Application method of nanoparticle-coated microorganisms in concrete crack self-repairing

The method of coating Bacillus sp.B6 Bacillus in nanotin dioxide particles solves the problem of low microbial survival rate in concrete, significantly improves the self-repair ability and durability of concrete, and achieves better crack repair results, avoiding the use of The defects of traditional carriers.

CN118979032APending Publication Date: 2024-11-19SHENZHEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411215913.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The low survival rate of microorganisms in concrete leads to poor self-repair effect. The existing carriers have defects in pressure resistance, economy and compatibility, making it difficult to effectively repair concrete cracks.

Method used

Bacillus sp.B6 was coated with nanotin dioxide particles, and the combination of vegetative cells, spores and nanomaterials was prepared to form a mixed suspension, and stirred with MCC microcrystalline cellulose powder into small balls with a diameter of 4mm for use in Repair concrete cracks.

Benefits of technology

It significantly improves the survival rate and mineralization ability of microorganisms in concrete, enhances the self-repairing ability of concrete, and has better restoration effect than traditional methods. It is environmentally friendly and economical, improving the durability and structural stability of concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979032A_ABST
    Figure CN118979032A_ABST
Patent Text Reader

Abstract

The invention provides an application method of nanoparticles-coated microorganisms in concrete crack self-repairing, which comprises the following steps: step 1, preparing nutritional cells, and preparing a solid culture medium; step 2, preparing spores; the method comprises the following steps: inoculating Bacillus sp.B6 into a culture solution of an LB culture medium by using a culture solution culture method, and then transferring the Bacillus sp.B6 into a culture solution for promoting spores to form an MSP culture medium; 3, spores are diluted, and qualified bacteria concentration is selected; step 4, preparing nano particles, and selecting nano tin dioxide particles; step 5, combining the spores with the nano material; forming a mixed suspension; step 6, preparing self-repairing small balls; the prepared concrete self-repairing agent is small in microsphere size, large in specific surface area and higher in interaction capacity with microorganisms, the novel nanometer material has high catalytic activity, adsorption and catalytic reaction are prone to occurring on the surface of the novel nanometer material, and the survival rate of the microorganisms in concrete can be effectively increased when the novel nanometer material is attached to the surfaces of the microorganisms.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The invention relates to the cross-technical field of microbiology and civil engineering materials, and in particular to an application method of nanoparticle-coated microorganisms in self-repairing of concrete cracks. [Background Technology]

[0002] Concrete cracking is the most challenging problem in the construction industry. Concrete cracking can lead to corrosion of the steel bars, which may cause damage to the entire concrete structure, and the cost of repairing these cracks is very expensive. A microbial-based repair strategy has been proposed, using bacteria to induce calcium carbonate precipitation in concrete structures, known as self-healing concrete. The self-healing mechanism is a promising solution to the problem of concrete cracking. However, there are still many problems to be solved in this technology, and the low survival rate of microorganisms in concrete is one of them. The main reason is that the environment in concrete is harsh, not only with a high pH and low oxygen content, but also with low moisture content, which is not conducive to the growth and reproduction of most microorganisms.

[0003] Microbial self-repair technology often uses porous carriers to immobilize microorganisms and then mixes them into fresh concrete. The attached carriers include silica gel, nanographite sheets, ceramsite and zeolite, etc. However, from the perspective of pressure resistance, economy, bacterial immobilization capacity and compatibility between the carrier and the concrete matrix, the above carriers all have their own inherent shortcomings. Therefore, it is crucial to select an attached carrier with good comprehensive performance and a microbial immobilization method to promote microbial mineralization concrete crack self-repair technology. [Summary of the invention]

[0004] In view of the defects of the above-mentioned prior art, the present invention proposes a method for applying nanoparticle-coated microorganisms in the self-repair of concrete cracks, which can effectively provide a living space for microorganisms and prevent bacteria from being damaged during the concrete preparation process.

[0005] The application method of the nanoparticle-coated microorganisms in the self-repair of concrete cracks of the present invention is as follows: the microorganisms are: Bacillus sp. B6 (CGMCC 13360), and the nanoparticle carrier is nano-tin dioxide particles; the nanoparticles are applied to concrete repair through the following steps:

[0006] Step 1, prepare nutrient cells and prepare solid culture medium; add 15g / L agar powder to LB culture medium, place in a 30°C constant temperature incubator for culturing for 1 day, and keep at a constant temperature of 4°C;

[0007] Step 2, preparing spores: using a culture medium method, inoculating Bacillus sp. B6 into a culture medium of LB medium, then transferring it to a culture medium of MSP medium for promoting spore formation, fermenting and centrifuging, and resuspending the spore precipitate after centrifugation with deionized water to a concentration of about 5×10 8 The spore suspension of 1000 g / mL was kept at a constant temperature of 4°C;

[0008] Step 3, dilute the spores and select qualified bacterial concentrations; dilute the selected spores prepared in step 2 to 1×10 7 After fixation and drying, a bacterial counting plate was used to observe the spore morphology and count the number of spores.

[0009] Step 4, preparing nanoparticles, selecting nano-tin dioxide particles; the size is 20-40nm, and the purity is 99.9%;

[0010] Step 5, combining spores and nanomaterials; concentrating the spores in the qualified spore culture medium to 2.5×10 9 / mL, and combine qualified nano-tin dioxide particles with spores to form a mixed suspension;

[0011] Step 6, prepare self-repairing beads, add the mixed suspension to MCC microcrystalline cellulose powder and stir to form a ball, take out the ball, make a ball with a diameter of 4 mm, place the ball in a culture dish, and dry it in an incubator at 37°C to obtain self-repairing agent microspheres for repairing concrete.

[0012] Furthermore, the formula of the LB medium is (g / L): 5 g yeast powder, 10 g tryptone, 0.84 g NaHCO3, 9.54 g Na2CO3, and the pH value of the medium is 9.7.

[0013] Furthermore, the formula of the MSP culture medium is (g / L): NH4NO3 0.3 g, KH2PO4 0.02 g, CaCl2·2H2O 0.225 g, KC l 0.476 g, MgCl2·6H2O 0.2 g, MnSO4·2H2O 0.01 g, yeast powder 3 g, soluble starch 1 g, NaHCO3 4.2 g, Na2CO3 5.3 g, and the pH value of the culture medium is 9.7.

[0014] Furthermore, in the step 2, before transferring to the MSP medium, the LB medium is placed in a shaker at 30° C. and 150 rpm for constant temperature shaking culture for about 18 hours.

[0015] Furthermore, in step 6, CHL nutrient solution is added to improve the growth reliability of spores, and the CHL nutrient solution is prepared in the following amount per 50 mL: 20 mL of A solution: 2.38 g of KNO3, 0.0075 g of KH2PO4, 0.325 g of MgSO4, and 1.25 g of inosine, and the pH is adjusted to 12.0 with 6M NaOH after dissolution; 20 mL of B solution: 10 g of starch is dissolved in 20 mL of water, stirred into a paste, and then mixed evenly with 10 mL of boiling water, and then repeatedly boiled 2-3 times in a microwave oven, mixed with A solution, and added to the mixed suspension of spores and nano-tin dioxide.

[0016] The present invention has the following advantages: the concrete self-repairing agent microspheres prepared by the present invention are small in size, large in specific surface area, and have stronger ability to interact with microorganisms; and the new nanomaterials have high catalytic activity, and adsorption and catalytic reactions are easily generated on their surfaces. Attaching to the surfaces of microorganisms can effectively improve the survival rate of microorganisms in concrete. [Drawings]

[0017] Figure 1 This is a flow chart of the method for applying the nanoparticle-coated microorganisms of the present invention to the self-repair of concrete cracks;

[0018] Figure 2 This is an electron microscopic image of the combination of spores and nanomaterials in step 5 of the method for using nanoparticle-coated microorganisms in concrete crack self-repair of the present invention;

[0019] Figure 3 It is a schematic diagram of the microstructure of the self-repairing spheres in step 6 of the method for applying nanoparticle-coated microorganisms in the self-repair of concrete cracks of the present invention.

[0020] Figure 4 The spore germination test results of the application method of the nanoparticle-coated microorganisms in the self-repair of concrete cracks of the present invention;

[0021] Figure 5 It is the result of spore growth test of the application method of the nanoparticle-coated microorganisms in the self-repair of concrete cracks of the present invention;

[0022] Figure 6 The present invention is an application method of the microorganisms coated with nanoparticles in the self-repair of concrete cracks to detect the deposition of spores CaCO3;

[0023] Figure 7 It is a comparison of the self-repairing agent microspheres of the present invention used for repairing concrete cracks;

[0024] Figure 8 It is a comparison of the concrete crack repair rate of the present invention;

[0025] Fig. 9This is a comparison of the porosity test results of concrete by the present invention. [Specific implementation method]

[0026] In order to make the technical means implemented by the present invention clear and understandable, the present invention is further described below with reference to the accompanying drawings.

[0027] The present invention uses microorganisms and nanoparticles as carriers in concrete repair. The method uses Bacillus sp. B6 (CGMCC 13360), which is isolated from mangrove sediments with high salinity, low oxygen content, complex structure and biological species, and is an alkaliphilic bacillus. At the same time, nano-tin dioxide particles are selected to mix with the prepared Bacillus sp. B6 bacillus, the process is simple, easy to prepare, and the protective carrier fixes the bacterial cells to solve the problems related to directly adding bacteria to the concrete matrix. The unique biological and chemical properties of nanoparticles make it applicable to biotechnology, effective interaction with microbial membranes, and great potential for promoting concrete self-repair, and there is no adverse effect on the vitality of microorganisms. Therefore, the nanoparticles selected by the present invention can be considered as a carrier for fixing bacterial cells. Next, how to combine Bacillus sp. B6 with nano-tin dioxide particles to prepare biological balls that can be used to repair concrete is described in detail.

[0028] Step 1, prepare nutrient cells, prepare solid culture medium, add 15g / L agar powder to LB culture medium, pick Bacillus sp.B6 culture, inoculate the bacillus prepared in step 1, and after the inoculation is completed, place it in a 30°C constant temperature incubator for culturing for 1 day and keep it at 4°C; the formula of the LB culture medium is (g / L): 5g yeast powder, 10g tryptone, 0.84g NaHCO3, 9.54g Na2CO3, and the pH value of the culture medium is 9.7.

[0029] Step 2, prepare spores, use the culture medium culture method, inoculate Bacillus sp. B6 bacillus in alkaline LB (Lur i a-Bertan i) culture medium, put the inoculated culture medium into a 30 ° C, 150rpm shaker for constant temperature shaking culture for about 18 hours, and then inoculate it into the culture medium of the MSP culture medium for spore formation, and then take a volume fraction of 10% B6 bacillus and transfer it to the MSP culture medium for spore formation, and put it into a 30 ° C, 150rpm shaker for constant temperature shaking culture for 4-7 days. At the same time, take samples regularly every day, detect the spore ratio by phase contrast microscopy, and use a cell counting plate to detect the bacterial concentration to monitor the spore fermentation. When the culture medium becomes obviously turbid, that is, the spore ratio is greater than 95%, the fermentation liquid is centrifuged at 6000rpm for 15min, and deionized water is added for centrifugal washing 6-8 times to terminate the fermentation. Then centrifuge, and resuspend the spore precipitate after centrifugation with deionized water to a concentration of about 5×10 8 The spore suspension of 1000 g / mL was placed at a constant temperature of 4°C; the formula of the MSP medium is (g / L): 0.3 g NH4NO3, 0.02 g KH2PO4, 0.225 g CaCl2·2H2O, 0.476 g KCl, 0.2 g MgCl2·6H2O, 0.01 g MnSO4·2H2O, 3 g yeast powder, 1 g soluble starch, 4.2 g NaHCO3, 5.3 g Na2CO3, and the pH value of the medium is 9.7. Figure 4 The spore germination test results shown in the figure show that, under the same time comparison, the spore germination rate of the experimental group after adding nano-tin dioxide is higher than that of the control group containing only spores, which effectively improves the spore germination rate. Figure 5 The spore growth test results shown are as follows: after the spores germinate into nutrient cells, they can grow and reproduce rapidly under suitable conditions, and their growth can be evaluated using the ETSA value. The ETSA value measures the activity of the electron transport chain of the bacterial cell membrane. The higher the ETSA value, the more vigorous the bacterial growth. The experimental groups with an added nano-tin dioxide concentration of more than 150 μg / ml can promote the growth and reproduction of bacteria. The four experimental groups all reached the ETSA peak after 36 hours of cultivation, and the peak values ​​were: 200 μg / ml>250 μg / ml>300 μg / ml>150 μg / ml. The remaining three experimental groups showed a downward trend after reaching the ETSA peak value in 12 hours. Therefore, the added nano-tin dioxide concentration of more than 150 μg / ml can be considered to be able to effectively promote the growth of bacteria.

[0030] Step 3: dilute the spores and select qualified bacterial concentrations. Dilute the selected spores prepared in step 2 to 1×10 7 / mL, after fixing and drying, use a bacterial counting plate to observe the spore morphology and count the number of spores; this step needs to ensure the qualified fermentation concentration of bacteria, and a bacterial counting plate can be used for observation and statistics. Take the bacterial counting plate, disinfect it, and rinse the bacterial counting plate with deionized water to ensure that there are no other bacteria or impurities remaining on the counting plate. Wipe it with lens paper and dry it, and place it on the stage. Place a clean cover glass on the right side of the Newton ring of the bacterial counting plate, fit it tightly, and slowly move it to the center of the counting plate. Then draw 2μL of the diluted spore suspension and drop it on the side of the cover glass, and flow into the gap between the counting plate and the cover glass through capillary action. Randomly select five small squares with appropriate spore numbers (about 50) in the field of view. When the number of spores in each square in the field of view is within 30-300, count the number of spores in the square and on the top and left, calculate the total value and average it. If the number of spores exceeds or is insufficient, modify the spore dilution multiple and re-experiment.

[0031] Step 4, prepare nanoparticles, select nano-tin dioxide particles, which must meet at least the following two dimensions: a size of 20-40nm and a purity of 99.9%; the nano-tin dioxide particles need to be sampled and analyzed, and qualified nano-tin dioxide particles are selected. The selection method can use at least one of the following methods, such as

[0032] Nano-laser particle size analysis: The particle size is detected by measuring the fluctuation of particle scattered light caused by the Brownian motion of nanoparticles. A small amount of nano-tin dioxide sample is dissolved in deionized water, and the size of the nanoparticles is determined using a nano-laser particle size analyzer (DLS, Del saMax COR).

[0033] Infrared absorption spectroscopy: The infrared spectrum is determined by measuring the interference pattern and performing Fourier transform on the interference pattern. According to the different characteristics of the spectrum, the functional groups of unknown substances can be determined, the chemical structure can be determined, the chemical reaction process can be observed, isomers can be distinguished, and the purity of the substance can be analyzed.

[0034] X-ray diffraction analysis: Take 3g of nano-tin dioxide sample, use X-ray diffractometer (XRD, empyrean) to obtain the source file of XRD analysis by using the principle of electromagnetic vibration, import it into MDI Jade 6.5 software, compare the X-ray diffraction spectrum of the object under test with its PDF standard card, and qualitatively analyze the crystal structure of the material, as well as the elemental composition of the material and other information.

[0035] Step 5: Combination of spores and nanomaterials to concentrate the spores in the qualified spore culture medium to 2.5×10 9 / mL, and combine qualified nano-tin dioxide particles with spores to form a mixed suspension; during the process, a high-resolution scanning electron microscope (SEM, Thermo APREO S) can be used to observe the microscopic combination morphology of spores and nano-tin dioxide. Figure 2 As shown, the upper left is the nanomaterial, the lower left is the spore, and the right is the electron microscope image of the combination of the two.

[0036] Step 6, prepare self-repairing beads, add the mixed suspension containing spores and nano-tin dioxide to MCC microcrystalline cellulose powder and stir to form a ball, take out the ball, and make it into a ball with a diameter of 4 mm. Every 5.5g of MCC microcrystalline cellulose powder can make 120 balls. Place the ball in a culture dish and dry it in an incubator at 37°C for 4 days to obtain self-repairing agent microspheres for repairing concrete.

[0037] In step 6, CHL nutrient solution can be added to improve the growth reliability of spores, such as Figure 3 The microstructure of the self-repairing spheres shown in the figure is as follows: CHL nutrient solution is prepared in the following amount per 50 mL: 20 mL of A solution (2.38 g of KNO3, 0.0075 g of KH2PO4, 0.325 g of MgSO4, 1.25 g of inosine, and the pH is adjusted to 12.0 with 6M NaOH after dissolution), 20 mL of B solution, 10 g of starch is dissolved in 20 mL of water, stirred into a paste and mixed evenly with 10 mL of boiling water, and then boiled repeatedly in a microwave oven for 2 to 3 times and mixed with A solution, and added to the mixed suspension of spores and nano-tin dioxide.

[0038] like Figure 6 The CaCO3 deposition activity of spores is an important indicator to measure the efficiency of calcium carbonate deposition of spores, which can reflect the mineralization of spores in concrete. It can be seen from the figure that the addition of nano-tin dioxide particles significantly improves the mineralization ability of spores. Figure 7 As shown, the crack repair situation; Figure 8 As shown in Figure 2, the concrete crack repair rate is Fig. 9 The porosity test results of concrete are shown in the figure; C is the control group, without spores and nanoparticles; N contains only nanoparticles; S contains only spores; SN contains spores and nanoparticles. It can be seen that the SN group repairs concrete cracks better and more completely. It can also partially repair concrete with 5mm cracks.

[0039] The present invention promotes the growth of bacteria and improves the self-repairing ability of concrete through a protective carrier environment, which is conducive to improving the survival rate of bacteria in concrete. In traditional methods, bacteria are easily damaged or even die in the harsh process of concrete preparation and hardening. Using tin dioxide nanoparticles as carriers can effectively protect bacteria from shear force, extrusion and high alkaline environment, significantly improving the survival rate of bacteria in concrete. Secondly, the self-repairing ability of concrete is enhanced. When concrete cracks, the bacteria protected in the tin dioxide nanoparticles will be activated, thereby inducing calcium carbonate precipitation to seal the cracks. Compared with traditional chemical and polymer sealants, this method is more environmentally friendly, economical and durable. At the same time, it can also improve the durability of concrete. The calcium carbonate generated by the biomineralization process can not only seal cracks, but also enhance the structural stability of concrete and improve its durability. This self-repairing process can be repeated, so that the concrete structure can maintain a good state for a long time. A significant advantage of using nanomaterials as carriers is that it does not reduce the mechanical strength of the concrete itself. On the contrary, due to the small size and high specific surface area of ​​nanomaterials, they can be better dispersed in concrete, which helps to maintain or even improve the overall performance of concrete.

[0040] All technical solutions that fall within the principle of the present invention fall within the protection scope of the present invention. For those skilled in the art, several improvements made without departing from the principle of the present invention should also be considered as falling within the protection scope of the present invention.

Claims

1. A method for applying nanoparticle-coated microorganisms in self-repair of concrete cracks, characterized in that: The microorganism is Bacillus sp. B6 (CGMCC 13360), and the nanoparticle carrier is nano-tin dioxide particles; the method is applied to concrete repair through the following steps: Step 1, prepare nutrient cells and prepare solid culture medium; add 15g / L agar powder to LB culture medium, place in a 30°C constant temperature incubator for culturing for 1 day, and keep at a constant temperature of 4°C; Step 2, preparing spores: using a culture medium method, inoculating Bacillus sp. B6 into a culture medium of LB medium, then transferring it to a culture medium of MSP medium for promoting spore formation, fermenting and centrifuging, and resuspending the spore precipitate after centrifugation with deionized water to a concentration of about 5×10 8 The spore suspension of 1000 g / mL was kept at a constant temperature of 4°C; Step 3, dilute the spores and select qualified bacterial concentrations; dilute the selected spores prepared in step 2 to 1×10 7 After fixation and drying, a bacterial counting plate was used to observe the spore morphology and count the number of spores. Step 4, preparing nanoparticles, selecting nano-tin dioxide particles; the size is 20-40nm, and the purity is 99.9%; Step 5, combining spores and nanomaterials; concentrating the spores in the qualified spore culture medium to 2.5×10 9 / mL, and combine qualified nano-tin dioxide particles with spores to form a mixed suspension; Step 6, prepare self-repairing beads, add the mixed suspension to MCC microcrystalline cellulose powder and stir to form a ball, take out the ball, make a ball with a diameter of 4 mm, place the ball in a culture dish, and dry it in an incubator at 37°C to obtain self-repairing agent microspheres for repairing concrete.

2. The method for applying the nanoparticle-coated microorganisms in self-repairing concrete cracks according to claim 1, characterized in that: The formula of the LB culture medium is (g / L): 5 g yeast powder, 10 g tryptone, 0.84 g NaHCO3, 9.54 g Na2CO3, and the pH value of the culture medium is 9.

7.

3. The method for applying the nanoparticle-coated microorganisms in self-repairing concrete cracks according to claim 1, characterized in that: The formula of the MSP culture medium is (g / L): 0.3 g of NH4NO3, 0.02 g of KH2PO4, 0.225 g of CaCl2·2H2O, 0.476 g of KCl, 0.2 g of MgCl2·6H2O, 0.01 g of MnSO4·2H2O, 3 g of yeast powder, 1 g of soluble starch, 4.2 g of NaHCO3, and 5.3 g of Na2CO3, and the pH value of the culture medium is 9.

7.

4. The method for applying nanoparticle-coated microorganisms in concrete crack self-repair according to claim 1, characterized in that: In the step 2, before transferring to the MSP medium, the LB medium was placed in a shaker at 30° C. and 150 rpm for constant temperature shaking culture for about 18 hours.

5. The method for applying nanoparticle-coated microorganisms in concrete crack self-repair according to claim 1, characterized in that: In the step 6, CHL nutrient solution is added to improve the growth reliability of spores, and the CHL nutrient solution is prepared in the following amount per 50 mL: 20 mL of A solution: 2.38 g of KNO3, 0.0075 g of KH2PO4, 0.325 g of MgSO4, and 1.25 g of inosine, and the pH is adjusted to 12.0 with 6M NaOH after dissolution; 20 mL of B solution: 10 g of starch is dissolved in 20 mL of water, stirred into a paste, and then mixed evenly with 10 mL of boiling water, and then repeatedly boiled 2-3 times in a microwave oven, mixed with A solution, and added to the mixed suspension of spores and nano-tin dioxide.