Preparation method of anti-sticking coating on surface of welding nozzle

Through laser hairening and heat treatment technology, a high binding force anti-adhesive coating is formed on the surface of the welding nozzle, which solves the problems of complex process, high cost and insufficient coating bonding in the existing technology, and improves the anti-dirty performance of the welding nozzle and service life.

CN118979250APending Publication Date: 2024-11-19苏州芯合半导体材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411061162.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing anti-adhesive coating preparation process for the surface of the welding nozzle is complex and has high cost. The coating bonding force is insufficient and it is easy to peel off, which affects the service life and anti-dirty properties.

Method used

Using a combination of laser hairening pretreatment and laser heat treatment, the surface of the welding nozzle is blanched and heat treated under the N2 protection atmosphere by a nanosecond pulse laser or visible laser, forming a hairening with a diameter of 0.1-4um and a depth of 1-200nm. and spray adhesive and coating material to form an anti-stick coating by laser scanning.

Benefits of technology

It reduces process costs and energy consumption, improves the binding force of the coating and anti-dirty ability, and extends the service life of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979250A_ABST
    Figure CN118979250A_ABST
Patent Text Reader

Abstract

The invention is applicable to the technical field of coating preparation, and provides a preparation method of a surface anti-sticking coating of a welding nozzle, which comprises the following steps: under N2 protective atmosphere, performing texturing treatment on the surface of the welding nozzle through laser, and performing laser scanning from inside to outside to obtain texturing points with the diameter of 0.1-4 microns and the depth of 1-200nm, and the roughness after treatment is 0.5-10 microns; spraying a layer of binder on the terminal surface of the roughened welding nozzle; pressing a welding nozzle with a binder layer into the coating material; and the welding nozzle with the binder layer and the coating material is subjected to heat treatment through laser, laser scanning is conducted from inside to outside under the N2 protective atmosphere, and the coating material is molten to form the anti-sticking coating. The adhesive force between the coating and the surface of the welding nozzle is remarkably improved while the product performance is not affected, and the service life of the product is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coating preparation, and in particular relates to a method for preparing an anti-stick coating on the surface of a welding nozzle. Background Art

[0002] The soldering nozzle is a key component used in semiconductor packaging bonding. Different structures and shapes are prepared according to different bonding materials. During the use of the soldering nozzle, the bonding material sticks to the surface of the soldering nozzle terminal, causing the soldering nozzle to fail too quickly before reaching its service life because the soldering point state cannot be guaranteed. Although the existing anti-fouling materials can adjust the anti-fouling performance of the soldering nozzle by coating, the coating preparation process is complicated and costly, which is not conducive to the large-scale production of the product. Although the coating obtained by physical bonding has low cost, the coating bonding force is small and easy to peel off during use. In addition, traditional coating pretreatment is mostly carried out by pickling or heating furnace heat treatment. If the pickling conditions are not properly controlled, the performance of the product will deteriorate; the heating furnace heat treatment cycle is long and the energy consumption is high. In view of the above problems, the present invention proposes a method for preparing an anti-sticking coating on the surface of the soldering nozzle, which reduces the cost while enhancing the bonding force of the coating. Summary of the invention

[0003] The object of the present invention is to provide a method for preparing an anti-stick coating on the surface of a welding nozzle, aiming to solve the problems raised in the above-mentioned background technology.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] A method for preparing an anti-stick coating on the surface of a welding nozzle comprises the following steps:

[0006] Step 1, laser texturing pre-treatment: Use nanosecond pulse laser or visible light laser after frequency doubling, and texturing the surface of the welding nozzle by laser in N2 protective atmosphere, control the pulse frequency, laser pulse width, spot size and energy density, and perform laser scanning from the inside (close to the axis side) to the outside (close to the edge side). The scanning rate is 100-10000mm / s, and the texturing point with a diameter of 0.1-4um and a depth of 1-200nm is obtained. The roughness after treatment is 0.5-10um;

[0007] Step 2, adhesive spraying: spray a layer of adhesive on the terminal surface of the welding nozzle after the roughening treatment;

[0008] Step 3, coating material pressing: press the welding nozzle with the adhesive layer into the coating material for 0-10 seconds;

[0009] Step 4, laser heat treatment: Use nanosecond pulse laser or visible light laser in large spot mode to perform laser heat treatment on the welding nozzle with adhesive layer and coating material. Under N2 protective atmosphere, adjust the spot size and energy density, perform laser scanning from inside to outside, and the scanning rate is 10-10000mm / s to melt the coating material to form an anti-stick coating.

[0010] Furthermore, in step 1, the pulse frequency is 0.5-10 MHz, the laser pulse width is 1-100 ns, the spot size is 1-10 um, and the energy density is controlled at 4-30 J / cm 2 .

[0011] Furthermore, the binder is at least one of phenolic resin, epoxy resin, polyaminophenol resin and unsaturated polyester.

[0012] Furthermore, the coating material is a mixture of one or more of CrN, Al2O3, SiO2, and Li2O.

[0013] Furthermore, when the coating material is a mixture of CrN, Al2O3, SiO2 and Li2O, the mass ratio of the coating material is CrN:Al2O3:SiO2:Li2O=(1-x):x:(1-y):y, wherein x=0-90, y=0-30.

[0014] Furthermore, the particle size of the coating material is 0.5-10 um.

[0015] Furthermore, in step 4, the spot size is 10-100um, and the energy density is controlled at 50-450J / cm 2 .

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] The laser texturing pre-treatment process proposed by the present invention has a short action time, low energy consumption and does not affect the performance of the product itself; the surface after laser texturing is conducive to improving the adhesion between the adhesive and the product substrate, while ensuring the smooth progress of the subsequent process, while reducing energy consumption and enhancing the bonding force of the coating; in addition, the surface roughness of the coating obtained by the present invention will not change due to the wear of the product, thereby improving the anti-fouling ability and service life of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a flow chart of the present invention.

[0019] Figure 2 This is a SEM image of the combination of the coating and the substrate in the best embodiment 1 of the present invention. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0021] The specific implementation of the present invention is described in detail below in conjunction with specific embodiments.

[0022] Embodiment 1: One embodiment of the present invention provides a method for preparing an anti-stick coating on the surface of a welding nozzle, comprising the following steps:

[0023] Step 1: Use nanosecond pulse laser to roughen the surface of the welding nozzle in N2 protective atmosphere. The pulse frequency is 5MHz, the laser pulse width is 50ns, the spot size is 5um, and the energy density is controlled at 14J / cm 2 , laser scanning was performed from the inside to the outside with a scanning rate of 5000mm / s, and a roughening point with a diameter of 2um and a depth of 100nm was obtained. The roughness after treatment was 5um.

[0024] Step 2: spray a layer of phenolic resin adhesive on the roughened terminal surface of the welding nozzle.

[0025] Step 3: Press the welding tip with the adhesive layer into the coating material for 5 seconds. The particle size of the coating material is 5 μm. The coating material is a mixture of CrN, Al2O3, SiO2 and Li2O, and the mass ratio of the coating material is CrN:Al2O3:SiO2:Li2O=(1-x):x:(1-y):y, where x=45 and y=15.

[0026] Step 4: Use nanosecond pulse laser in large spot mode to perform laser heat treatment on the welding nozzle under N2 protective atmosphere. The spot size is 50um and the energy density is controlled at 250J / cm 2 , laser scanning is performed from the inside out to melt the coating material to obtain a non-stick coating (see Figure 2 ).

[0027] Embodiment 2: One embodiment of the present invention provides a method for preparing an anti-stick coating on the surface of a welding nozzle, comprising the following steps:

[0028] Step 1: Use visible light laser to perform laser roughening on the surface of the welding nozzle in N2 protective atmosphere. The pulse frequency is 2MHz, the laser pulse width is 20ns, the spot size is 3um, and the energy density is controlled at 8J / cm 2 Laser scanning was performed from the inside to the outside at a scanning rate of 3000 mm / s, and roughening points with a diameter of 1 um and a depth of 50 nm were obtained. The roughness after treatment was 3 um.

[0029] Step 2: Spray a layer of epoxy resin adhesive on the roughened terminal surface of the welding nozzle.

[0030] Step 3: Press the welding tip with the adhesive layer into the coating material for 3s. The coating material has a particle size of 3um and is a mixture of CrN and Al2O3 in a mass ratio of 70:30.

[0031] Step 4: Use visible light laser in large spot mode to perform laser heat treatment on the welding nozzle under N2 protective atmosphere. The spot size is 30um and the energy density is controlled at 150J / cm 2 , laser scanning is performed from the inside out to melt the coating material to obtain a non-stick coating.

[0032] Embodiment 3: One embodiment of the present invention provides a method for preparing an anti-stick coating on the surface of a welding nozzle, comprising the following steps:

[0033] Step 1: Use nanosecond pulse laser to perform laser roughening on the surface of the welding nozzle under N2 protective atmosphere. The pulse frequency is 1MHz, the laser pulse width is 10ns, the spot size is 1um, and the energy density is controlled at 6J / cm 2 Scanning from the inside to the outside at a rate of 6000mm / s, a roughening point with a diameter of 0.5um and a depth of 50nm was obtained, and the roughness after treatment was 2um.

[0034] Step 2: Spray a layer of unsaturated polyester adhesive on the terminal surface of the welding nozzle.

[0035] Step 3: Press the welding tip into the Al2O3 coating material for 2s. The particle size of the coating material is 2um.

[0036] Step 4: Use nanosecond pulse laser in large spot mode to perform laser heat treatment on the welding nozzle under N2 protective atmosphere. The spot size is 20um and the energy density is controlled at 100J / cm 2 , laser scanning is performed from the inside out to melt the coating material to obtain a non-stick coating.

[0037] Embodiment 4: One embodiment of the present invention provides a method for preparing an anti-stick coating on the surface of a welding nozzle, comprising the following steps:

[0038] Step 1: Use visible light laser to roughen the surface of the welding nozzle in N2 protective atmosphere. The pulse frequency is 8MHz, the laser pulse width is 80ns, the spot size is 8um, and the energy density is controlled at 22J / cm 2 Scanning from the inside to the outside at a rate of 8000mm / s, a roughening point with a diameter of 3um and a depth of 150nm is generated, and the roughness after treatment is 7um.

[0039] Step 2: Spray a layer of polyaminophenol resin adhesive on the roughened terminal surface of the welding nozzle.

[0040] Step 3: Press the welding tip into the SiO2 coating material for 7s. The particle size of the coating material is 7um.

[0041] Step 4: Use visible light laser in large spot mode to perform laser heat treatment on the welding nozzle in N2 atmosphere. The spot size is 70um and the energy density is controlled at 300J / cm 2 , laser scanning is performed from the inside out to melt the coating material to obtain a non-stick coating.

[0042] Embodiment 5: One embodiment of the present invention provides a method for preparing an anti-stick coating on the surface of a welding nozzle, comprising the following steps:

[0043] Step 1: Use visible light laser to roughen the surface of the welding nozzle in N2 protective atmosphere. The pulse frequency is 10MHz, the laser pulse width is 100ns, the spot size is 10um, and the energy density is controlled at 30J / cm 2 Scanning from the inside to the outside at a rate of 10000mm / s, a roughening point with a diameter of 4um and a depth of 200nm was obtained, and the roughness after treatment was 10um.

[0044] Step 2: Spray a layer of phenolic resin adhesive on the roughened surface of the welding nozzle.

[0045] Step 3: Press the welding tip into the mixture coating material of CrN and SiO2 for 10 seconds. The particle size of the coating material is 10um, and the mass ratio is CrN:SiO2=60:40.

[0046] Step 4: Use visible light laser in large spot mode to perform laser heat treatment on the welding nozzle under N2 protective atmosphere. The spot size is 100um and the energy density is controlled at 450J / cm 2 , laser scanning is performed from the inside out to melt the coating material to obtain a non-stick coating.

[0047] The above are only preferred embodiments of the present invention. It should be pointed out that, for those skilled in the art, several modifications and improvements can be made without departing from the concept of the present invention. These should also be regarded as the protection scope of the present invention. These will not affect the effect of the implementation of the present invention and the practicality of the patent.

Claims

1. A method for preparing an anti-stick coating on the surface of a welding nozzle, characterized in that: The following steps are involved: Step 1, laser texturing pre-treatment: Use nanosecond pulse laser or visible light laser after frequency doubling, and texturing the surface of the welding nozzle by laser in N2 protective atmosphere, control the pulse frequency, laser pulse width, spot size and energy density, and perform laser scanning from the inside to the outside. The scanning rate is 100-10000mm / s, and the texturing point with a diameter of 0.1-4um and a depth of 1-200nm is obtained. The roughness after treatment is 0.5-10um; Step 2, adhesive spraying: spray a layer of adhesive on the terminal surface of the welding nozzle after the roughening treatment; Step 3, coating material pressing: press the welding nozzle with the adhesive layer into the coating material for 0-10 seconds; Step 4, laser heat treatment: Use nanosecond pulse laser or visible light laser in large spot mode to perform laser heat treatment on the welding nozzle with adhesive layer and coating material. Under N2 protective atmosphere, adjust the spot size and energy density, perform laser scanning from inside to outside, and the scanning rate is 10-10000mm / s to melt the coating material to form an anti-stick coating.

2. The method for preparing the anti-stick coating on the surface of the welding nozzle according to claim 1, characterized in that: In step 1, the pulse frequency is 0.5-10 MHz, the laser pulse width is 1-100 ns, the spot size is 1-10 um, and the energy density is controlled at 4-30 J / cm 2 .

3. The method for preparing the anti-stick coating on the surface of the welding nozzle according to claim 1, characterized in that: The binder is at least one of phenolic resin, epoxy resin, polyaminophenol resin and unsaturated polyester.

4. The method for preparing the anti-stick coating on the surface of the welding nozzle according to claim 1, characterized in that: The coating material is a mixture of one or more of CrN, Al2O3, SiO2 and Li2O.

5. The method for preparing the anti-stick coating on the surface of the welding nozzle according to claim 4, characterized in that: When the coating material is a mixture of CrN, Al2O3, SiO2 and Li2O, the mass ratio of the coating material is CrN:Al2O3:SiO2:Li2O=(1-x):x:(1-y):y, wherein x=0-90, y=0-30.

6. The method for preparing the anti-stick coating on the surface of the welding nozzle according to claim 4, characterized in that: The particle size of the coating material is 0.5-10 um.

7. The method for preparing the anti-stick coating on the surface of the welding nozzle according to claim 1, characterized in that: In step 4, the spot size is 10-100um, and the energy density is controlled at 50-450J / cm 2 .