Nanometer precipitation strengthening high-entropy alloy with wide temperature range and stable phase structure and preparation method of nanometer precipitation strengthening high-entropy alloy
By designing Ni42.9Co20Fe10Cr13Al9Nb3Ti2-xTaxB0.1 nano precipitation high-entropy alloy and adopting an optimized heat treatment process, the problem of phase structure instability of traditional high-temperature alloys at high temperatures is solved, and high strength and toughness and high yield strength over a wide temperature range are achieved. Suitable for high temperature applications.
Patent Information
- Application Number
- CN202411029012.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-30
AI Technical Summary
The phase structure of traditional high-temperature alloys is unstable at high temperatures of 800 °C and above, and the volume content of the reinforced phase is relatively small, making it difficult to maintain high strength and toughness within a wide temperature range.
A high-strength toughened wide temperature domain phase structure is designed. Through phase diagram calculation and experiment, the components of Ni42.9Co20Fe10Cr13Al9Nb3Ti2-xTaxB0.1 were used, and the heat treatment process is optimized, such as two-step aging treatment, and prepared Nano-precipitated high-entropy alloys with FCC and L12 phase structures are produced to ensure stable phase structure and high strength and toughness.
Maintaining a volume content of more than 50% of the enhanced phase within a temperature range of above 710°C, with high yield strength and good plastic deformation capabilities, and is suitable for high temperature applications.
Smart Images

Figure CN118979183A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a new material alloy and a preparation method thereof, and in particular to a nano-precipitation strengthened high-entropy alloy with high strength, toughness, wide temperature range and stable phase structure and a preparation method thereof, and belongs to the field of material processing. Background Art
[0002] High-temperature materials are mostly used in the aerospace field, such as aircraft engine turbine disks, blades, rings, elastic elements, sealing elements, rocket nozzles, turbine rotors, and high-temperature devices such as supersonic aircraft leading edges. The most widely used high-temperature metal materials currently include: cobalt-based high-temperature alloys, iron-based high-temperature alloys, and nickel-based high-temperature alloys. The traditional Inconel 718 alloy nickel-based forged high-temperature alloy is widely used in temperature-bearing parts such as turbine disks due to its excellent fatigue resistance, radiation resistance, oxidation resistance, corrosion resistance, and good processing and welding properties. However, its temperature range is often below 650 ℃. By adding nearly 10% of Co elements, the In718Plus alloy prepared is a new type of nickel-based high-temperature alloy, which increases its temperature bearing capacity to 700 ℃. In718Plus has become a new generation of deformable high-temperature alloy turbine disk materials. In order to further improve its service range, Udimet 720Li adds more ~ 15at. % Co elements to improve its temperature range, so the service range of this type of alloy can cover between 650°C-800°C. It can be seen that increasing the Co content can improve its temperature bearing capacity and stable phase structure. A higher Co content helps to accommodate complex elements while maintaining a stable phase structure. This is because the Co element has a higher melting point and can replace the Ni element equivalently.
[0003] In order to provide high-temperature turbine disk components that can adapt to higher service temperatures, it is urgent to develop a new type of nano-precipitation strengthened high-temperature high-entropy alloy. This type of high-temperature alloy must have the characteristics of stable phase structure and high strength and toughness over a wide temperature range. Summary of the invention
[0004] In view of the problems of phase structure instability and low volume content of strengthening phase in traditional high-temperature alloys when they are in long-term service at high temperatures of 800°C and above, the present invention provides a nano-precipitation-strengthened high-entropy alloy with high strength and toughness and stable phase structure over a wide temperature range and a preparation method thereof, thereby obtaining a high-entropy alloy with high strength and toughness. The present invention provides a multi-principal-element nano-precipitation-strengthened alloy and a preparation method thereof.
[0005] The present invention designs a nano-precipitation-strengthened high-entropy alloy with high temperature and wide temperature range and stable phase structure by combining phase diagram calculation with experiments. The alloy designed by the present invention has high strength and toughness, and only FCC and L12 phases exist in the temperature range above 710 ℃, the phase structure is stable, and the volume content of the reinforcement phase can still be maintained at more than 50% after long-term treatment at 800 ℃. Compared with other nano-precipitation high-entropy alloys and most traditional high-temperature alloys, the volume fraction of the precipitation phase is better, so it is very suitable for high-temperature applications. In addition, by optimizing the heat treatment process and adopting a double-step aging treatment, a bimodal structure nano-precipitation-strengthened high-entropy alloy with higher yield strength can be prepared.
[0006] The present invention provides a nano-precipitation strengthened high entropy alloy with high strength, toughness, wide temperature range and stable phase structure, wherein the alloy comprises Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti 2-x Ta x B 0.1 , 2 ≥ x ≥ 0, the microstructure is an equiaxed crystal structure accompanied by nano-precipitation strengthening phase, and the nano-precipitated particles maintain a coherent relationship with the matrix.
[0007] Furthermore, the mass fraction of Ni, Co, Fe, Cr, Al, Ti, Nb, Ta and B smelting raw materials used in the alloy is not less than 99.9%.
[0008] The present invention provides a method for preparing the above-mentioned nano-precipitation-strengthened high-entropy alloy with a stable phase structure in a wide temperature range, comprising the following steps: preparing a multi-principal alloy ingot by smelting raw materials of Ni, Co, Fe, Cr, Al, Ti, Nb, Ta and B; subjecting the multi-principal alloy ingot to a homogenization heat treatment at 1150-1200°C, and then sequentially subjecting the ingot to a cold rolling with a total deformation of 60-65%, a partial recrystallization heat treatment at 1200°C for 0.5-2min, and then an aging heat treatment at 800°C for 12-24h to prepare the above-mentioned alloy.
[0009] The above-mentioned preparation method specifically comprises the following steps: Step 1: Weighing: Using an electronic balance with an accuracy of 0.0001g, weigh and proportion the raw material particles of Ni, Co, Fe, Cr, Al, Nb, Ti, Ta and B with a purity of ≥99.9 wt.% in a molar ratio of 42.9:20:10:13:9:3:2-x:x:0.1 to obtain a nominal composition of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti 2-x Tax B 0.1 , alloy mixed particles with 2 ≥ x ≥ 0; The weighed raw material particles were placed in a beaker, ultrasonically cleaned for 5 minutes, and then dried with a hair dryer; Step 2: Melting: Use WK-II non-consumable vacuum arc furnace under argon protection to melt the weighed Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti 2-x Ta x B 0.1 The alloy mixed particles are first melted into alloy ingots, and the melting-flipping-melting process is repeated more than 5 times to ensure uniform distribution of alloy elements; Step 3: Casting: The uniformly smelted alloy ingot is placed on a water-cooled crucible with a casting mold by a robotic arm. There is circulating water under the crucible. Then, the uniformly smelted alloy is heated to a molten state, and the molten metal liquid is cast into a 5×10×40mm water-cooled copper mold. After the sample is cooled, the sample is taken out; Step 4: Thermomechanical treatment: The melted samples are subjected to homogenization heat treatment at 1150-1200 °C / 2h, followed by cold rolling with a reduction of 60-65%. After cold rolling, the samples are recrystallized at 1200 °C for 0.5-2min, followed by aging treatment at 800 °C for 12-24h to prepare an alloy with high strength and a stable phase structure in a wide temperature range.
[0010] As a preferred solution, the preparation method of the high entropy alloy is further optimized as follows: According to the above steps 1 to 3, Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti 2-x Ta x B 0.1 , 2 ≥ x ≥ 0 high entropy alloy ingots, and then perform thermomechanical treatment. The specific process of the thermomechanical treatment is: the smelted sample is subjected to homogenization heat treatment at 1150-1200 ℃ / 2h, followed by cold rolling with 60-65% reduction. After cold rolling, the samples are recrystallized at 1200 ℃ for 0.5~ 2min to obtain recrystallized samples with different grain sizes, followed by cold rolling with 50% reduction. After cold rolling, the samples are recrystallized at 1080 ℃ for 2min, and then aged at 800 ℃ for 12-24h to prepare nano-precipitation strengthened high entropy alloys with higher strength (yield strength of 1200-1500 MPa).
[0011] Beneficial effects of the present invention: (1) Ni prepared by the present invention 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti 2-x Ta x B 0.1 , 2 ≥ x ≥ 0 nano-precipitated high entropy alloy, with high volume content of high temperature strengthening phase, stable phase structure, strong toughness, etc., is a single FCC+L12 phase structure, uniform metallographic structure, not only has high yield strength (>1134.5 MPa), but also has good plastic deformation (>20%), and significant work hardening performance; (2) By optimizing the thermomechanical treatment process, a double-step aging method was used to obtain Ni with a double-peak structure 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti 2-x Ta x B 0.1 Nano-precipitated high entropy alloys have the characteristics of higher stability, stable phase structure, high strength and toughness. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 Example 1 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti2B 0.1 XRD spectrum and phase diagram of Figure 2 Example 1 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti2B 0.1 EBSD organization diagram; Figure 3 Example 1 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti2B 0.1 Engineering stress-strain curve diagram; Figure 4 Example 2 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti1Ta1B 0.1 XRD patterns and EBSD organization diagrams; Figure 5 Example 2 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti1Ta1B 0.1 Engineering stress-strain curve diagram; Figure 6 Example 3 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 XRD spectrum and phase diagram of Figure 7 Example 3 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 EBSD organization diagram; Figure 8 Example 3 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 Engineering stress-strain curve diagram; Fig. 9 Example 4 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 EBSD diffraction band contrast images of nano-precipitated high entropy alloys after rolling and recrystallization treatment at 1200 °C for (a) 30 s and (b) 2 min, followed by subsequent cold rolling and double-step aging treatment; Fig.10 Example 4 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 After rolling, the nano-precipitated high entropy alloy was annealed at 1200 °C for (a) 30 s and (b) 2 min, and then cold rolled and subjected to double-step aging treatment at room temperature with a strain rate of 1×10 -3 / s tensile engineering stress-strain curve spectrum. DETAILED DESCRIPTION
[0013] The present invention is further illustrated by the following examples, but is not limited to the following examples.
[0014] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention. Example 1
[0015] This embodiment provides an ultra-high toughness nano-precipitation strengthened high entropy alloy composition with a wide temperature range and stable phase structure. The alloy composition components are Ni, Co, Fe, Cr, Al, Nb, Ti and B, wherein the ratio of each element is: the molar ratio of Ni, Co, Fe, Cr, Al, Nb, Ti and B is 42.9, 20, 10, 13, 9, 3, 2, 0.1, that is, Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti2B 0.1 .
[0016] The preparation steps of the above high entropy alloy are as follows: Step 1: Weighing: Use an electronic balance with an accuracy of 0.0001g to weigh the raw material particles of Ni, Co, Fe, Cr, Al, Nb, Ti, and B with a purity of ≥99.95% according to the molar ratio of 42.9, 20, 10, 13, 9, 3, 2, and 0.1. 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti2B 0.1 The raw materials were placed in a beaker containing anhydrous ethanol and ultrasonically cleaned for about 5 minutes to remove impurities and dirt on the surface, and then dried with a hair dryer.
[0017] Step 2: Melting: In an argon atmosphere, melt the weighed and proportioned elements into alloy ingots, and repeat the melting-flipping-melting process for more than 5 times to ensure uniform distribution of the alloy elements.
[0018] Step 3: Casting: Heat the uniformly smelted alloy to a molten state and cast it into a 5×10×40mm 3 After the sample has cooled down, take it out.
[0019] Step 4: Heat treatment: The smelted sample was subjected to homogenization heat treatment at 1200 °C / 2 h, followed by cold rolling with a 60% reduction. After cold rolling, the sample was recrystallized at 1200 °C for 2 min, and then aged at 800 °C for 12 h. 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti2B 0.1Nano-precipitation strengthened alloys.
[0020] Figure 1 a and b are Ni prepared in Example 1 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti2B 0.1 The XRD spectrum and phase diagram show that the alloy has a FCC+L12 structure. Figure 2 Example 1 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti2B 0.1 The EBSD microstructure diagram shows that the alloy has an equiaxed crystal structure. Figure 3 The Ni prepared in Example 1 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti2B 0.1 Engineering stress-strain curve of the alloy. The alloy has a yield strength of 1050 MPa and a high room temperature ductility of 23.1%. Example 2
[0021] This embodiment provides an ultra-high toughness nano-precipitation strengthened high entropy alloy composition with a wide temperature range and stable phase structure. The alloy composition components are Ni, Co, Fe, Cr, Al, Nb, Ta, Ti and B, wherein the ratio of each element is: the molar ratio of Ni, Co, Fe, Cr, Al, Nb, Ta, Ti and B is 42.9, 20, 10, 13, 9, 3, 1, 1, 0.1, that is, Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta1Ti1B 0.1 .
[0022] The preparation steps of the above high entropy alloy are as follows: Step 1: Weighing: Use an electronic balance with an accuracy of 0.0001g to weigh the raw material particles of Ni, Co, Fe, Cr, Al, Nb, Ta, Ti, and B with a purity of ≥99.95% according to the molar ratio of 42.9, 20, 10, 13, 9, 3, 1, 1, and 0.1. 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta1Ti1B 0.1The raw materials were placed in a beaker containing anhydrous ethanol and ultrasonically cleaned for about 5 minutes to remove impurities and dirt on the surface, and then dried with a hair dryer.
[0023] Step 2: Melting: In an argon atmosphere, melt the weighed and proportioned elements into alloy ingots, and repeat the melting-flipping-melting process for more than 5 times to ensure uniform distribution of the alloy elements.
[0024] Step 3: Casting: Heat the uniformly smelted alloy to a molten state and cast it into a 5×10×40mm 3 After the sample has cooled down, take it out.
[0025] Step 4: Heat treatment: The smelted sample was subjected to homogenization heat treatment at 1200 °C / 2h, followed by cold rolling with a 60% reduction. After cold rolling, the sample was recrystallized at 1200 °C for 2 min, and then aged at 800 °C for 12h. 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta1Ti1B 0.1 Nano-precipitation strengthened alloys.
[0026] Figure 4 The Ni prepared in Example 2 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta1Ti1B 0.1 The XRD spectrum and EBSD organization diagram show that the alloy has FCC+L12 structure. Figure 5 Example 2 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta1Ti1B 0.1 Engineering stress-strain curve. The alloy has a yield strength of 1080 MPa and a high room temperature ductility of 25.3%. Example 3
[0027] This embodiment provides a nano-precipitation-strengthened high-entropy alloy composition with ultra-high room temperature toughness. The alloy composition components are Ni, Co, Fe, Cr, Al, Nb, Ta and B, wherein the ratio of each element is: the molar ratio of Ni, Co, Fe, Cr, Al, Nb, Ta and B is 42.9, 20, 10, 13, 9, 3, 2, 0.1, that is, Ni 42.9 Co 20 Fe 10 Cr 13Al9Nb3Ta2B 0.1 .
[0028] The preparation steps of the above high entropy alloy are as follows: Step 1: Weighing: Use an electronic balance with an accuracy of 0.0001g to weigh the raw material particles of Ni, Co, Fe, Cr, Al, Nb, Ta, and B with a purity of ≥99.95% according to the molar ratio of 42.9, 20, 10, 13, 9, 3, 2, and 0.1. 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 The raw materials were placed in a beaker containing anhydrous ethanol and ultrasonically cleaned for about 5 minutes to remove impurities and dirt on the surface, and then dried with a hair dryer.
[0029] Step 2: Melting: In an argon atmosphere, melt the weighed and proportioned elements into alloy ingots, and repeat the melting-flipping-melting process for more than 5 times to ensure uniform distribution of the alloy elements.
[0030] Step 3: Casting: Heat the uniformly smelted alloy to a molten state and cast it into a 5×10×40mm 3 After the sample has cooled down, take it out.
[0031] Step 4: Heat treatment: The smelted sample was subjected to homogenization heat treatment at 1200 °C / 2h, followed by cold rolling with a 60% reduction. After cold rolling, the sample was recrystallized at 1200 °C for 2 min, followed by aging treatment at 800 °C. 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 Nano-precipitation strengthened alloys.
[0032] Figure 6 Example 3 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 The XRD spectrum and phase diagram show that the alloy has a FCC+L12 dual-phase structure. Figure 7 Example 3 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 The EBSD microstructure diagram shows that the alloy has an equiaxed crystal structure. Figure 8 Example 3 Preparation of Ni42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 Engineering stress-strain curve of the alloy. The alloy has a yield strength of 1143MPa and maintains an ultra-high room temperature ductility of 23.8%. Example 4
[0033] This embodiment provides a nano-precipitated high entropy alloy composition with ultra-high room temperature tensile strength and ductility having a heterogeneous structure. The alloy composition components are Ni, Co, Fe, Cr, Al, Nb, Ta and B, wherein the ratio of each element is: the molar ratio of Ni, Co, Fe, Cr, Al, Nb, Ta and B is 42.9, 20, 10, 13, 9, 3, 2, 0.1, i.e., Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 .
[0034] The preparation steps of the above high entropy alloy are as follows: Step 1: Weighing: Use an electronic balance with an accuracy of 0.0001g to weigh the raw material particles of Ni, Co, Fe, Cr, Al, Nb, Ta, and B with a purity of ≥99.95% according to the molar ratio of 42.9, 20, 10, 13, 9, 3, 2, and 0.1. 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 The raw materials were placed in a beaker containing anhydrous ethanol and ultrasonically cleaned for about 5 minutes to remove impurities and dirt on the surface, and then dried with a hair dryer.
[0035] Step 2: Melting: In an argon atmosphere, melt the weighed and proportioned elements into alloy ingots, and repeat the melting-flipping-melting process for more than 5 times to ensure uniform distribution of the alloy elements.
[0036] Step 3: Casting: Heat the uniformly smelted alloy to a molten state and cast it into a 5×10×40mm 3 After the sample has cooled down, take it out.
[0037] Step 4: Heat treatment: The smelted samples were subjected to homogenization heat treatment at 1200 °C / 2h, followed by cold rolling with a 60% reduction. 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B0.1 Double-step aging heat treatment was performed to obtain a nano-precipitated high-entropy alloy with a finer grain size. The specific implementation method is: the sample after cold rolling was recrystallized at 1200 ° C for 30 s and 2 min respectively to obtain recrystallized samples with different grain sizes, followed by cold rolling with a 50% reduction, and the sample after cold rolling was recrystallized at 1080 ° C for 2 min, followed by aging treatment at 800 ° C for 12 h, which can prepare a heterogeneous structure nano-precipitation strengthened high-entropy alloy with higher strength.
[0038] Fig. 9 Example 4 Preparation of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 EBSD diffraction band contrast images of the nano-precipitated high entropy alloy after rolling, recrystallization treatment at 1200 °C for (a) 30 s and (b) 2 min, followed by rolling by 50%, annealing at 1080 °C for 2 min and aging at 800 °C for 12 h. The images show that the alloy has a heterogeneous structure and also has some equiaxed crystal morphology.
[0039] Fig.10 Example 4 Preparation of heterostructure Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ta2B 0.1 The strain rate of high entropy alloy after rolling, annealing at 1200 ℃ for (a) 30 s and (b) 2 min, and cold rolling and double-step aging at room temperature was 1×10 -3 / s tensile engineering stress-strain curve spectrum. It can be seen from the figure that the yield strength of the heterogeneous structure nano-precipitation high entropy alloy after rolling is 1480 and 1288 MPa, and the plasticity reaches more than 10%.
Claims
1. A nano-precipitation strengthened high entropy alloy with a stable phase structure over a wide temperature range, characterized in that: The alloy composition is Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti 2-x Ta x B 0.1 , 2 ≥ x ≥ 0, the molar ratio of each element Ni, Co, Fe, Cr, Al, Nb, Ti, Ta and B is 42.9∶20∶10∶13∶9∶3∶2-x∶x∶0.1, the alloy microstructure is an equiaxed crystal structure accompanied by a nano-precipitation strengthening phase, and the nano-precipitated particles maintain a coherent relationship with the matrix.
2. The nano-precipitation strengthened high entropy alloy with stable phase structure over a wide temperature range according to claim 1, characterized in that: The mass fraction of Ni, Co, Fe, Cr, Al, Ti, Nb, Ta and B smelting raw materials used in the alloy is not less than 99.9%.
3. A method for preparing a nano-precipitation-strengthened high-entropy alloy with a stable phase structure over a wide temperature range as claimed in claim 1 or 2, characterized in that The following steps are involved: A multi-principal alloy ingot is prepared using Ni, Co, Fe, Cr, Al, Ti, Nb, Ta and B smelting raw materials; the multi-principal alloy ingot is subjected to homogenization heat treatment at 1150-1200 ℃, and then sequentially subjected to cold rolling with a total deformation of 60-65%, partial recrystallization heat treatment at 1200 ℃ for 0.5-2 min, and then aging heat treatment at 800 ℃ for 12-24 h to prepare the above alloy.
4. The method for preparing a nano-precipitation-strengthened high-entropy alloy with a stable phase structure over a wide temperature range according to claim 3, characterized in that The specific steps include: Step 1: Weighing: Using an electronic balance with an accuracy of 0.0001g, weigh and proportion the raw material particles of Ni, Co, Fe, Cr, Al, Nb, Ti, Ta and B with a purity of ≥99.9 wt.% in a molar ratio of 42.9:20:10:13:9:3:2-x:x:0.1 to obtain a nominal composition of Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti 2-x Ta x B 0.1 , alloy mixed particles with 2 ≥ x ≥ 0; The weighed raw material particles were placed in a beaker, ultrasonically cleaned for 5 minutes, and then dried with a hair dryer; Step 2: Melting: Use WK-II non-consumable vacuum arc furnace under argon protection to melt the weighed Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti 2-x Ta x B 0.1 The alloy mixed particles are first melted into alloy ingots, and the melting-flipping-melting process is repeated more than 5 times to ensure uniform distribution of alloy elements; Step 3: Casting: The uniformly smelted alloy ingot is placed on a water-cooled crucible with a casting mold by a robotic arm. There is circulating water under the crucible. Then, the uniformly smelted alloy is heated to a molten state, and the molten metal liquid is cast into a 5×10×40mm 3 After the sample is cooled, take it out; Step 4: Thermomechanical treatment: The melted samples are subjected to homogenization heat treatment at 1150-1200 °C / 2h, followed by cold rolling with a reduction of 60-65%. After cold rolling, the samples are recrystallized at 1200 °C for 0.5-2min, followed by aging treatment at 800 °C for 12-24h to prepare an alloy with high strength and a stable phase structure in a wide temperature range.
5. The method for preparing a nano-precipitation-strengthened high-entropy alloy with a stable phase structure over a wide temperature range according to claim 4, characterized in that: According to steps 1 to 3, first prepare Ni 42.9 Co 20 Fe 10 Cr 13 Al9Nb3Ti 2-x Ta x B 0.1 , 2 ≥ x ≥ 0 high entropy alloy ingots, and then perform thermomechanical treatment. The specific process of the thermomechanical treatment is: the smelted sample is subjected to homogenization heat treatment at 1150-1200 ℃ / 2h, followed by cold rolling with a reduction of 60-65%. After cold rolling, the samples are recrystallized at 1200 ℃ for 0.5 ~ 2min to obtain recrystallized samples with different grain sizes, followed by cold rolling with a reduction of 50%. After cold rolling, the samples are recrystallized at 1080 ℃ for 2min, and then aged at 800 ℃ for 12h~24h to prepare a nano-precipitation strengthened high entropy alloy with higher strength.
Citation Information
Patent Citations
High-temperature alloy with low content of cobalt and nickel
CN101130844A
High-entropy alloy with dispersion nano-sized precipitate strengthening effect and preparing method thereof
CN104694808A
BCC-based high-strength, high-entropy and high-temperature alloy for coherent precipitation of cubic nano particles
CN107557645A
Nanometer ultra-fine grain high-entropy alloy and preparation method thereof
CN107893184A
Precipitation strengthening type high-entropy alloy and preparation process thereof
CN111139391A
Cited By
Necklace-shaped heterostructure high-entropy alloy and preparation method thereof
CN119776711A