Tin-plated copper wire production process capable of preventing tin-plated layer from falling off
Through modified rosin resin flux and high-temperature annealing treatment, the problem of tin-plated copper wire falling off is solved, the adhesion of the tin layer and the mechanical strength of the copper wire are improved, and the service life of the product is extended.
Patent Information
- Application Number
- CN202411069255.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-06
AI Technical Summary
In the existing production process of tin-plating copper wire, the tin-plating layer is prone to fall off, which affects the product's usage effect and life. The activity of traditional rosin resin flux is weak, resulting in poor surface treatment capacity of copper wire.
Modified rosin resin flux is used to combine with epoxy resin through hydrogenated rosin resin, and acrylic monomer and 2-mercaptobenzimidazole are added to prepare modified rosin resin through click chemical reaction, which is used in flux, combined with high temperature annealing. and tin plating to enhance the adhesion of the tin layer.
It significantly improves the adhesion of the tin-plated layer, enhances the mechanical strength of the copper wire, avoids the tin-plated layer falling off, extends the service life of the product, and improves the tin-plated effect.
Smart Images

Figure BDA0004980346520000071
Abstract
Description
Technical Field
[0001] The invention relates to a field, and in particular to a production process of tinned copper wire which can prevent the tinned layer from falling off. Background Art
[0002] Copper has excellent electrical conductivity, thermal conductivity and chemical stability and is widely used in industry and daily life. Tinned copper wire refers to copper wire with a thin layer of metal tin plated on the surface of the copper wire. Tinned copper wire is relatively soft and has good electrical conductivity. Compared with bare copper wire, it has stronger corrosion resistance and oxidation resistance, which can greatly extend the service life of weak current cables. Tinning of copper wire can prevent the insulating rubber from becoming sticky, the wire core from becoming black and brittle, and improve its solderability. Tinned copper wire is mainly used as the conductive core of rubber-insulated mining cables, soft wires, soft cables and marine cables, as well as the outer braiding layer and brush wire of the cable.
[0003] Tinned copper wire has many excellent properties, and its processing technology is simple, but the process flow is relatively large. At present, the production of tinned copper wire in my country's cable industry mainly includes chemical tinning and physical tinning. During the physical tinning process, there is a very thin oxide layer on the surface of the copper wire after annealing. Direct tinning will cause uneven tinning, frequent wire breakage during tinning, and copper leakage of tinned copper wire. Therefore, before entering the tin furnace, it must be cleaned with appropriate pickling liquid (flux) to ensure good adhesion between the tin layer and the copper wire. It can be said that pickling directly affects the tinning effect and product performance of tinned copper wire, and is one of the important links in the production of tinned copper wire. If it is not properly controlled, it will cause the surface tinning layer to have poor adhesion and easy to fall off, which will affect the use effect and service life of the product, thereby affecting the production quality of tinned copper wire. Summary of the invention
[0004] In view of the problems existing in the prior art, the object of the present invention is to provide a production process for tinned copper wire which can prevent the tinned layer from falling off.
[0005] The purpose of the present invention is achieved by the following technical solutions:
[0006] A production process for tinned copper wire to prevent the tinning layer from falling off comprises the following steps:
[0007] Step 1: Material preparation:
[0008] Choose pure copper wire and anneal it in a high-temperature furnace;
[0009] Step 2: Pre-treatment:
[0010] The annealed copper wire is immersed in the flux and then placed in an oven for drying to obtain the pre-treated copper wire;
[0011] Step 3: Tinning:
[0012] Placing the pretreated copper wire in a tinning furnace for tinning to obtain the pretreated tinned copper wire;
[0013] Step 4: Post-processing:
[0014] The pretreated tinned copper wire is placed in clean water again to wash away impurities, and then vacuum dried to obtain the tinned copper wire.
[0015] Preferably, in step 1, the purity of the copper wire is ≥99.99% and the diameter is 0.15-0.25 mm.
[0016] Preferably, in step 1, the annealing treatment is performed at a temperature of 650-720° C. and for a time of 1-2 h.
[0017] Preferably, in step 2, during the process of the annealed copper wire being infiltrated in the flux, the surface of the copper wire is completely covered with the flux.
[0018] Preferably, in step 2, the temperature in the oven is 80-90° C., and the drying time is 1-2 hours.
[0019] Preferably, in step 3, the temperature in the tinning furnace is 230-250° C., and the residence time is 2-5 s.
[0020] Preferably, the components of the soldering flux in step 2 are calculated by weight and include:
[0021] 40-60 parts of modified rosin resin, 16-20 parts of lubricant, 12-18 parts of metal chloride, 3-8 parts of dispersant and 10-20 parts of solvent.
[0022] Preferably, the metal chloride salt is one or more combinations of zinc chloride, magnesium chloride, samarium chloride and sodium chloride.
[0023] Preferably, the lubricant is hexadecanoic acid or octadecanoic acid.
[0024] Preferably, the dispersant is ethylene glycol butyl ether or propylene glycol butyl ether.
[0025] Preferably, the solvent is one of isopropanol, toluene and ethyl acetate.
[0026] Preferably, the preparation method of the modified rosin resin comprises:
[0027] S1, weigh hydrogenated rosin resin and epoxy resin, mix them, add a catalyst, heat them to 80-100°C under the protection of nitrogen, stir and react for 3-6 hours, add acrylic acid monomer, continue to react for 2-5 hours, end the reaction, cool to room temperature, and obtain acrylic rosin resin;
[0028] S2. Mix the acrylic rosin resin and anhydrous ethanol, add 2-mercaptobenzimidazole, stir well until uniform, then add a photoinitiator, react under ultraviolet light at room temperature, stir for 2-4 hours, and remove the ethanol under reduced pressure after the reaction to obtain a modified rosin resin.
[0029] Preferably, in S1, the hydrogenated rosin resin has an acid value of 10 mgKOH / g and a softening point of 86°C.
[0030] Preferably, in S1, the epoxy value of the epoxy resin is 0.132eq / 100g, the softening point is 88°C, and the density is 1.18g / cm 3 .
[0031] Preferably, in S1, the catalyst is tetramethylammonium hydroxide with a purity of >98%.
[0032] Preferably, in S1, the amount of catalyst added is 3%-8% of the mass of the hydrogenated rosin resin.
[0033] Preferably, in S1, the mass ratio of hydrogenated rosin resin, epoxy resin and acrylic monomer is 1:3.5-4.2:0.63-0.96.
[0034] Preferably, in S2, the mass ratio of acrylic rosin resin, 2-mercaptobenzimidazole and anhydrous ethanol is 1:0.31-0.62:4-6.
[0035] Preferably, in S2, the photoinitiator is benzoin ethyl ether, and the added amount is 2%-8% of the mass of the acrylic rosin resin.
[0036] Preferably, in S2, the wavelength of the ultraviolet light is 365nm and the power is 50W.
[0037] Preferably, the soldering flux is prepared by mixing various raw materials and stirring them evenly.
[0038] The beneficial effects of the present invention are:
[0039] 1. The present invention provides a production process for tinned copper wire. In the process, the copper wire is first annealed to make it soft and eliminate internal residual stress. Before tinning, the copper wire is treated with flux and then subjected to high-temperature tinning. Such operation can increase the adhesion of the tinned layer, avoid the subsequent tinned layer from falling off to a large extent, and improve the use effect and service life of the product.
[0040] 2. The soldering flux used in the present invention is improved on the basis of the traditional rosin soldering flux. The soldering flux prepared by the traditional rosin resin has weak activity and poor surface treatment ability for the copper wire. The present invention modifies the rosin resin so that after being applied to the soldering flux, the activity is enhanced, which not only improves the surface treatment ability for the copper wire, but also enhances the mechanical strength of the copper wire after tinning.
[0041] 3. The preparation process of the modified rosin resin of the present invention is to first combine hydrogenated rosin resin and epoxy resin, then add acrylic acid to graft them to obtain rosin acrylate, and then use the double bond group in the acrylic acid structure and the thiol group in 2-mercaptobenzimidazole to produce a thiol-double bond click chemistry reaction, thereby introducing a benzimidazole group to obtain the modified rosin resin. Compared with traditional rosin resin, the modified rosin resin prepared by the present invention has better cross-linking adhesion, which can make the solder paste better adhere to the copper wire, thereby achieving a good tinning effect.
[0042] 4. In addition, it was found through testing that the copper wire treated with the flux of the present invention has better mechanical strength performance after tinning. DETAILED DESCRIPTION
[0043] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0044] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0045] The present invention will be further described below in conjunction with the following examples.
[0046] Example 1
[0047] A production process for tinned copper wire to prevent the tinning layer from falling off comprises the following steps:
[0048] Step 1: Material preparation:
[0049] Choose pure copper wire with a purity of ≥99.99% and a diameter of 0.2 mm, and anneal it in a high-temperature furnace at a temperature of 680°C for 2 hours;
[0050] Step 2: Pre-treatment:
[0051] The annealed copper wire is immersed in the flux so that the surface of the copper wire is completely covered with the flux, and then placed in an oven for drying. The temperature in the oven is 85°C and the drying time is 1.5 hours, thus obtaining the pre-treated copper wire;
[0052] Step 3: Tinning:
[0053] The pretreated copper wire is placed in a tinning furnace, the temperature in the tinning furnace is 240°C, and the tinning treatment is performed for a residence time of 3.5 seconds, thereby obtaining the pretreated tinned copper wire;
[0054] Step 4: Post-processing:
[0055] The pretreated tinned copper wire is placed in clean water again to wash away impurities, and then vacuum dried to obtain the tinned copper wire.
[0056] The above-mentioned components of the flux are calculated by weight and include:
[0057] 50 parts of modified rosin resin, 18 parts of octadecanoic acid, 15 parts of zinc chloride, 5 parts of ethylene glycol butyl ether and 15 parts of isopropyl alcohol.
[0058] Wherein, the preparation method of the modified rosin resin comprises:
[0059] S1. Weigh hydrogenated rosin resin (acid value of hydrogenated rosin resin is 10 mgKOH / g, softening point is 86°C) and epoxy resin (epoxy value is 0.132 eq / 100 g, softening point is 88°C, density is 1.18 g / cm 3 ) were mixed, tetramethyl ammonium hydroxide (purity> 98%) was added as a catalyst, the amount of which was 5% of the mass of the hydrogenated rosin resin, the temperature was raised to 90°C under the protection of nitrogen, and the reaction was stirred for 5 hours, and then acrylic acid (C 3 H 4 O 2 ), the mass ratio of hydrogenated rosin resin, epoxy resin and acrylic acid monomer is 1:3.8:0.79, and the reaction is continued for 3 hours, and then the reaction is completed and the temperature is lowered to room temperature to obtain acrylic rosin resin;
[0060] S2. Mix acrylic rosin resin and anhydrous ethanol, add 2-mercaptobenzimidazole, the mass ratio of acrylic rosin resin, 2-mercaptobenzimidazole and anhydrous ethanol is 1:0.46:5, stir until uniform, then add benzoin ethyl ether as a photoinitiator, the added amount is 5% of the mass of the acrylic rosin resin, react under room temperature by irradiation with ultraviolet light, the wavelength of the ultraviolet light is 365nm, the power is 50W, stir the reaction for 3h, and remove the ethanol under reduced pressure after the reaction is completed to obtain a modified rosin resin.
[0061] The preparation of the flux is to mix the raw materials and stir them thoroughly before use.
[0062] Example 2
[0063] A production process for tinned copper wire to prevent the tinning layer from falling off comprises the following steps:
[0064] Step 1: Material preparation:
[0065] Choose pure copper wire with a purity of ≥99.99% and a diameter of 0.15 mm, and anneal it in a high-temperature furnace at a temperature of 650°C for 2 hours;
[0066] Step 2: Pre-treatment:
[0067] The annealed copper wire is immersed in the flux so that the surface of the copper wire is completely covered with the flux, and then placed in an oven for drying at a temperature of 80°C for 2 hours to obtain the pre-treated copper wire;
[0068] Step 3: Tinning:
[0069] The pretreated copper wire is placed in a tinning furnace, the temperature in the tinning furnace is 230°C, and the tinning treatment is performed for a residence time of 5 seconds, thereby obtaining the pretreated tinned copper wire;
[0070] Step 4: Post-processing:
[0071] The pretreated tinned copper wire is placed in clean water again to wash away impurities, and then vacuum dried to obtain the tinned copper wire.
[0072] The above-mentioned components of the flux are calculated by weight and include:
[0073] 40 parts of modified rosin resin, 16 parts of hexadecanoic acid, 12 parts of magnesium chloride, 3 parts of propylene glycol butyl ether and 10 parts of toluene.
[0074] Wherein, the preparation method of the modified rosin resin comprises:
[0075] S1. Weigh hydrogenated rosin resin (acid value of hydrogenated rosin resin is 10 mgKOH / g, softening point is 86°C) and epoxy resin (epoxy value is 0.132 eq / 100 g, softening point is 88°C, density is 1.18 g / cm 3 ) were mixed, tetramethyl ammonium hydroxide (purity> 98%) was added as a catalyst, the amount of which was 3% of the mass of the hydrogenated rosin resin, the temperature was raised to 80°C under the protection of nitrogen, and the reaction was stirred for 6 hours, and then acrylic acid (C 3 H 4 O 2 ), the mass ratio of hydrogenated rosin resin, epoxy resin and acrylic acid monomer is 1:3.5:0.63, and the reaction is continued for 2 hours, and then the reaction is completed and cooled to room temperature to obtain acrylic rosin resin;
[0076] S2. Mix acrylic rosin resin and anhydrous ethanol, add 2-mercaptobenzimidazole, the mass ratio of acrylic rosin resin, 2-mercaptobenzimidazole and anhydrous ethanol is 1:0.31:4, stir until uniform, then add benzoin ethyl ether as a photoinitiator, the added amount is 2% of the mass of the acrylic rosin resin, react under room temperature by irradiation with ultraviolet light, the wavelength of the ultraviolet light is 365nm, the power is 50W, stir the reaction for 2h, and remove the ethanol under reduced pressure after the reaction is completed to obtain a modified rosin resin.
[0077] The preparation of the flux is to mix the raw materials and stir them thoroughly before use.
[0078] Example 3
[0079] A production process for tinned copper wire to prevent the tinning layer from falling off comprises the following steps:
[0080] Step 1: Material preparation:
[0081] Choose pure copper wire with a purity of ≥99.99% and a diameter of 0.25 mm, and anneal it in a high-temperature furnace at a temperature of 720°C for 1 hour;
[0082] Step 2: Pre-treatment:
[0083] The annealed copper wire is immersed in the flux so that the surface of the copper wire is completely covered with the flux, and then placed in an oven for drying. The temperature in the oven is 90°C and the drying time is 1 hour, thus obtaining the pre-treated copper wire;
[0084] Step 3: Tinning:
[0085] The pre-treated copper wire is placed in a tinning furnace, the temperature in the tinning furnace is 250°C, and the tinning treatment is performed for a residence time of 2s, thereby obtaining the pre-treated tinned copper wire;
[0086] Step 4: Post-processing:
[0087] The pretreated tinned copper wire is placed in clean water again to wash away impurities, and then vacuum dried to obtain the tinned copper wire.
[0088] The above-mentioned components of the flux are calculated by weight and include:
[0089] 60 parts of modified rosin resin, 20 parts of octadecanoic acid, 18 parts of sodium chloride, 8 parts of propylene glycol butyl ether and 20 parts of ethyl acetate.
[0090] Wherein, the preparation method of the modified rosin resin comprises:
[0091] S1. Weigh hydrogenated rosin resin (acid value of hydrogenated rosin resin is 10 mgKOH / g, softening point is 86°C) and epoxy resin (epoxy value is 0.132 eq / 100 g, softening point is 88°C, density is 1.18 g / cm 3 ) were mixed, tetramethyl ammonium hydroxide (purity> 98%) was added as a catalyst, the amount of which was 8% of the mass of the hydrogenated rosin resin, the temperature was raised to 100°C under the protection of nitrogen, and the reaction was stirred for 3 hours, and then acrylic acid (C 3 H 4 O 2 ), the mass ratio of hydrogenated rosin resin, epoxy resin and acrylic acid monomer is 1:4.2:0.96, and the reaction is continued for 5 hours, and then the reaction is completed and cooled to room temperature to obtain acrylic rosin resin;
[0092] S2. Mix acrylic rosin resin and anhydrous ethanol, add 2-mercaptobenzimidazole, the mass ratio of acrylic rosin resin, 2-mercaptobenzimidazole and anhydrous ethanol is 1:0.62:6, stir until uniform, then add benzoin ethyl ether as a photoinitiator, the addition amount is 8% of the mass of the acrylic rosin resin, react under room temperature by irradiation with ultraviolet light, the wavelength of the ultraviolet light is 365nm, the power is 50W, stir the reaction for 4h, and remove the ethanol under reduced pressure after the reaction is completed to obtain a modified rosin resin.
[0093] The preparation of the flux is to mix the raw materials and stir them thoroughly before use.
[0094] Comparative Example 1
[0095] A production process for tinned copper wire, which is different from Example 1 in that the composition of the flux is different, and the modified rosin resin in the composition is replaced by hydrogenated rosin resin.
[0096] In this comparative example, the soldering flux is calculated by weight and includes:
[0097] 50 parts of hydrogenated rosin resin, 18 parts of octadecanoic acid, 15 parts of zinc chloride, 5 parts of ethylene glycol butyl ether and 15 parts of isopropyl alcohol.
[0098] Comparative Example 2
[0099] A production process for tinned copper wire, which differs from Example 1 in that the composition of the flux is different, and the modified rosin resin in the composition is replaced by acrylic rosin resin (preparation is the same as S1 in Example 1).
[0100] In this comparative example, the soldering flux is calculated by weight and includes:
[0101] 50 parts of acrylic rosin resin, 18 parts of octadecanoic acid, 15 parts of zinc chloride, 5 parts of ethylene glycol butyl ether and 15 parts of isopropyl alcohol.
[0102] Comparative Example 3
[0103] A production process for tinned copper wire, which is different from Example 1 in that the composition of the flux is different, and the modified rosin resin in the composition is replaced by a mixture of hydrogenated rosin resin and 2-mercaptobenzimidazole (the mass ratio of hydrogenated rosin resin to 2-mercaptobenzimidazole is 1:0.62).
[0104] In this comparative example, the soldering flux is calculated by weight and includes:
[0105] 50 parts of a mixture of hydrogenated rosin resin and 2-mercaptobenzimidazole, 18 parts of octadecanoic acid, 15 parts of zinc chloride, 5 parts of ethylene glycol butyl ether and 15 parts of isopropyl alcohol.
[0106] Experimental example
[0107] The tensile strength and elongation of the tinned copper wires prepared in Example 1 and Comparative Examples 1-3 were tested, and the surface of the copper wire was observed to see if the tin layer appeared. The tensile strength and elongation tests were based on GB / T 228.1-2021 "Tensile Test for Metallic Materials"; the adhesion test was based on GB / T 4909.11-2009 "Test Methods for Bare Wires".
[0108] Table 1 Test results of tinned copper wire produced by different treatment methods
[0109]
[0110] From the above test results, it can be seen that the tinned copper wire produced by the process of the present invention has higher mechanical strength, is not prone to tinning, and has better adhesion of the tin layer. Therefore, it can be shown that the production process of the present invention can prevent the tin layer from falling off and enhance the strength performance of the copper wire.
[0111] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0112] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A production process for tinned copper wire to prevent the tin coating from falling off, characterized in that: The following steps are involved: Step 1: Material preparation: Choose pure copper wire and anneal it in a high-temperature furnace; Step 2: Pre-treatment: The annealed copper wire is immersed in the flux and then placed in an oven for drying to obtain the pre-treated copper wire; Step 3: Tinning: Placing the pretreated copper wire in a tinning furnace for tinning to obtain the pretreated tinned copper wire; Step 4: Post-processing: The pretreated tinned copper wire is placed in clean water again to wash away impurities, and then vacuum dried to obtain the tinned copper wire.
2. A production process for tinned copper wire to prevent the tin coating from falling off according to claim 1, characterized in that: In the step 1, the annealing temperature is 650-720° C. and the time is 1-2 hours.
3. A production process for tinned copper wire to prevent the tin coating from falling off according to claim 1, characterized in that: In step 2, the temperature in the oven is 80-90° C., and the drying time is 1-2 hours.
4. A production process for tinned copper wire to prevent the tin coating from falling off according to claim 1, characterized in that: In step 3, the temperature in the tinning furnace is 230-250° C., and the residence time is 2-5 seconds.
5. The production process of tinned copper wire for preventing the tinned layer from falling off according to claim 1, characterized in that: The components of the soldering flux in step 2 are calculated by weight and include: 40-60 parts of modified rosin resin, 16-20 parts of lubricant, 12-18 parts of metal chloride, 3-8 parts of dispersant and 10-20 parts of solvent.
6. A production process for tinned copper wire to prevent the tin coating from falling off according to claim 5, characterized in that: The metal chloride salt is one or more combinations of zinc chloride, magnesium chloride, samarium chloride and sodium chloride.
7. A production process for tinned copper wire to prevent the tin coating from falling off according to claim 5, characterized in that: The lubricant is hexadecanoic acid or octadecanoic acid; the dispersant is ethylene glycol butyl ether or propylene glycol butyl ether; and the solvent is one of isopropanol, toluene and ethyl acetate.
8. A production process for tinned copper wire to prevent the tin coating from falling off according to claim 5, characterized in that: The preparation method of the modified rosin resin comprises: S1, weigh hydrogenated rosin resin and epoxy resin, mix them, add a catalyst, heat them to 80-100°C under the protection of nitrogen, stir and react for 3-6 hours, add acrylic acid monomer, continue to react for 2-5 hours, end the reaction, cool to room temperature, and obtain acrylic rosin resin; S2. Mix the acrylic rosin resin and anhydrous ethanol, add 2-mercaptobenzimidazole, stir well until uniform, then add a photoinitiator, react under ultraviolet light at room temperature, stir for 2-4 hours, and remove the ethanol under reduced pressure after the reaction to obtain a modified rosin resin.
9. A production process for tinned copper wire to prevent the tinned layer from falling off according to claim 8, characterized in that: In the S1, the amount of the catalyst added is 3%-8% of the mass of the hydrogenated rosin resin; the mass ratio of the hydrogenated rosin resin, the epoxy resin and the acrylic acid monomer is 1:3.5-4.2:0.63-0.
96.
10. A production process for tinned copper wire to prevent the tinned layer from falling off according to claim 8, characterized in that: In the S2, the mass ratio of acrylic rosin resin, 2-mercaptobenzimidazole and anhydrous ethanol is 1:0.31-0.62:4-6; the photoinitiator is benzoin ethyl ether, and the added amount is 2%-8% of the mass of the acrylic rosin resin.
Citation Information
Patent Citations
Tinning scaling powder for tinned copper wire and preparation method of tinning scaling powder
CN107419209A
Production process of tinned copper wire
CN110952056A
Hot tinning process of ultrafine copper wire
CN113106369A
Production process for tin-plated copper wire and capable of preventing tin-plated layer from falling off
CN113249674A
A process and apparatus for the production of tinned wires
GB1130260A