention provide a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which includes a molten salt phase change material, wherein a nano-carbon micro-network structure is distributed inside the molten salt phase change material, and the nano-carbon micro-network structure includes nano-carbon sheets.

[0047] Nanocarbon is distributed in the molten salt phase change material in the form of a nanocarbon micro-network structure containing nanosheet layers. Compared with the traditional situation where nanocarbon-based materials cannot be evenly dispersed and cannot form a network structure after being mixed and dispersed with the phase change material, nanocarbon in a micro-network structure can effectively form a thermal bridge, increase the heat transfer rate in the system, and thus improve the thermal conductivity of the composite phase change material, which is conducive to the rapid charging and discharging of heat storage materials, thereby promoting the construction and application of high-efficiency heat storage systems. It should be noted that the nanocarbon micro-network structure is basically evenly dispersed in the molten salt phase change material, and the nanocarbon sheet layer is the main skeleton structure of the nano-micro-network structure, that is, the nano-micro-network structure is mainly composed of multiple nanocarbon sheets interwoven to form the skeleton of the micro-network structure.

[0048] In some embodiments, in order not to affect the phase change properties of the phase change material and to achieve better thermal conductivity, the mass percentage of the nanocarbon network structure in the micronetwork thermally conductive enhanced nanocarbon-based molten salt composite material is 0.5% to 6%. Exemplarily, it can be selected as 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5% or 6%, etc., or between any two of the above mass percentages. In a preferred embodiment, the mass percentage of the nanocarbon network structure in the micronetwork thermally conductive enhanced nanocarbon-based molten salt composite material is 1% to 4%.

[0049] In order to make the nanocarbon micronetwork structure more stable and the heat transfer efficiency faster, in some embodiments, the nanocarbon micronetwork structure also includes silicon carbide nanowires (SiCnw), and the uniformly distributed nanosheet layers are cross-modified by silicon carbide nanowires to make the nanocarbon micronetwork structure become a nanosheet-wire interwoven structure, that is, silicon carbide nanowires are interspersed in the micronetwork skeleton structure composed of nanocarbon sheets.

[0050] For reference, in order to ensure better interwoven heat transfer effect, the mass ratio of nano-carbon sheets to silicon carbide nanowires is (12-1):1. Exemplarily, the mass ratio can be selected as 12:1, 11:1, 10:1, 9:1, 8:1, 7:1, 6:1, 5:1, 4:1, 3:1, 2:1 or 1:1, etc., or between any two of the above ratios. In a preferred embodiment, the mass ratio of nano-carbon sheets to silicon carbide nanowires is (8-2):1.

[0051] Furthermore, some embodiments of the present invention also provide a method for preparing the above-mentioned micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which comprises: heat-treating a mixture containing a molten salt phase change material and expanded graphite so that the expanded graphite is exfoliated in situ to form the nano-carbon sheet layer.

[0052] By using expanded graphite as a carbon precursor, adopting an in-situ exfoliation method, and utilizing the mild melting reaction conditions of molten salt, a nano-carbon micro-network structure is generated in-situ inside the molten salt phase change material, thereby avoiding the problems of material aggregation and uneven dispersion caused by directly adding nano-carbon-based materials. It should be noted that the temperature can be better controlled by molten salt, and the molten salt can facilitate the exfoliation of graphite to form nano-sheets, thereby reducing the surface defects of the nano-sheets to achieve better heat conduction effects.

[0053] Specifically, in some embodiments of the present invention, the molten salt phase change material includes but is not limited to a multi-component molten salt. Exemplarily, the molten salt phase change material is a ternary eutectic molten salt. As a reference, the ternary eutectic molten salt is composed of a lithium-based fluoride salt, a chloride salt and a nitrate. The selection of the ternary eutectic molten salt is conducive to further improving the heat storage density of the phase change material. It should be noted that this phase change heat storage material can also be replaced with other compatible heat storage materials.

[0054] For reference, the preparation method of the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material provided in some embodiments of the present invention specifically includes the following steps:

[0055] S1. Remove moisture from the molten salt phase change material.

[0056] Specifically, the molten salt phase change material is dried, for example, the molten salt phase change material is placed in an oven at 120±20° C. and dried for more than 12 hours.

[0057] S2. Preparation of expanded graphite (EG).

[0058] Specifically, in some embodiments, the graphite flakes are rapidly heated from room temperature in a muffle furnace and then cooled, for example, rapidly heated to 750° C. to 850° C. and then cooled.

[0059] It should be noted that the order of step S1 and step S2 is not limited and can be swapped.

[0060] S3. Mix the molten salt phase change material and expanded graphite (EG) evenly.

[0061] Specifically, in some embodiments, the dried molten salt phase change material is ground and mixed with a certain amount of EG, and then placed in a ball mill for a period of time. If silicon carbide nanowires are contained, the two materials are ball milled together with the molten salt. For example, the ball milling speed can be selected to be 250-350 r / min, and the ball milling time is at least 2 hours.

[0062] S4. heat-treating the mixture containing the molten salt phase change material and the expanded graphite.

[0063] Specifically, in some embodiments, before the heat treatment, an inert gas (eg, nitrogen) is introduced at room temperature to remove impurity atmosphere.

[0064] For reference, the heat treatment is to raise the temperature to 320°C to 400°C. Exemplarily, it can be selected as 320°C, 330°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C or 400°C, or between any two of the above temperatures, and keep warm for 1 hour to 4 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours, etc.

[0065] In some embodiments, the heating rate can be selected to be 4°C / min to 6°C / min, such as 4°C / min, 5°C / min, 6°C / min, etc.

[0066] In the process of in-situ exfoliation to form nanocarbon sheets, the amount of expanded graphite has a relatively important influence on the morphology of the nanocarbon micronetwork structure. If the amount is too low, the nanocarbon obtained by exfoliation will be in the form of broken flakes, and the nanocarbon obtained by exfoliation will be unable to carry excessive molten salt ions, and the nanocarbon sheet structure will collapse and fragment; if the amount is too much, the expanded graphite is prone to incomplete exfoliation. Therefore, in some embodiments, the mass content of the expanded graphite in the mixture is 0.5% to 6%, which can be selected as 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5% or 6%, or between any two of the above mass percentages, preferably 1% to 4%.

[0067] If the mixture also contains silicon carbide nanowires, the total mass of the expanded graphite and the silicon carbide nanowires in the mixture is 0.5% to 6%, preferably 1% to 4%, and the mass ratio of the expanded graphite to the silicon carbide nanowires is (12 to 1):1. The mass ratio can be selected as 12:1, 11:1, 10:1, 9:1, 8:1, 7:1, 6:1, 5:1, 4:1, 3:1, 2:1 or 1:1, etc., or between any two of the above ratios, preferably (8 to 2):1.

[0068] Some embodiments of the present invention also provide applications of the above-mentioned micro-network thermally conductive enhanced nano-carbon-based molten salt composite material in solar water heaters, solar thermal power generation systems, building exterior walls, waste heat recovery systems, electronic equipment cooling systems or cold chain transportation devices.

[0069] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0070] Example 1

[0071] The embodiment of the present invention provides a method for preparing a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which comprises the following steps:

[0072] The ternary molten salt phase change material LiF-LiCl-LiNO3 (the mass ratio of LiF, LiCl and LiNO3 is 2:8:90) is placed in a 120℃ oven for more than 12h to ensure that the moisture is completely removed. Then, the flake graphite is placed in a muffle furnace and heated from room temperature to 800℃ at a heating rate of 10℃ / min, and then cooled rapidly to obtain expanded graphite (EG). The dried LiF-LiCl-LiNO3 is ground and mixed with EG, and the mass content of EG is 0.5%. It is then placed in a ball mill at a speed of 300r / min for 2h, and then the sample is placed in a nitrogen-protected tubular furnace. First, ventilate at room temperature for 1h to thoroughly remove the impurity atmosphere remaining in the furnace. Then, under the condition of a nitrogen flow rate of 50mL / min, the tubular furnace is heated at a heating rate of 5℃ / min, and the temperature is raised to 360℃ and maintained for 180min. Finally, the sample is naturally cooled to room temperature and taken out to obtain a nano-carbon molten salt phase change composite material.

[0073] One portion was washed with deionized water to remove the molten salt on the surface and inside of the original EG, and the corresponding nanocarbon sample was obtained after drying. Figure 1 This is the SEM image of nanocarbon obtained when the EG mass content is 0.5%. Figure 1 As shown, the nanocarbon prepared under this condition is in the form of broken flakes, indicating that the EG content is low at this time, and the nanocarbon obtained by exfoliation cannot carry excessive molten salt ions, and the nanocarbon sheet structure collapses and fragments. Fig.11is the thermal conductivity diagram of the corresponding nano-carbon molten salt phase change composite material. Fig.11 As shown, under this condition, the thermal conductivity of the composite material is 2.16 W / (m·K), which is 122.47% higher than the thermal conductivity of pure LiF-LiCl-LiNO3 (0.97 W / (m·K)). Figure 8 is the DSC curve of the corresponding nano-carbon molten salt phase change composite material. Fig.12 As shown, under this condition, the phase change temperature of the composite material is 232.24℃, and the phase change latent heat is 361.23J / g, which is significantly different from the phase change temperature of pure LiF-LiCl-LiNO3, indicating that the introduction of nanocarbon improves the thermal conductivity of the composite material system, resulting in a phase change of the molten salt at a lower temperature, and the phase change latent heat changes little, indicating that the addition of 0.5% EG by mass fraction has little effect on the phase change latent heat of the composite material.

[0074] Example 2

[0075] The embodiment of the present invention provides a method for preparing a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which comprises the following steps:

[0076] The ternary molten salt phase change material LiF-LiCl-LiNO3 (the mass ratio of LiF, LiCl and LiNO3 is 2:8:90) is placed in a 120℃ oven for drying for more than 12h to ensure that the moisture is completely removed. Then, the flake graphite is placed in a muffle furnace and heated from room temperature to 800℃ at a heating rate of 10℃ / min, and then cooled rapidly to obtain expanded graphite (EG). The dried LiF-LiCl-LiNO3 is ground and mixed with EG, and the mass content of EG is 1%. It is then placed in a ball mill at a speed of 300r / min for 2h, and then the sample is placed in a nitrogen-protected tubular furnace. First, ventilate at room temperature for 1h to thoroughly remove the impurity atmosphere remaining in the furnace. Then, under the condition of a nitrogen flow rate of 50mL / min, the tubular furnace is heated at a heating rate of 5℃ / min, and the temperature is raised to 360℃ and maintained for 180min. Finally, the sample is naturally cooled to room temperature and taken out to obtain a nanocarbon molten salt phase change composite material.

[0077] One portion was washed with deionized water to remove the molten salt on the surface and inside of the original EG, and the corresponding nanocarbon sample was obtained after drying. Figure 2 This is the SEM image of nanocarbon obtained when the EG mass content is 1%. Figure 2 As shown, the nanocarbon prepared under this condition is in the form of incomplete flakes, indicating that the higher content of molten salt ions at this time caused excessive exfoliation of the nanocarbon, resulting in the destruction of the complete lamellar structure of the nanocarbon. Fig.11 is the thermal conductivity diagram of the corresponding nano-carbon molten salt phase change composite material. Fig.11As shown, under this condition, the thermal conductivity of the composite material is 2.57 W / (m·K), which is 165.05% higher than the thermal conductivity of pure LiF-LiCl-LiNO3 (0.97 W / (m·K)). Fig.13 is the DSC curve of the corresponding nano-carbon molten salt phase change composite material. Fig.13 As shown, the phase change temperature of the composite material is 237.33℃, and the phase change latent heat is 357.21J / g, which is significantly different from the phase change temperature of pure LiF-LiCl-LiNO3, indicating that the introduction of nanocarbon improves the thermal conductivity of the composite system, resulting in a phase change of the molten salt at a lower temperature, and the phase change latent heat changes less, indicating that the addition of 1% by mass EG has little effect on the phase change latent heat of the composite material.

[0078] Example 3

[0079] The embodiment of the present invention provides a method for preparing a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which comprises the following steps:

[0080] The ternary molten salt phase change material LiF-LiCl-LiNO3 (the mass ratio of LiF, LiCl and LiNO3 is 2:8:90) is placed in a 120℃ oven for more than 12h to ensure that the moisture is completely removed. Then, the flake graphite is placed in a muffle furnace and heated from room temperature to 800℃ at a heating rate of 10℃ / min, and then cooled rapidly to obtain expanded graphite (EG). The dried LiF-LiCl-LiNO3 is ground and mixed with EG, and the mass content of EG is 2%. It is then placed in a ball mill at a speed of 300r / min for 2h, and then the sample is placed in a nitrogen-protected tubular furnace. First, ventilate at room temperature for 1h to thoroughly remove the impurity atmosphere remaining in the furnace. Then, under the condition of a nitrogen flow rate of 50mL / min, the tubular furnace is heated at a heating rate of 5℃ / min, and the temperature is raised to 360℃ and maintained for 180min. Finally, the sample is naturally cooled to room temperature and taken out to obtain a nanocarbon molten salt phase change composite material.

[0081] One portion was washed with deionized water to remove the molten salt on the surface and inside of the original EG, and the corresponding nanocarbon sample was obtained after drying. Figure 3 This is the SEM image of nanocarbon obtained when the EG mass content is 2%. Figure 3 As shown, the nanocarbon prepared under this condition exhibits a relatively complete flake structure, indicating that the EG content is moderate at this time. Fig.11 is the thermal conductivity diagram of the corresponding nano-carbon molten salt phase change composite material. Fig.11As shown in the figure, under this condition, the thermal conductivity of the composite material is 3.12 W / (m·K), which is 221.65% higher than that of pure LiF-LiCl-LiNO3 (0.97 W / (m·K)). The improvement effect is significant, indicating that the introduction of nanocarbon effectively improves the thermal conductivity of the composite material. Fig.14 is the DSC curve of the corresponding nano-carbon molten salt phase change composite material. Fig.14 As shown in the figure, under this condition, the phase change temperature of the composite material is 231.46℃, and the phase change latent heat is 351.46J / g, which is significantly different from the phase change temperature and phase change latent heat of pure LiF-LiCl-LiNO3, indicating that the introduction of nanocarbon improves the thermal conductivity of the composite system, thereby causing the molten salt to undergo phase change at a lower temperature. Since EG itself does not have a phase change function, the introduction of nanocarbon causes the content of the molten salt component in the composite system to decrease, thereby weakening the phase change latent heat of the composite material.

[0082] Example 4

[0083] The embodiment of the present invention provides a method for preparing a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which comprises the following steps:

[0084] The ternary molten salt phase change material LiF-LiCl-LiNO3 (the mass ratio of LiF, LiCl and LiNO3 is 2:8:90) is placed in a 120℃ oven for more than 12h to ensure that the moisture is completely removed. Then, the flake graphite is placed in a muffle furnace and heated from room temperature to 800℃ at a heating rate of 10℃ / min, and then cooled rapidly to obtain expanded graphite (EG). The dried LiF-LiCl-LiNO3 is ground and mixed with EG, and the mass content of EG is 4%. It is then placed in a ball mill at a speed of 300r / min for 2h, and then the sample is placed in a nitrogen-protected tubular furnace. First, ventilate at room temperature for 1h to thoroughly remove the impurity atmosphere remaining in the furnace. Then, under the condition of a nitrogen flow rate of 50mL / min, the tubular furnace is heated at a heating rate of 5℃ / min, and the temperature is raised to 360℃ and maintained for 180min. Finally, the sample is naturally cooled to room temperature and taken out to obtain a nanocarbon molten salt phase change composite material.

[0085] One portion was washed with deionized water to remove the molten salt on the surface and inside of the original EG, and the corresponding nanocarbon sample was obtained after drying. Figure 4 This is the SEM image of nanocarbon obtained when the EG mass content is 4%. Figure 4 As shown, the nanocarbon prepared under this condition presents a relatively complete flaky structure with a certain thickness, indicating that the degree of EG exfoliation is low at this time. This is related to the fact that when the EG content is high, the molten salt ions cannot provide sufficient ion exfoliation to overcome the van der Waals force between the EG flakes, resulting in most of the carbon material existing in the form of thick EG flakes. Fig.11 is the thermal conductivity diagram of the corresponding nano-carbon molten salt phase change composite material. Fig.11 As shown, under this condition, the thermal conductivity of the composite material is 3.06 W / (m·K), which is 215.46% higher than the thermal conductivity of pure LiF-LiCl-LiNO3 (0.97 W / (m·K)). Fig.15 is the DSC curve of the corresponding nano-carbon molten salt phase change composite material. Fig.15 As shown in the graph, the phase change temperature of the composite material is 231.56℃, and the phase change latent heat is 347.42J / g, which are significantly different from the phase change temperature and phase change latent heat of pure LiF-LiCl-LiNO3, indicating that the introduction of nanocarbon improves the thermal conductivity of the composite system, thereby causing the molten salt to undergo a phase change at a lower temperature. Since EG itself does not have a phase change function, the introduction of nanocarbon causes the content of the molten salt component in the composite system to decrease, thereby weakening the phase change latent heat of the composite material.

[0086] Example 5

[0087] The embodiment of the present invention provides a method for preparing a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which comprises the following steps:

[0088] The ternary molten salt phase change material LiF-LiCl-LiNO3 (the mass ratio of LiF, LiCl and LiNO3 is 2:8:90) is placed in a 120℃ oven for more than 12h to ensure that the moisture is completely removed. Then, the flake graphite is placed in a muffle furnace and heated from room temperature to 800℃ at a heating rate of 10℃ / min, and then cooled rapidly to obtain expanded graphite (EG). The dried LiF-LiCl-LiNO3 is ground and mixed with EG, and the mass content of EG is 6%. It is then placed in a ball mill at a speed of 300r / min for 2h, and then the sample is placed in a nitrogen-protected tubular furnace. First, ventilate at room temperature for 1h to thoroughly remove the impurity atmosphere remaining in the furnace. Then, under the condition of a nitrogen flow rate of 50mL / min, the tubular furnace is heated at a heating rate of 5℃ / min, and the temperature is raised to 360℃ and maintained for 180min. Finally, the sample is naturally cooled to room temperature and taken out to obtain a nanocarbon molten salt phase change composite material.

[0089] One portion was washed with deionized water to remove the molten salt on the surface and inside of the original EG, and the corresponding nanocarbon sample was obtained after drying. Figure 5 This is the SEM image of nanocarbon obtained when the EG mass content is 6%. Figure 5As shown in the figure, the nanocarbon prepared under this condition presents a complete but thick sheet structure, indicating that the EG exfoliation is incomplete at this time. This may be because when the EG content is high, the fewer molten salt ions cannot fully overcome the van der Waals force between the EG sheets, the activation and exfoliation of EG are incomplete, and the carbon material still exists in the form of thick EG sheets. Fig.11 is the thermal conductivity diagram of the corresponding nano-carbon molten salt phase change composite material. Fig.11 As shown, under this condition, the thermal conductivity of the composite material is 2.52 W / (m·K), which is 159.79% higher than the thermal conductivity of pure LiF-LiCl-LiNO3 (0.97 W / (m·K)). Fig.16 is the DSC curve of the corresponding nano-carbon molten salt phase change composite material. Fig.16 As shown in the figure, under this condition, the phase change temperature of the composite material is 230.97℃, and the phase change latent heat is 338.21J / g, which is significantly different from the phase change temperature and phase change latent heat of pure LiF-LiCl-LiNO3, indicating that the introduction of nanocarbon improves the thermal conductivity of the composite system, thereby causing the molten salt to undergo phase change at a lower temperature. Since EG itself does not have a phase change function, the introduction of nanocarbon causes the content of the molten salt component in the composite system to decrease, thereby weakening the phase change latent heat of the composite material.

[0090] Example 6

[0091] The embodiment of the present invention provides a method for preparing a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which comprises the following steps:

[0092] The ternary molten salt phase change material LiF-LiCl-LiNO3 (the mass ratio of LiF, LiCl and LiNO3 is 2:8:90) was placed in a 120℃ oven for more than 12h to ensure that the moisture was completely removed. Then, the flake graphite was placed in a muffle furnace and heated from room temperature to 800℃ at a heating rate of 10℃ / min and then cooled rapidly to obtain expanded graphite (EG). The dried LiF-LiCl-LiNO3 was ground and mixed with EG-SiCnw, the mass content of EG-SiCnw was 2%, and the mass ratio of EG to SiCnw was 12:1. It was then placed in a ball mill at a speed of 300r / min for 2h, and then the sample was placed in a nitrogen-protected tubular furnace. First, ventilate at room temperature for 1h to thoroughly remove the impurity atmosphere remaining in the furnace. Then, under the condition of a nitrogen flow rate of 50mL / min, the tubular furnace was heated at a heating rate of 5℃ / min, and the temperature was raised to 360℃ and maintained for 180min. Finally, the sample was taken out after naturally cooling to room temperature to obtain a nano-carbon substrate-wire interwoven micro-network structure thermally conductive enhanced molten salt phase change composite material.

[0093] One of the samples was washed with deionized water to remove the molten salt on the surface and inside of EG and SiCnw, and then dried to obtain the corresponding nanocarbon micronetwork sample. Figure 6 This is the SEM image of the nanocarbon micronetwork obtained when the mass ratio of EG to SiCnw is 12:1. Figure 6 As shown, under this condition, SiCnw is only scattered between the nanocarbon sheets, indicating that the SiCnw content is low under this condition and an effective network cannot be formed. Fig.11 is the thermal conductivity diagram of the corresponding micro-network nano-carbon-based molten salt phase change composite material. Fig.11 As shown in the figure, under this condition, the thermal conductivity of the composite material is 2.86W / (m·K), and the thermal conductivity of the composite material is lower than that of the nanocarbon molten salt phase change composite material. This is because the introduction of low thermal conductivity SiCnw has a certain negative impact on the thermal conductivity of the micro-network nanocarbon-based molten salt composite system. In addition, the low content of SiCnw is scattered in the nanocarbon and exists in the form of "islands", which cannot achieve continuous heat transfer. Fig.17 is the DSC curve of the corresponding micro-network nano-carbon-based molten salt phase change composite material. Fig.17 As shown, under this condition, the phase change latent heat of the composite material is 341.98 J / g, which is not much different from that of the composite material with an EG content of 2%, indicating that the introduction of SiCnw does not change the heat storage properties of the composite material, and there is good chemical compatibility between molten salt, nanocarbon and SiCnw.

[0094] Example 7

[0095] The embodiment of the present invention provides a method for preparing a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which comprises the following steps:

[0096] The ternary molten salt phase change material LiF-LiCl-LiNO3 (the mass ratio of LiF, LiCl and LiNO3 is 2:8:90) was placed in a 120℃ oven for more than 12h to ensure that the moisture was completely removed. Then, the flake graphite was placed in a muffle furnace and heated from room temperature to 800℃ at a heating rate of 10℃ / min, and then cooled rapidly to obtain expanded graphite (EG). The dried LiF-LiCl-LiNO3 was ground and mixed with EG-SiCnw, the mass content of EG-SiCnw was 2%, and the mass ratio of EG to SiCnw was 8:1. It was then placed in a ball mill at a speed of 300r / min for 2h, and then the sample was placed in a nitrogen-protected tubular furnace. First, ventilate at room temperature for 1h to thoroughly remove the impurity atmosphere remaining in the furnace. Then, under the condition of a nitrogen flow rate of 50mL / min, the tubular furnace was heated at a heating rate of 5℃ / min, and the temperature was raised to 360℃ and maintained for 180min. Finally, the sample was taken out after naturally cooling to room temperature to obtain a nano-carbon substrate-wire interwoven micro-network structure thermally conductive enhanced molten salt phase change composite material.

[0097] One of the samples was washed with deionized water to remove the molten salt on the surface and inside of EG and SiCnw, and then dried to obtain the corresponding nanocarbon micronetwork sample. Figure 7 This is the SEM image of the nanocarbon micronetwork obtained when the mass ratio of EG to SiCnw is 8:1. Figure 7 As shown, under this condition, a small amount of SiCnw is dispersed between the nanocarbon sheets to form a network with a certain degree of cross-linking. Fig.11 is the thermal conductivity diagram of the corresponding micro-network nano-carbon-based molten salt phase change composite material. Fig.11 As shown in the figure, under this condition, the thermal conductivity of the composite material is 3.19W / (m·K), and the thermal conductivity of the composite material is slightly lower than that of the nanocarbon molten salt phase change composite material. Although the introduction of low thermal conductivity SiCnw has a certain negative impact on the thermal conductivity of the micro-network nanocarbon-based molten salt composite system, a certain amount of SiCnw is distributed in the nanocarbon to form an incomplete cross-linked network, which promotes the rapid transfer of heat to a certain extent. Fig.18 is the DSC curve of the corresponding micro-network nano-carbon-based molten salt phase change composite material. Fig.18 As shown, under this condition, the phase change latent heat of the composite material is 346.37 J / g, which is not much different from that of the composite material with an EG content of 2%, indicating that the introduction of SiCnw does not change the heat storage properties of the composite material, and there is good chemical compatibility between molten salt, nanocarbon and SiCnw.

[0098] Example 8

[0099] The embodiment of the present invention provides a method for preparing a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which comprises the following steps:

[0100] The ternary molten salt phase change material LiF-LiCl-LiNO3 (the mass ratio of LiF, LiCl and LiNO3 is 2:8:90) was placed in a 120℃ oven for more than 12h to ensure that the moisture was completely removed. Then, the flake graphite was placed in a muffle furnace and heated from room temperature to 800℃ at a heating rate of 10℃ / min and then cooled rapidly to obtain expanded graphite (EG). The dried LiF-LiCl-LiNO3 was ground and mixed with EG-SiCnw, the mass content of EG-SiCnw was 2%, and the mass ratio of EG to SiCnw was 4:1. It was then placed in a ball mill at a speed of 300r / min for 2h, and then the sample was placed in a nitrogen-protected tubular furnace. First, ventilate at room temperature for 1h to thoroughly remove the impurity atmosphere remaining in the furnace. Then, under the condition of a nitrogen flow rate of 50mL / min, the tubular furnace was heated at a heating rate of 5℃ / min, and the temperature was raised to 360℃ and maintained for 180min. Finally, the sample was taken out after naturally cooling to room temperature to obtain a nano-carbon substrate-wire interwoven micro-network structure thermally conductive enhanced molten salt phase change composite material.

[0101] One of the samples was washed with deionized water to remove the molten salt on the surface and inside of EG and SiCnw, and then dried to obtain the corresponding nanocarbon micronetwork sample. Figure 8 This is the SEM image of the nanocarbon micronetwork obtained when the mass ratio of EG to SiCnw is 4:1. Figure 8 As shown, under this condition, SiCnw is only scattered between the nano-carbon sheets, indicating that under this condition, SiCnw is widely and evenly distributed between the nano-carbon sheets, forming a relatively dense network structure, indicating that the SiCnw content is moderate at this time, and the micro-network thermal conductive structure is successfully constructed, effectively forming a heat transfer path. Fig.11 is the thermal conductivity diagram of the corresponding nanocarbon micronetwork molten salt phase change composite material. Fig.11 As shown in the figure, under this condition, the thermal conductivity of the composite material is 3.51W / (m·K), which is significantly higher than that of the nanocarbon molten salt phase change composite material. This is because the appropriate amount of SiCnw is evenly distributed in the nanocarbon, forming a complete xylem-like micro-network structure, which is conducive to the rapid transmission of heat, thereby significantly improving the thermal conductivity of the composite material system. Fig.19 is the DSC curve of the corresponding nano-carbon molten salt phase change composite material. Fig.19 As shown in the figure, under this condition, the phase change latent heat of the composite material is 348.37 J / g, which is not much different from that of the composite material with an EG content of 2%, indicating that the introduction of SiCnw does not change the heat storage properties of the composite material, and there is good chemical compatibility between molten salt, nanocarbon and SiCnw.

[0102] Example 9

[0103] The embodiment of the present invention provides a method for preparing a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which comprises the following steps:

[0104] The ternary molten salt phase change material LiF-LiCl-LiNO3 (the mass ratio of LiF, LiCl and LiNO3 is 2:8:90) was placed in a 120℃ oven for more than 12h to ensure that the moisture was completely removed. Then, the flake graphite was placed in a muffle furnace and heated from room temperature to 800℃ at a heating rate of 10℃ / min, and then cooled rapidly to obtain expanded graphite (EG). The dried LiF-LiCl-LiNO3 was ground and mixed with EG-SiCnw, the mass content of EG-SiCnw was 2%, and the mass ratio of EG to SiCnw was 2:1. It was then placed in a ball mill at a speed of 300r / min for 2h, and then the sample was placed in a nitrogen-protected tubular furnace. First, ventilate at room temperature for 1h to thoroughly remove the impurity atmosphere remaining in the furnace. Then, under the condition of a nitrogen flow rate of 50mL / min, the tubular furnace was heated at a heating rate of 5℃ / min, and the temperature was raised to 360℃ and maintained for 180min. Finally, the sample was taken out after naturally cooling to room temperature to obtain a nano-carbon substrate-wire interwoven micro-network structure thermally conductive enhanced molten salt phase change composite material.

[0105] One of the samples was washed with deionized water to remove the molten salt on the surface and inside of EG and SiCnw, and then dried to obtain the corresponding nanocarbon micronetwork sample. Fig. 9 This is the SEM image of the nanocarbon micronetwork obtained when the mass ratio of EG to SiCnw is 2:1. Fig. 9 As shown, under this condition, part of SiCnw is exposed between the nano-carbon sheets and on the surface, and stacking occurs, indicating that the SiCnw content is relatively high at this time, which destroys the uniform dispersion of nano-carbon and SiCnw. Fig.11 is the thermal conductivity diagram of the corresponding micro-network nano-carbon-based molten salt phase change composite material. Fig.11 As shown in the figure, under this condition, the thermal conductivity of the composite material is 2.49W / (m·K), and the thermal conductivity of the composite material is lower than that of the nanocarbon molten salt phase change composite material. This is because a large amount of SiCnw has agglomerated between the nanocarbon sheets and on the surface, hindering the heat transfer between the materials. Fig. 20 is the DSC curve of the corresponding micro-network nano-carbon-based molten salt phase change composite material. Fig. 20 As shown, under this condition, the phase change latent heat of the composite material is 345.09 J / g, which is not much different from that of the composite material with an EG content of 2%, indicating that the introduction of SiCnw does not change the heat storage properties of the composite material, and there is good chemical compatibility between molten salt, nanocarbon and SiCnw.

[0106] Example 10

[0107] The embodiment of the present invention provides a method for preparing a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, which comprises the following steps:

[0108] The ternary molten salt phase change material LiF-LiCl-LiNO3 (the mass ratio of LiF, LiCl and LiNO3 is 2:8:90) was placed in a 120℃ oven for more than 12h to ensure that the moisture was completely removed. Then, the flake graphite was placed in a muffle furnace and heated from room temperature to 800℃ at a heating rate of 10℃ / min, and then cooled rapidly to obtain expanded graphite (EG). The dried LiF-LiCl-LiNO3 was ground and mixed with EG-SiCnw, and the mass content of EG-SiCnw was 2% and the mass ratio of EG-SiCnw was 1:1. It was then placed in a ball mill at a speed of 300r / min for 2h, and then the sample was placed in a nitrogen-protected tubular furnace. First, ventilate at room temperature for 1h to thoroughly remove the impurity atmosphere remaining in the furnace. Then, under the condition of a nitrogen flow rate of 50mL / min, the tubular furnace was heated at a heating rate of 5℃ / min, and the temperature was raised to 360℃ and maintained for 180min. Finally, the sample was taken out after naturally cooling to room temperature to obtain a nano-carbon substrate-wire interwoven micro-network structure thermally conductive enhanced molten salt phase change composite material.

[0109] One of the samples was washed with deionized water to remove the molten salt on the surface and inside of EG and SiCnw, and then dried to obtain the corresponding nanocarbon micronetwork sample. Fig.10 This is the SEM image of the nanocarbon micronetwork obtained when the mass ratio of EG to SiCnw is 1:1. Fig.10 As shown, under this condition, SiCnw is more exposed between the nanocarbon sheets and on the surface, showing serious self-aggregation and stacking phenomena, indicating that the SiCnw content is too high at this time, and the nanocarbon and SiCnw are not evenly dispersed. Fig.11 is the thermal conductivity diagram of the corresponding nanocarbon micronetwork molten salt phase change composite material. Fig.11 As shown in the figure, under this condition, the thermal conductivity of the composite material is 2.33W / (m·K), and the thermal conductivity of the composite material is lower than that of the nanocarbon molten salt phase change composite material. This is because the excessive SiCnw is seriously aggregated between the nanocarbon sheets and on the surface, destroying the integrity and smoothness of the micro-thermal network and seriously hindering heat transfer. Fig.21 is the DSC curve of the corresponding nano-carbon molten salt phase change composite material. Fig.21 As shown, under this condition, the phase change latent heat of the composite material is 345.54 J / g, which is not much different from that of the composite material with an EG content of 2%, indicating that the introduction of SiCnw does not change the heat storage properties of the composite material, and there is good chemical compatibility between molten salt, nanocarbon and SiCnw.

[0110] In summary, the in-situ exfoliation method is used to construct a nanocarbon-based phase change composite material with a micro-network structure that imitates wood, which can increase the heat transfer path in the material, thereby improving the thermal conductivity of the material, solving the problem of low thermal conductivity of existing phase change materials, and fundamentally solving the agglomeration problem caused by the high surface energy of nanomaterials.

[0111] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A micro-network thermally conductive enhanced nano-carbon-based molten salt composite material, characterized in that: The invention comprises a molten salt phase change material, wherein a nano-carbon micro-network structure is distributed inside the molten salt phase change material, and the nano-carbon micro-network structure comprises a nano-carbon sheet layer.

2. The micro-network thermally conductive enhanced nano-carbon-based molten salt composite material according to claim 1, characterized in that: The nanocarbon micronetwork structure also includes silicon carbide nanowires. The nanocarbon micronetwork structure is a nanosheet-wire interwoven structure. Preferably, the mass ratio of the nanocarbon sheet layer to the silicon carbide nanowire is (12-1):1, more preferably (8-2):

1.

3. The micro-network thermally conductive enhanced nano-carbon-based molten salt composite material according to claim 1 or 2, characterized in that: The mass percentage of the nano-carbon network structure in the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material is 0.5% to 6%, preferably 1% to 4%.

4. The micro-network thermally conductive enhanced nano-carbon-based molten salt composite material according to claim 1, characterized in that: The molten salt phase change material is a multi-component molten salt, preferably a ternary eutectic molten salt, and more preferably, the ternary eutectic molten salt is composed of a lithium-based fluoride salt, a chloride salt and a nitrate salt.

5. A method for preparing a micro-network thermally conductive enhanced nano-carbon-based molten salt composite material according to any one of claims 1 to 4, characterized in that: It includes: The mixture containing the molten salt phase change material and the expanded graphite is heat-treated so that the expanded graphite is in-situ exfoliated to form the nano-carbon sheet layer.

6. The preparation method according to claim 5, characterized in that: The heat treatment is to raise the temperature to 320°C to 400°C and keep the temperature for 1 hour to 4 hours; Preferably, the heating rate is 4°C / min to 6°C / min.

7. The preparation method according to claim 5 or 6, characterized in that: The mixture containing molten salt phase change material and expanded graphite is obtained by the following steps: placing the molten salt phase change material and expanded graphite in a ball mill for ball milling; when containing silicon carbide nanowires, placing the molten salt phase change material, expanded graphite and silicon carbide nanowires in a ball mill for ball milling; Preferably, the molten salt phase change material is dried before ball milling; Preferably, the expanded graphite is obtained by rapidly heating flake graphite from room temperature in a muffle furnace and then cooling it down.

8. The preparation method according to claim 5, characterized in that: The mass content of the expanded graphite in the mixture is 0.5% to 6%, preferably 1% to 4%; when the mixture also contains silicon carbide nanowires, the total mass of the expanded graphite and the silicon carbide nanowires in the mixture is 0.5% to 6%, preferably 1% to 4%, and the mass ratio of the expanded graphite to the silicon carbide nanowires is (12 to 1):1, preferably (8 to 2):

1.

9. The preparation method according to claim 5, characterized in that: The heat treatment is performed in a tube furnace. Before the heat treatment, an inert gas is introduced at room temperature to remove impurity atmosphere.

10. Application of the micro-network thermally conductive enhanced nano-carbon-based molten salt composite material as described in any one of claims 1 to 4 in solar water heaters, solar thermal power generation systems, building exterior walls, waste heat recovery systems, electronic equipment cooling systems or cold chain transportation devices.