Cleaning agent and cleaning method
By using cleaning agents of organic acids, nonionic surfactants and corrosion inhibitors, combined with appropriate soaking, water washing and drying treatment, the problem of existing cleaning agents being poorly removed on the oxide layer of tin-plating products has been solved, and cleaning has been improved Efficiency and hourly output of tin-plated products.
Patent Information
- Application Number
- CN202411039162.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-19
AI Technical Summary
Existing cleaning agents are not effective when removing the oxide layer of tin-plating products, especially blue plating with severe oxidation, and it is difficult to completely dry after use, affecting the hourly output of the product.
Using cleaning agents including organic acids, nonionic surfactants and corrosion inhibitors, combined with soaking, water washing, dehydration and drying treatment methods, effective cleaning is achieved through organic acids, nonionic surfactants reduce oxidation reactions and corrosion inhibitors reduce Corrosion effect, the ratio of surfactant and corrosion inhibitor is optimized to improve cleaning efficiency.
It significantly improves the cleaning efficiency, reduces the cleaning time and drying time, enhances the hourly output of tin-plating products, maintains the quality of the product surface, and avoids the aggravation of the oxidation reaction.
Smart Images

Figure CN118978958A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the technical field of semiconductor packaging, and more particularly to a cleaning agent and a cleaning method. Background Art
[0002] Under certain temperature and humidity conditions, the tin layer of tin-plated products is prone to oxidation and discoloration when it comes into contact with oxygen in the air, mostly showing yellow and blue. When the oxide layer reaches a certain level, generally greater than 30nm, it will affect the welding function of the product.
[0003] At present, inorganic acids are generally used to clean yellowed products. However, the cleaning effect is relatively weak for blue coatings with severe oxidation (generally, the oxide film thickness is greater than 30nm).
[0004] After cleaning with inorganic acid, pure water is generally used to remove the acid remaining on the surface of the coating, which is difficult to dry. If it is not dried in time, water stains will remain, aggravating the oxidation of the coating. Summary of the invention
[0005] The problem solved by the embodiments of the present invention is to provide a cleaning agent and a cleaning method, which are beneficial to improving the hourly output of the product.
[0006] To solve the above problems, an embodiment of the present invention provides a cleaning agent, including: an organic acid; additives, including a surfactant and a corrosion inhibitor, wherein the surfactant is a non-ionic surfactant; and water.
[0007] Optionally, the organic acid includes one or more of methanesulfonic acid and alkylsulfonic acid.
[0008] Optionally, in the cleaning agent, the mass fraction of the organic acid is greater than or equal to 5wt%.
[0009] Optionally, in the cleaning agent, the mass fraction of the organic acid is in the range of 5wt%-25wt%.
[0010] Optionally, the nonionic surfactant includes one or more of long-chain fatty acid polyoxyethylene ether, alkylphenol polyoxyethylene ether and fatty acid polyoxyethylene ester.
[0011] Optionally, in the cleaning agent, the mass fraction of the surfactant is in the range of 0.5wt%-2wt%.
[0012] Optionally, the corrosion inhibitor includes one or more of potassium sulfate and potassium persulfate.
[0013] Optionally, in the cleaning agent, the mass fraction of the corrosion inhibitor is in the range of 3wt%-8wt%.
[0014] Optionally, the additives also include flame retardants.
[0015] Optionally, in the cleaning agent, the mass fraction of the additive is in the range of 3.5wt%-10wt%.
[0016] Optionally, the water is deionized water.
[0017] Correspondingly, an embodiment of the present invention further provides a cleaning method, comprising: using the cleaning agent provided by the embodiment of the present invention to soak the workpiece.
[0018] Optionally, the cleaning method further includes: washing the treated parts with water after the soaking treatment; dehydrating the treated parts with water after the washing treatment; and drying the treated parts with water after the dehydration treatment.
[0019] Optionally, the parts to be processed include tin-plated products or copper-plated products.
[0020] Optionally, in the step of immersing the workpiece, the immersion temperature is 35°C to 50°C.
[0021] Optionally, after the soaking treatment and before the dehydration treatment, multiple water washing treatments are performed.
[0022] Optionally, in the step of washing the treated parts with water, the washing time is 2 minutes to 5 minutes.
[0023] Optionally, in the step of dehydrating the workpiece, ethanol or isopropanol is used for the dehydration.
[0024] Optionally, in the step of dehydrating the workpiece, the dehydration time is 2 minutes to 5 minutes.
[0025] Optionally, in the step of drying the workpiece, the drying temperature is 100°C to 130°C.
[0026] Compared with the prior art, the technical solution of the embodiment of the present invention has the following advantages:
[0027] In the cleaning agent provided by the embodiment of the present invention, the cleaning agent includes an organic acid, an additive and water, and the additive includes a surfactant and a corrosion inhibitor, wherein the surfactant is a non-ionic surfactant; in the embodiment of the present invention, an organic acid is used to realize the cleaning function of the cleaning agent, and a better cleaning effect can be achieved for the cleaned product, and the corrosion effect on the product is small, which is conducive to better cleaning and reducing the damage caused by cleaning. The surfactant has the functions of good wettability and easy cleaning, which is conducive to enhancing the cleaning ability of the cleaning agent. At the same time, the corrosion inhibitor is used to further reduce the corrosion effect of the cleaning agent. Moreover, the surfactant is a non-ionic surfactant, which is conducive to reducing the ions on the surface of the product, thereby reducing the oxidation reaction on the surface of the product and maintaining the surface quality of the product, thereby shortening the cleaning time of the cleaning agent using the embodiment of the present invention, improving the cleaning efficiency, and further facilitating the improvement of the unit per hour (UPH) of the product.
[0028] In the cleaning method provided by the embodiment of the present invention, the cleaning agent provided by the embodiment of the present invention is used to soak the workpiece to be treated; in the embodiment of the present invention, the cleaning agent provided by the embodiment of the present invention is used to soak the workpiece to be treated, so as to clean the workpiece to be treated, wherein the organic acid is used to realize the cleaning function of the cleaning agent, which can achieve a better cleaning effect, and has a smaller corrosive effect on the workpiece to be treated, which is conducive to better cleaning and reducing cleaning damage, the surfactant has good wettability and easy cleaning functions, which is conducive to enhancing the cleaning ability of the cleaning agent, and the use of a corrosion inhibitor is conducive to further reducing the corrosive effect of the cleaning agent, and the surfactant is a non-ionic surfactant, which is conducive to reducing the ions on the surface of the workpiece to be treated, thereby reducing the oxidation reaction on the surface of the workpiece to be treated and maintaining the surface quality of the workpiece to be treated, thereby shortening the cleaning time of the cleaning method of the embodiment of the present invention, improving the cleaning efficiency, and further conducive to improving the output per hour (Units Per Hour, UPH) of the workpiece to be treated.
[0029] In an optional solution, after the water washing treatment and before the drying treatment, the workpiece to be treated is also dehydrated, which is beneficial to shorten the processing time of the drying treatment and thus beneficial to improve the cleaning efficiency of the workpiece to be treated. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 (a) to Figure 1 (i) is a photo of the experimental results corresponding to the experimental numbers 0-8 in an embodiment of the cleaning method of the present invention;
[0031] Figure 2 (a) to Figure 2 (i) is a photo of the experimental results corresponding to the experimental numbers 9-17 in the embodiment of the cleaning method of the present invention;
[0032] Figure 3 (a) to Figure 3 (f) is a photograph of the experimental results corresponding to the experimental numbers 18-23 in the embodiment of the cleaning method of the present invention;
[0033] Figure 4 (a) to Figure 4 (d) is a photograph of the experimental results corresponding to the experimental numbers 24-27 in an embodiment of the cleaning method of the present invention. DETAILED DESCRIPTION
[0034] The hourly output of products of the current cleaning method needs to be improved. The reasons why the hourly output of products needs to be improved are analyzed in combination with a cleaning method.
[0035] A current cleaning method includes: placing the product in a 5% dilute sulfuric acid cleaning agent and soaking for 5 minutes; after soaking, placing it in water to clean it; after cleaning it, placing it in an ion blower to blow dry it.
[0036] The cleaning effect of 5% dilute sulfuric acid cleaning agent is not good, especially for products with blue coatings that are severely oxidized. In addition, after cleaning with dilute sulfuric acid cleaning agent, it is difficult to dry it with water. If it is not dried in time, water stains will remain, aggravating the oxidation of the coating. If it is to be completely dried, it will take a long time, affecting the hourly output of the product.
[0037] To solve the above problems, an embodiment of the present invention provides a cleaning agent, including: an organic acid; additives, including a surfactant and a corrosion inhibitor, wherein the surfactant is a non-ionic surfactant; and water.
[0038] In the embodiment of the present invention, an organic acid is used to realize the cleaning function of the cleaning agent, and a good cleaning effect can be achieved for the cleaned product, and the corrosion effect on the product is small, which is conducive to better cleaning and reducing cleaning damage. The surfactant has good wettability and easy cleaning functions, which is conducive to enhancing the cleaning ability of the cleaning agent. At the same time, the use of a corrosion inhibitor is conducive to further reducing the corrosion effect of the cleaning agent. Moreover, the surfactant is a non-ionic surfactant, which is conducive to reducing the ions on the surface of the product, thereby reducing the oxidation reaction on the surface of the product and maintaining the surface quality of the product. Therefore, the cleaning time of the cleaning agent of the embodiment of the present invention is shortened, the cleaning efficiency is improved, and then it is conducive to improving the hourly output (Units Per Hour, UPH) of the product.
[0039] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below.
[0040] The cleaning agent of this embodiment is suitable for removing the oxide layer on the surface of metal materials. Specifically, in the semiconductor field, tin-plated or copper-plated products are prone to oxidation and discoloration when the coating comes into contact with oxygen in the air under certain temperature and humidity conditions. The cleaning agent of this embodiment can be used to clean the oxidized and discolored coating.
[0041] In this embodiment, the cleaning agent includes: an organic acid; additives including a surfactant and a corrosion inhibitor, wherein the surfactant is a non-ionic surfactant; and water.
[0042] Organic acids can play a better cleaning role and have less corrosive effect on products.
[0043] In the embodiment of the present invention, organic acid is used to realize the cleaning function of the cleaning agent, which can achieve a better cleaning effect on the product to be cleaned, and has a smaller corrosive effect on the product, which is conducive to better cleaning and reduces cleaning damage.
[0044] In this embodiment, the organic acid includes one or more of methanesulfonic acid and alkylsulfonic acid.
[0045] Using one or more of methanesulfonic acid and alkylsulfonic acid as the organic acid of the cleaning agent is beneficial to obtaining a better cleaning effect, especially for products with severely oxidized coatings, thereby helping to save the loss of solderability failure caused by product oxidation due to improper storage.
[0046] It should be noted that in this embodiment, the mass fraction of the organic acid in the cleaning agent should not be too small. If the mass fraction of the organic acid is too small, it is easy to cause the cleaning ability of the cleaning agent to be not too strong, resulting in poor cleaning effect on the product coating. For this reason, in this embodiment, the mass fraction of the organic acid in the cleaning agent is greater than or equal to 5wt%.
[0047] Specifically, it should be noted that in this embodiment, the mass fraction of the organic acid in the cleaning agent should not be too large or too small. If the mass fraction of the organic acid is too large, the cost of the cleaning agent is high, which is easy to cause unnecessary waste; if the mass fraction of the organic acid is too small, it is easy to cause the cleaning ability of the cleaning agent to be not too strong, resulting in poor cleaning effect on the product coating. For this reason, in this embodiment, the mass fraction of the organic acid in the cleaning agent is in the range of 5wt%-25wt%.
[0048] Additives are used to enhance the cleaning effect of cleaning agents, and are also used to add corresponding beneficial effects to cleaning agents according to actual process requirements.
[0049] It should be noted that, in this embodiment, the mass fraction of the additive in the cleaning agent should not be too large or too small. If the mass fraction of the additive is too large, it is easy to cause residues of the cleaning agent after the sample cleaning agent is used to clean the product, and it is also easy to increase the cost of the cleaning agent; if the mass fraction of the additive is too small, it is difficult to achieve the effect of enhancing the cleaning ability of the cleaning agent. For this reason, in this embodiment, the mass fraction of the additive in the cleaning agent is in the range of 3.5wt%-10wt%.
[0050] In this embodiment, the additives include a surfactant and a corrosion inhibitor. The surfactant has good wettability and is easy to clean, which is beneficial to enhancing the cleaning ability of the cleaning agent, thereby shortening the cleaning time of the cleaning agent using the embodiment of the present invention, improving the cleaning efficiency, and further facilitating the increase of the hourly output (Units Per Hour, UPH) of the product. At the same time, the use of the corrosion inhibitor is beneficial to further reduce the corrosive effect of the cleaning agent.
[0051] Surfactants are used to improve the wetting properties of cleaning agents.
[0052] In this embodiment, the surfactant is a nonionic surfactant.
[0053] Using non-ionic surfactants as additives to cleaning agents is beneficial to reducing ions on the product surface, thereby reducing oxidation reactions on the product surface and maintaining product surface quality. Especially for tin-plated products, reducing ions on the surface of the tin coating is beneficial to reducing oxidation reactions of the tin coating, thereby helping to ensure the surface quality of the tin-plated product.
[0054] In this embodiment, the nonionic surfactant includes one or more of long-chain fatty acid polyoxyethylene ether, alkylphenol polyoxyethylene ether and fatty acid polyoxyethylene ester.
[0055] Using one or more of long-chain fatty acid polyoxyethylene ether, alkylphenol polyoxyethylene ether and fatty acid polyoxyethylene ester as non-ionic surfactant is beneficial to reducing product surface ions and making the cleaning agent have better wettability.
[0056] It should be noted that, in this embodiment, the mass fraction of the surfactant should not be too large or too small. If the mass fraction of the surfactant is too large, it is easy to cause the cleaning agent to be difficult to remove after the product is cleaned with the cleaning agent, and the residual cleaning agent is easy to cause further damage to the product; if the mass fraction of the surfactant is too small, it is easy to cause insufficient wettability of the cleaning agent, and it is difficult to further improve the cleaning function of the cleaning agent. For this reason, in this embodiment, the mass fraction of the surfactant in the cleaning agent ranges from 0.5wt% to 2wt%.
[0057] Corrosion inhibitors are used to prevent excessive corrosion during product cleaning.
[0058] In this embodiment, the corrosion inhibitor includes one or more of potassium sulfate and potassium persulfate.
[0059] Using one or more of potassium sulfate and potassium persulfate as corrosion inhibitors is beneficial to better improve the anti-corrosion effect of the product.
[0060] It should be noted that in this embodiment, the mass fraction of the corrosion inhibitor in the cleaning agent should not be too large or too small. If the mass fraction of the corrosion inhibitor is too large, it is easy to increase the cost of the cleaning agent and cause unnecessary waste; if the mass fraction of the corrosion inhibitor is too small, it is difficult to effectively prevent over-corrosion during product cleaning. For this reason, in this embodiment, the mass fraction of the corrosion inhibitor in the cleaning agent ranges from 3wt% to 8wt%.
[0061] In this embodiment, the additive further includes a flame retardant.
[0062] Adding flame retardants to cleaning agents can increase the flash point of cleaning agents and help improve the safety of cleaning agents.
[0063] In this embodiment, the flame retardant includes a nitrogen-based halogen-free flame retardant, such as carbamate.
[0064] In this embodiment, in addition to the aforementioned components, the remaining components in the cleaning agent are all water, that is, the sum of the mass fractions of the aforementioned components and water is 100%.
[0065] In this embodiment, water is deionized water (DI Water).
[0066] The cleaning agent of this embodiment uses deionized water, which is beneficial to improving the purity of the cleaning agent.
[0067] Combined with reference Figures 1 to 4 , an embodiment of the present invention also provides a cleaning method.
[0068] In this embodiment, the cleaning method includes: using the cleaning agent provided in the above embodiment to soak the workpiece.
[0069] In this embodiment, the cleaning agent provided in the above-mentioned embodiment is used to soak the workpiece.
[0070] By using the cleaning agent provided in the above embodiment to soak the workpiece to be processed, the yellowish and bluish discolored oxide layer on the workpiece to be processed can be removed.
[0071] In this embodiment, the cleaning agent provided by the embodiment of the present invention is used to soak the parts to be treated so as to clean them. The organic acid is used to realize the cleaning function of the cleaning agent, which can achieve a better cleaning effect and has less corrosive effect on the parts to be treated, which is conducive to better cleaning and reduces cleaning damage. The surfactant has good wettability and easy cleaning functions, which is conducive to enhancing the cleaning ability of the cleaning agent. At the same time, the use of corrosion inhibitors is conducive to further reducing the corrosive effect of the cleaning agent. Moreover, the surfactant is a non-ionic surfactant, which is conducive to reducing the ions on the surface of the parts to be treated, thereby reducing the oxidation reaction on the surface of the parts to be treated and maintaining the surface quality of the parts to be treated.
[0072] Specifically, in this embodiment, the workpiece to be processed includes a tin-plated product or a copper-plated product.
[0073] The cleaning method of this embodiment is suitable for removing the oxide layer on the surface of metal materials. Specifically, in the semiconductor field, tin-plated products or copper-plated products are prone to oxidation and discoloration when the coating comes into contact with oxygen in the air under certain temperature and humidity conditions. The cleaning method of this embodiment can be used to clean the oxidized and discolored coating.
[0074] It should be noted that in this embodiment, in the step of soaking the treated part, the soaking temperature should not be too high or too low. If the soaking temperature is too high, it is easy to cause the components in the cleaning agent to volatilize, thereby weakening the cleaning effect of the cleaning agent; if the soaking temperature is too low, it is easy to cause the components in the cleaning agent to react too slowly with the oxide layer of the coating, resulting in a long cleaning time and poor cleaning efficiency. For this reason, in this embodiment, in the step of soaking the treated part, the soaking temperature is 35°C to 50°C.
[0075] It should be noted that, in the present embodiment, in the step of immersing the workpieces to be treated, the immersion treatment time is set according to the treatment area and the number of the workpieces to be treated.
[0076] In this embodiment, the cleaning method further includes: after the immersion treatment, washing the parts to be treated with water; after the washing treatment, dehydrating the parts to be treated; after the dehydration treatment, drying the parts to be treated.
[0077] In this embodiment, after the immersion treatment, the workpiece is washed with water.
[0078] After the soaking treatment, the treated parts are washed with water to clean the residual cleaning agent and avoid the residual cleaning agent from damaging the treated parts.
[0079] In this embodiment, after the soaking treatment, multiple water washing treatments are performed before the subsequent dehydration treatment.
[0080] Perform multiple water washing processes to further remove residual cleaning agent.
[0081] It should be noted that, in the step of washing the treated parts with water in this embodiment, the treatment time of the water washing treatment should not be too long or too short. If the treatment time of the water washing treatment is too long, it is easy to cause unnecessary damage to the treated parts; if the treatment time of the water washing treatment is too short, it is difficult to effectively wash away the residual cleaning agent. For this reason, in the step of washing the treated parts with water in this embodiment, the treatment time of the water washing treatment is 2 minutes to 5 minutes.
[0082] In this embodiment, after the water washing process, the workpiece is dehydrated.
[0083] After the water washing treatment, the workpiece is dehydrated to remove the residual water from the water washing treatment to a large extent.
[0084] In this embodiment, after the water washing treatment and before the drying treatment, the parts to be treated are also dehydrated, which is beneficial to shorten the treatment time of the drying treatment, thereby helping to shorten the cleaning time of the cleaning method of the embodiment of the present invention, improving the cleaning efficiency, thereby helping to improve the cleaning efficiency of the parts to be treated, and further helping to increase the output per hour (Units Per Hour, UPH) of the parts to be treated.
[0085] In this embodiment, in the step of dehydrating the workpiece, ethanol or isopropanol is used for the dehydration.
[0086] Specifically, placing the workpiece to be processed in ethanol or isopropanol for dehydration can achieve a better dehydration effect.
[0087] It should be noted that, in the step of dehydrating the workpiece in this embodiment, the dehydration time should not be too long or too short. If the dehydration time is too long, it is easy to cause unnecessary damage to the workpiece; if the dehydration time is too short, it is easy to fail to achieve a good dehydration effect. For this reason, in the step of dehydrating the workpiece in this embodiment, the dehydration time is 2 minutes to 5 minutes.
[0088] In this embodiment, after the dehydration treatment, the workpiece is dried.
[0089] After the dehydration treatment, the workpiece to be treated is dried to remove the water stains remaining on the workpiece to be treated and keep the surface of the workpiece to be treated clean.
[0090] It should be noted that in this embodiment, in the step of drying the workpiece, the processing temperature of the drying treatment should not be too high or too low. If the processing temperature of the drying treatment is too high, it is easy to cause unnecessary damage to the workpiece due to the excessively high ambient temperature; if the processing temperature of the drying treatment is too low, it is difficult to achieve a good drying effect, and it is easy to cause the drying time to be too long and the drying effect to be too low. For this reason, in this embodiment, in the step of drying the workpiece, the processing temperature of the drying treatment is 100°C to 130°C.
[0091] In this embodiment, methanesulfonic acid is used as an organic acid of the cleaning agent, and multiple experiments are carried out on the workpiece to be treated.
[0092] Specifically, this embodiment carried out experiments numbered 0-8, in which experiment number 0 used a traditional cleaning agent whose component was dilute sulfuric acid to clean the workpiece to be treated, and experiment number 1-8 used the cleaning agent provided in this embodiment, in which the cleaning agent component was methanesulfonic acid to clean the workpiece to be treated. Experiments were conducted under different conditions of methanesulfonic acid concentration (i.e., cleaning agent concentration), surfactant concentration, corrosion inhibitor concentration, cleaning time (i.e., processing time of immersion treatment), dehydrating agent (i.e., component used for dehydration treatment) and drying time (i.e., processing time of drying treatment) to observe the effect of removing the oxide layer on the surface of the workpiece to be treated, as shown in Table 1, where concentration refers to mass fraction.
[0093]
[0094]
[0095] Table 1
[0096] This embodiment also carried out experiments No. 9-17, using the cleaning agent provided in this embodiment, using methanesulfonic acid as the cleaning agent component to clean the workpiece to be treated, with surfactant concentrations of 0.5%, corrosion inhibitor concentrations of 3%, and methanesulfonic acid concentrations (i.e., cleaning agent concentrations), cleaning time (i.e., immersion treatment time), dehydrating agent (i.e., the component used for dehydration treatment) and drying time (i.e., drying treatment time) under different conditions to observe the effect of removing the oxide layer on the surface of the workpiece to be treated, see Table 2, where concentration refers to mass fraction.
[0097]
[0098]
[0099] Table 2
[0100] This embodiment also carried out experiments No. 18-23, using the cleaning agent provided in this embodiment, using methanesulfonic acid as the cleaning agent component to clean the workpiece to be treated, with surfactant concentrations of 2%, corrosion inhibitor concentrations of 8%, and experiments conducted under different conditions of methanesulfonic acid concentration (i.e., cleaning agent concentration), cleaning time (i.e., immersion treatment time), dehydrating agent (i.e., the component used for dehydration treatment) and drying time (i.e., drying treatment time) to observe the effect of removing the oxide layer on the surface of the workpiece to be treated, see Table 3, where concentration refers to mass fraction.
[0101]
[0102] Table 3
[0103] This embodiment also carried out experiments No. 24-27, using the cleaning agent provided in this embodiment, using methanesulfonic acid as the cleaning agent component to clean the workpiece to be treated, and conducting experiments under different conditions of methanesulfonic acid concentration (i.e., cleaning agent concentration), surfactant concentration, corrosion inhibitor concentration, cleaning time (i.e., treatment time of immersion treatment), dehydrating agent (i.e., the component used for dehydration treatment) and drying time (i.e., treatment time of drying treatment) to observe the effect of removing the oxide layer on the surface of the workpiece to be treated, see Table 4, where concentration refers to mass fraction.
[0104]
[0105]
[0106] Table 4
[0107] It can be seen that in this embodiment, methanesulfonic acid is used as the organic acid of the cleaning agent, which can better remove the coating oxide, and the experimental effect of methanesulfonic acid concentration of 5wt%-25wt% is better. When too little surfactant is used, the cleaning time will be increased. The experimental effect of surfactant concentration of 0.5wt%-2wt% is better, and the experimental effect of corrosion inhibitor concentration of 3wt%-8wt% is better. When dehydration treatment is not performed, the drying time will be increased, so it is necessary to add drying treatment to the cleaning method.
[0108] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A cleaning agent, It is characterized in that include: Organic acids; Additives, including surfactants and corrosion inhibitors, wherein the surfactant is a nonionic surfactant; water.
2. The cleaning agent according to claim 1, It is characterized in that The organic acid includes one or more of methanesulfonic acid and alkylsulfonic acid.
3. The cleaning agent according to claim 1, It is characterized in that In the cleaning agent, the mass fraction of the organic acid is greater than or equal to 5wt%.
4. The cleaning agent according to claim 1, It is characterized in that In the cleaning agent, the mass fraction of the organic acid is in the range of 5wt%-25wt%.
5. The cleaning agent according to claim 1, It is characterized in that The nonionic surfactant includes one or more of long-chain fatty acid polyoxyethylene ether, alkylphenol polyoxyethylene ether and fatty acid polyoxyethylene ester.
6. The cleaning agent according to claim 1, It is characterized in that In the cleaning agent, the mass fraction of the surfactant is in the range of 0.5wt%-2wt%.
7. The cleaning agent according to claim 1, It is characterized in that The corrosion inhibitor includes one or more of potassium sulfate and potassium persulfate.
8. The cleaning agent according to claim 1, It is characterized in that In the cleaning agent, the mass fraction of the corrosion inhibitor is in the range of 3wt%-8wt%.
9. The cleaning agent according to claim 1, It is characterized in that The additives also include flame retardants.
10. The cleaning agent according to claim 1, It is characterized in that In the cleaning agent, the mass fraction of the additive is in the range of 3.5wt%-10wt%.
11. The cleaning agent according to claim 1, It is characterized in that The water is deionized water.
12. A cleaning method, It is characterized in that include: The cleaning agent according to any one of claims 1 to 11 is used to immerse the workpiece.
13. The cleaning method according to claim 12, It is characterized in that The cleaning method further comprises: after the immersion treatment, washing the workpiece with water; After the water washing process, the workpiece to be processed is subjected to a dehydration process; After the dehydration treatment, the workpiece to be treated is dried.
14. The cleaning method according to claim 12, It is characterized in that The workpiece to be processed includes a tin-plated product or a copper-plated product.
15. The cleaning method according to claim 12, It is characterized in that In the step of immersing the workpiece, the treatment temperature of the immersion treatment is 35°C to 50°C.
16. The cleaning method according to claim 13, It is characterized in that After the soaking treatment, the water washing treatment is performed multiple times before the dehydration treatment.
17. The cleaning method according to claim 13, It is characterized in that In the step of washing the workpiece to be treated with water, the treatment time of the water washing treatment is 2 minutes to 5 minutes.
18. The cleaning method according to claim 13, It is characterized in that In the step of dehydrating the workpiece to be processed, ethanol or isopropanol is used for the dehydration.
19. The cleaning method according to claim 13, It is characterized in that In the step of dehydrating the workpiece to be processed, the dehydration treatment time is 2 minutes to 5 minutes.