Composite plugging slurry and application method thereof
By combining gelling materials and bridged leak plugging agent in the leak plugging slurry, a composite leak plugging slurry of appropriate density is solved, and the problems of poor retention ability of inorganic gel leak plugging materials are solved, and the shallow sealing effect of the inorganic gel leak plugging materials are achieved. Effective sealing and high pressure bearing capacity of multi-stage leakage channels.
Patent Information
- Application Number
- CN202411050063.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
In the prior art, the inorganic gel leak plugging material has poor retention ability, poor effect on shallow sealing, and poor effect on multi-stage leaking channel leak plugging material.
A composite leak plugging slurry is adopted, including water, gelling material, and bridge leak plugging agent. The gelling material consists of a gel base material, slurry stabilizer and water absorbing expansion agent. The bridge leak plugging agent includes fiber material, particle material and The sheet-like material is formulated and processed in a specific proportion and forms a slurry with a density of 1.07-1.40g/cm3, combining the bridging effect of fibers, particulate materials and sheet-like materials to achieve effective sealing and retention.
It significantly improves the shallow sealing effect and retention capacity, can block multiple-level missing channels at one time, and improves the pressure bearing capacity and stability of the formation.
Smart Images

Figure BDA0004974659430000061 
Figure BDA0004974659430000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil and gas well plugging, and in particular to a composite plugging slurry and an application method thereof. Background Art
[0002] With the improvement of oil and gas exploration technology, more and more complex wells such as marginal wells, deep wells, and special wells are being developed. Due to the complexity of these formations themselves and the influence of the means of extraction during oil and gas extraction, the pressure bearing capacity of some formations has been significantly reduced, and the problem of well leakage has become more and more prominent. Well leakage not only prolongs the drilling cycle, but also affects the stability of the well wall, causing significant economic losses. Therefore, solving the problem of well leakage is of great practical significance.
[0003] At present, the commonly used plugging materials for formation leakage mainly include bridging plugging materials, polymer gel plugging materials, inorganic gel plugging materials, etc. The particle size distribution of bridging plugging materials is difficult to match with the leakage channel, it is difficult to form a long plugging belt, and it is easy to leak again; polymer gel plugging materials have low construction safety risks, can effectively plug long-section leakage, and have strong retention capacity, but the operation process is complicated and the cost is high, and it is difficult to plug multiple leakage channels at one time; inorganic gel plugging materials are simple to construct, cheap, and have high pressure bearing capacity after plugging the leakage layer, but the retention capacity is poor and it is easily affected by formation fluids. At the same time, the plugging effect on multi-level leakage channels is not obvious. Although there are many types of plugging materials, they all have defects to varying degrees.
[0004] The Chinese invention patent "A composite pressure-bearing plugging slurry, preparation method and construction method" (publication number: CN108456510B) authorizes a composite pressure-bearing plugging slurry. The plugging slurry of this invention includes bridge plugging slurry and consolidation slurry, wherein the consolidation slurry is cement slurry or chemical consolidation slurry. The combined use of bridge plugging slurry and consolidation slurry improves the pressure bearing capacity of the formation. The injection of bridge plugging slurry opens the cracks in the low-pressure formation and initially improves the pressure bearing capacity of the formation. The injection of consolidation slurry pushes the previously injected bridge plugging slurry to move deeper into the formation, further improving the pressure bearing capacity of the formation. The consolidation slurry with good fluidity is blocked by the bridge plugging slurry and stays near the wellbore, permanently improving the pressure bearing capacity of the formation. However, the density of the consolidation slurry is higher than 1.40g / cm 3 The shallow plugging effect is poor, and it is easy to leak into the deep formation under the action of pressure difference, which is difficult to meet the use requirements.
[0005] Therefore, how to provide a plugging agent with good shallow plugging effect and strong retention capacity is a problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0006] In view of this, the present invention provides a composite plugging slurry and an application method thereof, which are used to solve the problems in the prior art of poor retention capacity of inorganic gel plugging materials, poor plugging effect on shallow layers, and poor effect of multi-level leakage channel plugging materials.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] A composite plugging slurry, comprising, by weight, 100 parts of water, 20-25 parts of a cementitious material, and 1.6-7 parts of a bridging plugging agent;
[0009] The gelling material comprises a gelling base material, a slurry stabilizer, and a water-absorbing swelling agent, and the bridging plugging agent comprises a fiber material, a granular material, and a flaky material.
[0010] Preferably, the mass ratio of the gelling base, the slurry stabilizer and the water-absorbing swelling agent is (60-90):(5-13):(4-11).
[0011] Preferably, the weight proportions of the fiber material, granular material and sheet material in the composite plugging slurry are 0.1-1 part of the fiber material, 1-3 parts of the granular material and 0.5-3 parts of the sheet material respectively.
[0012] Preferably, the gelling base material is composed of one or a mixture of two of sulphoaluminate gelling materials and silicate gelling materials.
[0013] Preferably, the slurry stabilizer is one or a mixture of nano-silicon dioxide, nano-calcium carbonate and / or graphene oxide, and its particle size is 7-90nm.
[0014] Preferably, the water-absorbing swelling agent is diatomaceous earth, calcium carbonate and / or a water-absorbing resin, or a mixture of several of them.
[0015] Preferably, the fiber material is a mixture of one or more of plant fiber, aluminum silicate fiber, steel fiber, ceramic fiber and / or polypropylene fiber, and its length is less than 1 mm.
[0016] Preferably, the granular material is a mixture of one or more of walnut shells, olive shells, calcium carbonate, river sand, wollastonite and / or barium sulfate, and its size is in the range of 1-2 mm.
[0017] Preferably, the sheet material is a mixture of one or more of mica sheets, sheet polybutylene ester and / or sheet thermosetting resin, and its size is in the range of 2-5 mm.
[0018] The application method of the composite plugging slurry provided by the above technical solution includes the following processes:
[0019] (1) Weighing a gelling base material, a slurry stabilizer and a water-absorbing swelling agent according to the weight ratio, placing them in a stirrer and stirring for 2-4 hours, placing them in an oven at 60-80° C. and drying them for 8-12 hours, and cooling them to room temperature to obtain a gelling material;
[0020] (2) According to the density requirements on site, the cementitious material is added to clean water and stirred evenly, and then the fiber material, granular material and flaky material weighed in weight proportion are added in sequence and mixed evenly to obtain the composite plugging slurry;
[0021] (3) The composite plugging slurry obtained in step (2) is pumped into the designed position while drilling, and then the squeezing pressure is adjusted according to the on-site demand, the well is shut down and the pressure is reduced, and the plugging is performed. After the composite plugging slurry is gelled at the designed position and effective plugging is achieved, drilling or production is resumed.
[0022] It can be seen from the above technical solution that, compared with the prior art, the present invention discloses a composite plugging slurry and an application method thereof, wherein the density of the slurry prepared by the cementitious material is 1.07-1.40 g / cm 3 The density is close to the equivalent density of the lost formation pressure, which makes the slurry easy to stay in the lost channel. The bridging plugging materials such as fiber, granular material and flaky material are used together. While plugging the lost channel, it plays the role of retaining cementitious material. Compared with a single plugging agent, the plugging effect is significantly improved. At the same time, through gap squeezing, multiple lost channels can be plugged at one time, which has a high field application value. DETAILED DESCRIPTION
[0023] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] The various raw materials in the embodiments can be commercially available or prepared according to conventional methods in the art, which will not be described in detail here.
[0025] Example 1
[0026] (1) 80 parts of sulphoaluminate, 12 parts of nano-silicon dioxide and 8 parts of diatomaceous earth were weighed by weight, stirred in a stirrer for 2 h, placed in an oven at 60° C. for drying for 8 h, and cooled to room temperature to obtain a gelling material A1;
[0027] (2) Weigh 100 parts of water by weight, add 24 parts by weight of cementitious material A1 into the water while stirring, and after the mixture is evenly stirred, add 0.5 parts of plant fiber, 2 parts of calcium carbonate, and 1 part of mica flakes into the slurry in sequence to obtain a composite plugging slurry B1.
[0028] Example 2
[0029] (1) 52 parts of sulphoaluminate, 25 parts of silicate, 12 parts of nano-silicon dioxide and 11 parts of diatomaceous earth were weighed in parts by weight, stirred in a stirrer for 3 h, placed in an oven at 60° C. for drying for 10 h, and cooled to room temperature to obtain a gelling material A2;
[0030] (2) Weigh 100 parts of water by weight, add 23 parts by weight of cementitious material A2 into the water while stirring, and after the mixture is evenly stirred, add 0.5 parts of plant fiber, 1.5 parts of calcium carbonate, and 2 parts of mica flakes into the slurry in sequence to obtain a composite plugging slurry B2.
[0031] Example 3
[0032] (1) Weigh 40 parts of sulphoaluminate, 38 parts of silicate, 11 parts of nano-silicon dioxide and 11 parts of diatomaceous earth by weight, stir them in a stirrer for 2 hours, dry them in an oven at 60° C. for 10 hours, and cool them to room temperature to obtain a gelling material A3;
[0033] (2) Weigh 100 parts of water by weight, add 22 parts by weight of cementitious material A3 into the water while stirring, and after the mixture is evenly stirred, add 1 part of plant fiber, 3 parts of calcium carbonate, and 2 parts of mica flakes into the slurry in sequence to obtain a composite plugging slurry B3.
[0034] Example 4
[0035] (1) 90 parts by weight of sulphoaluminate gelling material and 10 parts by weight of diatomaceous earth were placed in a stirrer and stirred for 3 h, placed in an oven at 60° C. for drying for 10 h, and cooled to room temperature to obtain gelling material A4;
[0036] (2) Weigh 100 parts of water by weight, add 25 parts by weight of cementitious material A4 into the water while stirring, and after the mixture is evenly stirred, add 0.5 parts of plant fiber, 2 parts of calcium carbonate, and 2 parts of flaky thermosetting resin into the slurry in sequence to obtain a composite plugging slurry B4.
[0037] Comparative Example 1
[0038] A composite plugging slurry was prepared in the same manner as in Example 3, except that nano-carbon dioxide was replaced with nano-calcium carbonate to obtain composite plugging slurry C1.
[0039] Comparative Example 2
[0040] A composite plugging slurry was prepared in the same manner as in Example 3, except that no plant fiber, calcium carbonate and mica flakes were added, to obtain a composite plugging slurry C2.
[0041] Test Example 1
[0042] The composite plugging slurries B1-B4 in Examples 1-4 and the composite plugging slurries C1-C2 in Comparative Examples 1-2 were poured into a calibrated liquid density meter cup, and the density of the composite plugging slurries B1-B4 and C1-C2 was tested. The test results are shown in Table 1.
[0043] Table 1
[0044] Composite plugging slurry <![CDATA[Density (g / cm 3 )]]> Composite plugging slurry <![CDATA[Density (g / cm 3 )]]> B1 1.35 C1 1.16 B2 1.24 C2 1.14 B3 1.16 B4 1.45
[0045] It can be seen from Table 1 that the composite plugging slurries B1 and B4 prepared in Example 1 and Example 4 have a higher density, ≥1.35 g / cm 3 This is because the slurry has a high content of sulphoaluminate and a low content of silicate, resulting in a high density of the slurry. Compared with the composite plugging slurries B3 and C1-C2 prepared in Example 3 and Comparative Examples 1 and 2, the slurry density increases after the addition of the bridging plugging material, but the increase is not large; after the slurry stabilizer is replaced with nano calcium carbonate, the density of the slurry itself changes little.
[0046] Test Example 2
[0047] The composite plugging slurries B1-B4 and C1-C2 in Examples 1-4 and Comparative Examples 1-2 were placed at different temperatures, and the gelling time of the composite plugging slurries B1-B4 and C1-C2 was tested according to the standard GB10238-2005 "Oil Well Cement". The test results are as follows.
[0048] Table 2
[0049]
[0050] It can be seen from the gelling time of the composite plugging slurry in Table 2 that the gelling time of the composite plugging slurries B1-B4 and C1-C2 prepared in Examples 1-4 and Comparative Examples 1-2 shortens with increasing temperature, and the variation range is large, indicating that temperature has a great influence on the gelling time of the composite plugging slurry; the difference between Example 3 and Comparative Example 2 is whether a bridging material is added, and it is found that the difference in the gelling time of the two slurries is small, indicating that the addition of the bridging material does not affect the gelling time of the slurry material, indicating that the gelling material and the bridging material have good compatibility. It can be seen from Comparative Example 1 that nano calcium carbonate, as a slurry stabilizer, has a certain influence on the gelling properties of the composite plugging slurry, which will lead to an extension of the gelling time of the slurry.
[0051] Test Example 3
[0052] The sealing ability of the composite plugging slurries B1-B4 and C1-C2 prepared in Examples 1-4 and Comparative Examples 1-2 was tested using a high-temperature and high-pressure crack plugging instrument, and the cracks (4 mm inlet and 1 mm outlet) were plugged at 60°C. The specific testing method was as follows: pour the composite plugging slurry into the water loss cylinder of the plugging device, place a movable piston on the upper part, and then tighten the cylinder cover to seal it. After it solidifies, use a pump to inject liquid for pressurization, and record the pressure at the inlet end of the crack model in real time. The highest pressure when the liquid leaks from the outlet end of the crack model is taken as the highest sealing pressure of the gel on the crack. The test results are as follows.
[0053] Table 3
[0054]
[0055] It can be seen from the experimental data in Table 3 that the composite plugging slurries B1-B4 and C1-C2 prepared in Examples 1-4 and Comparative Examples 1-2 have good plugging effects on fracture-type leakage channels after gelling, among which the composite plugging slurry B3 has the best plugging effect, and the pressure bearing capacity after gelling is higher than 7MPa. Compared with the composite plugging slurry C2 without bridging material, the pressure bearing capacity is significantly improved, indicating that adding a bridging plugging agent to the gelling material can significantly improve the plugging effect of the slurry. The composite plugging slurry C1 leaks at 5MPa, indicating that in terms of pressure bearing capacity, the plugging ability of the slurry containing nano-calcium carbonate is not as good as that of the slurry containing nano-silicon dioxide. This may be because nano-silicon dioxide can strengthen the strength of the spatial network structure formed by sulphoaluminate salts and silicates, thereby improving the strength of the gel block, while nano-calcium carbonate does not have this effect.
[0056] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0057] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A composite plugging slurry, characterized in that: In parts by weight, it includes 100 parts of water, 20-25 parts of gelling material, and 1.6-7 parts of bridging plugging agent; The gelling material comprises a gelling base material, a slurry stabilizer, and a water-absorbing swelling agent, and the bridging plugging agent comprises a fiber material, a granular material, and a flaky material.
2. A composite plugging slurry according to claim 1, characterized in that: The mass ratio of the gelling base material, the slurry stabilizer and the water-absorbing swelling agent is (60-90):(5-13):(4-11).
3. The composite plugging slurry according to claim 1, characterized in that: The weight proportions of the fiber material, the granular material and the sheet material in the composite plugging slurry are respectively 0.1-1 part of the fiber material, 1-3 parts of the granular material and 0.5-3 parts of the sheet material.
4. The composite plugging slurry according to claim 1, characterized in that: The gelling base material is composed of one or a mixture of two of sulphoaluminate gelling materials and silicate gelling materials.
5. The composite plugging slurry according to claim 1, characterized in that: The slurry stabilizer is one or a mixture of nano silicon dioxide, nano calcium carbonate and / or graphene oxide, and its particle size is 7-90nm.
6. The composite plugging slurry according to claim 1, characterized in that: The water-absorbing swelling agent is diatomaceous earth, calcium carbonate and / or a water-absorbing resin, or a mixture of several of them.
7. The composite plugging slurry according to claim 1, characterized in that: The fiber material is a mixture of one or more of plant fiber, aluminum silicate fiber, steel fiber, ceramic fiber and / or polypropylene fiber, and its length is less than 1 mm.
8. The composite plugging slurry according to claim 1, characterized in that: The granular material is a mixture of one or more of walnut shells, olive shells, calcium carbonate, river sand, wollastonite and / or barium sulfate, and the size thereof is in the range of 1-2 mm.
9. The composite plugging slurry according to claim 1, characterized in that: The sheet material is a mixture of one or more of mica sheets, sheet polybutylene ester and / or sheet thermosetting resin, and its size is in the range of 2-5 mm.
10. An application method of the composite plugging slurry according to any one of claims 1 to 9, characterized in that: Including the following processes: (1) Weighing a gelling base material, a slurry stabilizer and a water-absorbing swelling agent according to the weight ratio, placing them in a stirrer and stirring for 2-4 hours, placing them in an oven at 60-80° C. and drying for 8-12 hours, and cooling them to room temperature to obtain a gelling material; (2) According to the density requirements on site, the cementitious material is added to clean water and stirred evenly, and then the fiber material, granular material and flaky material weighed in weight proportion are added in sequence and mixed evenly to obtain the composite plugging slurry; (3) The composite plugging slurry obtained in step (2) is pumped into the designed position while drilling, and then the squeezing pressure is adjusted according to the on-site demand, the well is shut down and the pressure is reduced, and the plugging is performed. After the composite plugging slurry is gelled at the designed position and effective plugging is achieved, drilling or production is resumed.
Citation Information
Patent Citations
A composite pressure-bearing sealing grout, its preparation method and construction method
CN108456510B