Surface modification method of high-silicon-aluminum composite material for electronic packaging shell
Through wet sandblasting, ultrasonic oil removal and cleaning, magnetron sputtering and electroplating, the problems of numerous processes, insufficient binding force and hydrogen poisoning in the surface treatment technology of high-silicon aluminum composite materials are solved, and the plating is efficient. Surface modification with strong stability and applicability.
Patent Information
- Application Number
- CN202411078501.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
AI Technical Summary
The existing surface treatment technology of high-silicon aluminum composite materials has problems caused by a variety of processes, long cycles, insufficient binding force between the plating and substrate, and the difficulty of single process parameters to cover the entire series of materials and the chemical nickel plating process.
Multi-step methods of wet sandblasting, ultrasonic oil removal and cleaning, magnetron sputtering titanium copper metal film, activation treatment, nickel plating and gold plating are used, combining dry magnetron sputtering vacuum coating and wet electroplating nickel gold to optimize the process Parameters to improve coating bonding and adapt materials with different silicon content.
It effectively improves the binding force of the coating, shortens the process cycle, is highly applicable, is suitable for large-scale industrial production, avoids hydrogen poisoning, and meets the plating stability requirements after high-temperature baking.
Smart Images

Figure CN118979252A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface treatment of electronic packaging shell materials, and in particular to a surface modification method of a high-silicon aluminum composite material used for electronic packaging shells. Background Art
[0002] High silicon aluminum composite materials have the characteristics of low expansion coefficient, low density, high thermal conductivity, airtight packaging, and machinability. They can meet the requirements of electronic packaging materials for high thermal conductivity, low expansion coefficient, low density, and high airtightness, and have been widely used in electronic packaging fields such as radar T / R components. Compared with aluminum alloys, the silicon content in high silicon aluminum composite materials mostly exceeds 27%, reaching 50% and 70%, and cannot be directly packaged and welded, so the surface needs to be modified. However, due to the special physical and chemical properties of the material, the traditional wet electroplating is difficult, the process is complicated, and the cycle is long. It is easy to have low bonding strength of the coating. After high and low temperature cycles such as welding, the coating has quality problems such as bubbling and peeling. Chinese invention patent CN201310553767.2 discloses a gold plating method for high silicon aluminum composite materials. After conventional aluminum alloy electroplating pretreatment, chemical nickel plating, aging treatment, activation, nickel plating and electroplating gold treatment are performed, and finally the thickness of the gold plating layer on the surface of the Si-50Al composite material is 2-3 microns. However, this method can only meet the needs of aluminum-silicon composite materials with a silicon content of ≤50%. The higher the silicon content of the base material, the more difficult this wet electroplating is. A single process parameter cannot cover the entire series of high-silicon aluminum substrates. After the silicon content of the base material changes, a large number of tests and verifications are required to obtain the optimal process parameters. In addition, the traditional wet electroplating process often involves plating processes such as chemical nickel plating, which causes excessive hydrogen content inside the shell, easily causing hydrogen poisoning in the electronic chip.
[0003] In view of the above-mentioned defects, the inventors of the present invention finally obtained the present invention after a long period of research and practice. Summary of the invention
[0004] The purpose of the present invention is to solve the problems existing in the prior art, such as numerous processes, long cycles, insufficient bonding between the coating and the substrate, difficulty in covering the full range of high-silicon aluminum substrates with a single process parameter, and excessive hydrogen content in the coating during chemical nickel plating, which can easily cause hydrogen poisoning of electronic chip products. A surface modification method for a high-silicon aluminum composite material for an electronic packaging shell is provided.
[0005] In order to achieve the above object, the present invention discloses a surface modification method of a high silicon aluminum composite material for an electronic packaging shell, comprising the following steps:
[0006] S1, sandblasting the surface of the high silicon aluminum composite material by wet sandblasting;
[0007] S2, ultrasonically degreasing and cleaning the high silicon aluminum composite material after sandblasting, rinsing it with water, and drying and storing it;
[0008] S3, magnetron reactive sputtering titanium-copper metal film on the surface of pre-treated high silicon-aluminum composite material;
[0009] S4, put the parts after magnetron sputtering treatment into the activation solution, soak for 5-10 seconds at a temperature of 20-35°C, take out and rinse with water;
[0010] S5, placing the activated parts into a nickel plating solution for nickel plating, and taking them out and cleaning them;
[0011] S6, use pure gold plate or platinum titanium mesh as anode and high silicon aluminum composite material as cathode, and gold-plate the nickel-plated parts according to the conventional pure gold plating method, and then take them out and clean them.
[0012] In the step S1, the wet sandblasting uses glass beads of 150-250 meshes, and the sandblasting pressure is set to 0.15-0.2 MPa.
[0013] In step S2, the ultrasonic degreasing cleaning solution is prepared from 5-10 g / L sodium hydroxide, 30-40 g / L sodium carbonate, 40-50 g / L sodium phosphate and deionized water, the temperature of the ultrasonic degreasing cleaning solution is 55-65° C., and the cleaning time is 3-5 min.
[0014] In the step S3, during the magnetron sputtering coating process, the substrate temperature is always maintained at 350°C, and the thickness of the Ti layer obtained on the surface of the high-silicon-aluminum composite material is 0.5-1 μm, and the thickness of the Cu layer is 1-3 μm.
[0015] In the step S3, during the magnetron sputtering coating process, a titanium target and a copper target are arranged in parallel in the vacuum chamber of the magnetron sputtering, a high silicon aluminum composite material is placed on a turntable in the vacuum chamber, the turntable speed is controlled to 15 rpm, the distance between the substrate and the target is adjusted to 8 to 12 cm, and the vacuum in the vacuum chamber reaches 10 -4 The working atmosphere is pure argon, the argon flow rate is controlled at 10-30 sccm, and the gas pressure is maintained at 0.25-0.45 Pa.
[0016] In step S4, the activation solution is a 50-100 mol / L dilute sulfuric acid solution.
[0017] In step S5, during the nickel plating process, the cathode current density is 0.5 to 1 A / dm 2 , reaction temperature is 20-35°C, pH is 4.6-5.2, reaction time is 15-25min, and nickel plating layer thickness is 2-5μm.
[0018] In step S6, during the gold plating process, the current density is 0.2 to 0.8 A / dm 2 , the reaction temperature is 55-70°C, the pH is 4.5-5.5, the reaction time is 10-15min, and the thickness of the gold layer is 2-3μm.
[0019] Compared with the prior art, the beneficial effects of the present invention are:
[0020] 1. The surface modification method of the high silicon aluminum composite material of the present invention combines dry magnetron sputtering vacuum coating and wet nickel-gold electroplating, which can effectively improve the bonding strength of the coating. After the coating is baked at 450°C for 5 to 10 minutes, there is no blistering or shedding of the coating. The bonding strength of the coating reaches the standard specified in Appendix A of GJB 1420A-1999 "General Specification for Semiconductor Integrated Circuit Housings". Under SEM electron microscope observation, the Ti / Cu / Ni / Au layers are tightly bonded, and the transition interface between the layers is clear;
[0021] 2. In the magnetron sputtering coating process described in the present invention, ion beam cleaning is first performed to effectively remove the loose layer on the surface of the aluminum-silicon composite material to obtain a fresh surface, thereby improving the bonding force between Ti and the substrate. At the same time, the substrate temperature during the sputtering process is controlled to be 350°C, which is beneficial to enhancing the surface atomic diffusion effect, making the surface coating composition more uniform, and reducing the coating stress. Theoretical analysis shows that at this temperature, a certain interface interdiffusion will occur between the Ti layer and the substrate, which can further improve the bonding force of the coating. The thickness of the sputtered Ti layer is controlled to be 0.5-1 μm, and the thickness of the Cu layer is controlled to be 1-3 μm;
[0022] 3. The silicon content of the high silicon aluminum composite material described in the present invention is 27%, 50%, and 70%, which have all been verified in practice. However, according to the principle of this technology, it can be extended to aluminum silicon composite materials with other silicon contents. The advantages of the present invention are that it is not limited by the amount of silicon in the substrate, has strong applicability, shortens the process of wet electroplating, has the advantages of energy saving and environmental protection, and is suitable for large-scale industrial production;
[0023] 4. The surface modified electronic packaging aluminum silicon shell obtained by the technical solution of the present invention has a total coating thickness of about 6 to 12 μm according to the SEM magnification scale, of which the Ti layer is about 0.5 to 1 μm, the Cu layer is about 1 to 3 μm, the Ni layer is about 2 to 5 μm, and the Au layer is about 2 to 3 μm. The transitions between the layers are clear when viewed from the cross section, the coatings are tightly combined without gaps or detachment, the solder spreads and infiltrates on the coating surface, and there is no cold solder joints or desoldering. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a flow chart for the surface modification preparation of the high silicon aluminum composite material of the present invention;
[0025] Figure 2This is a SEM microscopic morphology image of the high silicon aluminum composite material of the present invention;
[0026] Figure 3 The SEM microscopic morphology and element distribution of the cross section of the high silicon aluminum composite material after surface modification in the present invention;
[0027] Figure 4 This is a SEM microscopic morphology of the cross section of the weldable sample in the present invention. DETAILED DESCRIPTION
[0028] The above and other technical features and advantages of the present invention are described in more detail below in conjunction with the accompanying drawings.
[0029] The equipment and materials used in the following examples include: a box-type wet sandblasting machine, a magnetron sputtering vacuum coating equipment; glass beads (150-250 mesh), sodium hydroxide (NaOH), sodium carbonate (Na2CO3), sodium phosphate (Na3PO4), sulfuric acid (H2SO4), nickel sulfate (NiSO4·6H2O), nickel chloride (NiCl2·6H2O), boric acid (H3BO3), sodium dodecyl sulfate (C 12 H 25 SO4Na), gold potassium citrate, Temperex 9500 tank opening fluid, and deionized water are all conventional chemical reagents sold in the market with chemical purity.
[0030] Example 1
[0031] The high silicon aluminum composite material for electronic packaging shells uses AlSi50 with a silicon content of 50%. The specific modification steps are as follows:
[0032] Prepare ultrasonic degreasing cleaning solution: weigh sodium hydroxide, sodium carbonate and sodium phosphate according to the formula and prepare a solution. The composition and content of the prepared cleaning solution are: NaOH 10g / L, Na2CO3 40g / L, Na3PO4 50g / L and deionized water 1L.
[0033] Prepare activation solution: Pour one-third of deionized water into the plating tank, slowly add the measured sulfuric acid into the plating tank, stir thoroughly, add deionized water to the working liquid level, cool to room temperature for use. The composition and content of the prepared activation solution are: 50ml / L sulfuric acid.
[0034] Prepare nickel plating solution: inject one-third of deionized water into the plating tank, add weighed nickel sulfate and fully dissolve it, dissolve weighed nickel chloride separately and add it to the plating tank, dissolve weighed sodium dodecyl sulfate separately and add it to the plating tank, and then dissolve weighed boric acid separately with hot deionized water under boiling and add it to the plating tank, add deionized water to the working liquid level, and adjust the pH value to the required range of the formula with dilute sodium hydroxide solution. The composition and content of the prepared nickel plating solution are: nickel sulfate 180g / L, sodium chloride 50g / L, boric acid 30g / L, sodium dodecyl sulfate 0.08g / L, pH 5.0 at 25℃.
[0035] Preparation of gold plating solution: put the calculated amount of Temperex 9500 pre-bottle liquid into the plating tank and heat it to 65°C, add the calculated amount of gold salt while stirring, stir until the gold salt is completely dissolved, take 500mL of plating solution from the plating tank and cool it to 25°C, measure the pH value and specific gravity, the composition and content of the prepared gold plating solution are: Au (in the form of potassium citrate gold) 8g / L, pH 5.0 under the condition of temperature 25°C.
[0036] (1) Wet sandblasting: Place the processed high-silicon aluminum electronic packaging shell parts into the sandblasting room, adjust the pressure of the sandblasting machine to 0.15Mpa, select 200-mesh glass beads, aim the spray gun at the surface of the parts and turn on the equipment. During the sandblasting process, the angle between the spray gun and the parts needs to be adjusted to ensure that the surface of the parts is evenly sprayed. After sandblasting, take out the parts and rinse them with deionized water, and observe whether there are any missed locations on the surface of the parts.
[0037] (2) Ultrasonic degreasing: Place the sandblasted parts into the prepared ultrasonic degreasing cleaning solution, ultrasonically clean them for 5 minutes at a solution temperature of 60°C, then take them out, rinse them thoroughly in running deionized water, and then take them out and dry them.
[0038] (3) Vacuum coating: The pre-treated parts are placed on a turntable in a vacuum chamber. Titanium (Ti) palladium and copper (Cu) palladium are placed in parallel in the vacuum chamber of magnetron sputtering. The turntable speed is controlled to 15 rpm, and the distance between the substrate and the target is adjusted to 8 cm. The vacuum in the vacuum chamber reaches 10 -4 The working atmosphere is pure argon, the argon flow rate is controlled to be 10 sccm, and the gas pressure is maintained at 0.25 Pa.
[0039] The substrate temperature was adjusted to 350°C, and ion beam cleaning was started with a cleaning voltage of 1500V, a bias voltage of 1500V, a bias duty cycle of 5%, and a cleaning time of 20min. After the ion beam cleaning was completed, the titanium sputtering process was started directly with a titanium (Ti) palladium current of 0.05A, a negative bias voltage of 100V, and a reactive sputtering time of 20min to deposit a pure titanium (Ti) bonding layer on the surface of the part. After the titanium plating process was completed, the copper sputtering process was started directly with a copper (Cu) palladium current of 4A, a bias voltage of 500V, a bias duty cycle of 85%, and a reactive sputtering time of 60min. After the sputtering reaction was completed and the substrate temperature dropped to room temperature, the product was taken out and dried for storage.
[0040] (4) Activation treatment: Place the parts that have been vacuum coated into the prepared activation solution, soak them for 8 seconds at a solution temperature of 30°C, take them out and rinse them with water.
[0041] (5) Nickel electroplating: Place the activated parts into the prepared nickel plating solution for nickel plating, with a cathode current density of 1A / dm 2 The reaction temperature is 35℃, pH is 5.0, the reaction time is 20min, and the plate is taken out and cleaned.
[0042] (6) Gold plating: Use the platinum titanium mesh as the anode and the nickel-plated parts as the cathode. Perform gold plating on the nickel-plated parts according to the conventional pure gold plating method. The current density is 0.5A / dm 2 , reaction temperature 60 ℃, pH 5.0, reaction time 12min, take out and clean.
[0043] (7) Performance testing: After the parts are gold-plated according to the above method, the gold layer has fine crystals and uniform color. The coating thickness is tested with an X-ray coating thickness gauge, where the Ti layer is 0.65 μm, the Cu layer is 2.56 μm, the Ni layer is 3.17 μm, and the Au layer is 2.27 μm. The parts are placed in a muffle furnace and heated to 450°C. The furnace temperature is then maintained for 10 minutes. After being taken out, they are cooled to room temperature. The coating is observed under a 30x magnifying glass to show no peeling or bubbling, indicating excellent coating adhesion.
[0044] Example 2
[0045] The high silicon aluminum composite material for electronic packaging shells uses AlSi27 with a silicon content of 27%. The specific modification steps are as follows:
[0046] Prepare ultrasonic degreasing cleaning solution: weigh sodium hydroxide, sodium carbonate and sodium phosphate according to the formula and prepare a solution. The composition and content of the prepared cleaning solution are: NaOH 8g / L, Na2CO3 35g / L, Na3PO4 46g / L and deionized water 1L.
[0047] Prepare activation solution: inject one third of deionized water into the plating tank, slowly add the measured sulfuric acid into the plating tank, stir thoroughly, add deionized water to the working liquid level, cool to room temperature for use. The composition and content of the prepared activation solution are: 80ml / L sulfuric acid.
[0048] Prepare nickel plating solution: inject one-third of deionized water into the plating tank, add weighed nickel sulfate and fully dissolve it, dissolve weighed nickel chloride separately and add it to the plating tank, dissolve weighed sodium dodecyl sulfate separately and add it to the plating tank, and then dissolve weighed boric acid separately with hot deionized water under boiling and add it to the plating tank, add deionized water to the working liquid level, and adjust the pH value to the required range of the formula with dilute sodium hydroxide solution. The composition and content of the prepared nickel plating solution are: 200g / L nickel sulfate, 60g / L sodium chloride, 40g / L boric acid, 0.05g / L sodium dodecyl sulfate, and the pH is 4.8 at a temperature of 20°C.
[0049] Preparation of gold plating solution: Add the calculated amount of Temperex 9500 pre-bottle liquid into the plating tank and heat it to 68°C. Add the calculated amount of gold salt while stirring. Stir until the gold salt is completely dissolved. Take 500mL of plating solution from the plating tank and cool it to 25°C. Measure the pH value and specific gravity. The composition and content of the prepared gold plating solution are: Au (in the form of potassium citrate gold) 7g / L, pH 5.2 at 25°C.
[0050] (1) Wet sandblasting: Place the processed high-silicon aluminum electronic packaging shell parts into the sandblasting room, adjust the pressure of the sandblasting machine to 0.18Mpa, select 200-mesh glass beads, aim the spray gun at the surface of the parts and turn on the equipment. During the sandblasting process, the angle between the spray gun and the parts needs to be adjusted to ensure that the surface of the parts is evenly sprayed. After sandblasting, take out the parts and rinse them with deionized water, and observe whether there are any missed locations on the surface of the parts.
[0051] (2) Ultrasonic degreasing: Place the sandblasted parts into the prepared ultrasonic degreasing cleaning solution, and perform ultrasonic cleaning for 3 minutes at a solution temperature of 62°C. Then take them out, rinse them thoroughly in running deionized water, and then take them out and dry them.
[0052] (3) Vacuum coating: The pre-treated parts are placed on a turntable in a vacuum chamber. Titanium (Ti) palladium and copper (Cu) palladium are placed in parallel in the vacuum chamber of magnetron sputtering. The turntable speed is controlled to 15 rpm, and the distance between the substrate and the target is adjusted to 10 cm. The vacuum in the vacuum chamber reaches 10 -4 The working atmosphere is pure argon, the argon flow rate is controlled to be 15 sccm, and the gas pressure is maintained at 0.30 Pa.
[0053] The substrate temperature was adjusted to 350°C, and ion beam cleaning was started with a cleaning voltage of 1500V, a bias voltage of 1500V, a bias duty cycle of 5%, and a cleaning time of 30min. After the ion beam cleaning was completed, the titanium sputtering process was started directly with a titanium (Ti) palladium current of 0.05A, a negative bias voltage of 100V, and a reactive sputtering time of 15min to deposit a pure titanium (Ti) bonding layer on the surface of the part. After the titanium plating process was completed, the copper sputtering process was started directly with a copper (Cu) palladium current of 4A, a bias voltage of 500V, a bias duty cycle of 85%, and a reactive sputtering time of 40min. After the sputtering reaction was completed and the substrate temperature dropped to room temperature, the product was taken out and dried for storage.
[0054] (4) Activation treatment: Place the parts that have been vacuum coated into the prepared activation solution, soak them for 5 seconds at a solution temperature of 25°C, take them out and rinse them with water.
[0055] (5) Nickel electroplating: Place the activated parts into the prepared nickel plating solution for nickel plating, with a cathode current density of 1A / dm 2 The reaction temperature is 20℃, pH is 4.8, the reaction time is 18min, and the plate is taken out and cleaned.
[0056] (6) Electroplating gold: Platinum titanium mesh is used as the anode, and the nickel-plated parts are used as the cathode. The parts after nickel-plating are plated with gold according to the conventional method of pure gold plating. The current density is 0.8A / dm 2 , reaction temperature 65 ℃, pH 5.2, reaction time 13min, take out and clean.
[0057] (7) Performance testing: After the parts are gold-plated according to the above method, the gold layer has fine crystals and uniform color. The coating thickness is tested with an X-ray coating thickness gauge, where the Ti layer is 0.58μm, the Cu layer is 1.78μm, the Ni layer is 3.26μm, and the Au layer is 2.56μm. The parts are placed in a muffle furnace and heated to 450°C. The furnace temperature is then maintained for 10 minutes. After being taken out, they are cooled to room temperature. The coating is observed under a 30x magnifying glass to show no peeling or bubbling, indicating excellent coating adhesion.
[0058] Example 3
[0059] The high silicon aluminum composite material for electronic packaging shells uses AlSi70 with a silicon content of 70%. The specific modification steps are as follows:
[0060] Prepare ultrasonic degreasing cleaning solution: weigh sodium hydroxide, sodium carbonate and sodium phosphate according to the formula and prepare a solution. The composition and content of the prepared cleaning solution are: NaOH 10g / L, Na2CO3 38g / L, Na3PO4 50g / L and deionized water 1L.
[0061] Prepare activation solution: inject one third of deionized water into the plating tank, slowly add the measured sulfuric acid into the plating tank, stir thoroughly, add deionized water to the working liquid level, cool to room temperature for use. The composition and content of the prepared activation solution are: sulfuric acid 100ml / L.
[0062] Prepare nickel plating solution: inject one-third of deionized water into the plating tank, add weighed nickel sulfate and fully dissolve it, dissolve weighed nickel chloride separately and add it to the plating tank, dissolve weighed sodium dodecyl sulfate separately and add it to the plating tank, and then dissolve weighed boric acid separately with hot deionized water under boiling and add it to the plating tank, add deionized water to the working liquid level, and adjust the pH value to the required range of the formula with dilute sodium hydroxide solution. The composition and content of the prepared nickel plating solution are: nickel sulfate 160g / L, sodium chloride 55g / L, boric acid 36g / L, sodium dodecyl sulfate 0.09g / L, pH is 5.2 at a temperature of 32°C.
[0063] Preparation of gold plating solution: put the calculated amount of Temperex 9500 pre-bottle liquid into the plating tank and heat it to 66°C, add the calculated amount of gold salt while stirring, stir until the gold salt is completely dissolved, take 500mL of plating solution from the plating tank and cool it to 25°C, measure the pH value and specific gravity, and the composition and content of the prepared gold plating solution are: Au (in the form of potassium citrate gold) 10g / L, pH 4.6 under the condition of temperature 25°C.
[0064] (1) Wet sandblasting: Place the processed high-silicon aluminum electronic packaging shell parts into the sandblasting room, adjust the pressure of the sandblasting machine to 0.20Mpa, select 150-mesh glass beads, aim the spray gun at the surface of the parts and turn on the equipment. During the sandblasting process, the angle between the spray gun and the parts needs to be adjusted to ensure that the surface of the parts is evenly sprayed. After sandblasting, take out the parts and rinse them with deionized water, and observe whether there are any missed locations on the surface of the parts.
[0065] (2) Ultrasonic degreasing: Place the sandblasted parts into the prepared ultrasonic degreasing cleaning solution, ultrasonically clean them for 5 minutes at a solution temperature of 65°C, then take them out, rinse them thoroughly in running deionized water, and then take them out and dry them.
[0066] (3) Vacuum coating: The pre-treated parts are placed on a turntable in a vacuum chamber. Titanium (Ti) palladium and copper (Cu) palladium are placed in parallel in the vacuum chamber of magnetron sputtering. The turntable speed is controlled to 15 rpm, the distance between the substrate and the target is adjusted to 12 cm, and the vacuum in the vacuum chamber reaches 10 -4 The working atmosphere is pure argon, the argon flow rate is controlled to 20sccm, and the gas pressure is maintained at 0.35Pa.
[0067] The substrate temperature was adjusted to 350°C, and ion beam cleaning was started with a cleaning voltage of 1500V, a bias voltage of 1500V, a bias duty cycle of 5%, and a cleaning time of 40min. After the ion beam cleaning was completed, the titanium sputtering process was started directly with a titanium (Ti) palladium current of 0.05A, a negative bias voltage of 100V, and a reactive sputtering time of 20min to deposit a pure titanium (Ti) bonding layer on the surface of the part. After the titanium plating process was completed, the copper sputtering process was started directly with a copper (Cu) palladium current of 4A, a bias voltage of 500V, a bias duty cycle of 85%, and a reactive sputtering time of 50min. After the sputtering reaction was completed and the substrate temperature dropped to room temperature, the product was taken out and dried for storage.
[0068] (4) Activation treatment: Place the parts that have been vacuum coated into the prepared activation solution, soak them for 5 seconds at a solution temperature of 25°C, take them out and rinse them with water.
[0069] (5) Nickel electroplating: Place the activated parts into the prepared nickel plating solution for nickel plating, with a cathode current density of 0.8A / dm 2 The reaction temperature is 32℃, pH is 5.2, the reaction time is 25min, and the plate is taken out and cleaned.
[0070] (6) Electroplating gold: Platinum titanium mesh is used as the anode, and the nickel-plated parts are used as the cathode. The parts after nickel-plating are plated with gold according to the conventional method of pure gold plating. The current density is 0.6A / dm 2 , reaction temperature 70 ℃, pH 4.6, reaction time 15min, take out and clean.
[0071] (7) Performance testing: After the parts are gold-plated according to the above method, the gold layer has fine crystals and uniform color. The coating thickness is tested with an X-ray coating thickness gauge, where the Ti layer is 0.87 μm, the Cu layer is 2.35 μm, the Ni layer is 4.60 μm, and the Au layer is 2.70 μm. The parts are placed in a muffle furnace and heated to 450°C. The furnace temperature is then maintained for 10 minutes. After being taken out, they are cooled to room temperature. The coating is observed under a 30x magnifying glass to show no peeling or bubbling, indicating excellent coating adhesion.
[0072] Comparative Example 1:
[0073] The design of the coating system and the optimization of the coating process parameters are one of the main difficulties that the present invention needs to overcome. This comparative example adopts the method of Example 1 to perform surface modification on an electronic packaging shell with a silicon content of 50%, except that the sputtering coating system selects a Ni coating for transition, and the specific process is as follows:
[0074] Prepare ultrasonic degreasing cleaning solution: weigh sodium hydroxide, sodium carbonate and sodium phosphate according to the formula and prepare a solution. The composition and content of the prepared cleaning solution are: NaOH 10g / L, Na2CO3 40g / L, Na3PO4 50g / L and deionized water 1L.
[0075] Preparation of activation solution: The activation solution formula for the nickel layer is 150ml / L HCl and 100g / L FeCl3 solution prepared with deionized water.
[0076] Prepare nickel plating solution: inject one-third of deionized water into the plating tank, add weighed nickel sulfate and fully dissolve it, dissolve weighed nickel chloride separately and add it to the plating tank, dissolve weighed sodium dodecyl sulfate separately and add it to the plating tank, and then dissolve weighed boric acid separately with hot deionized water under boiling and add it to the plating tank, add deionized water to the working liquid level, and adjust the pH value to the required range of the formula with dilute sodium hydroxide solution. The composition and content of the prepared nickel plating solution are: nickel sulfate 180g / L, sodium chloride 50g / L, boric acid 30g / L, sodium dodecyl sulfate 0.08g / L, pH 5.0 at 25℃.
[0077] Preparation of gold plating solution: put the calculated amount of Temperex 9500 pre-bottle liquid into the plating tank and heat it to 65°C, add the calculated amount of gold salt while stirring, stir until the gold salt is completely dissolved, take 500mL of plating solution from the plating tank and cool it to 25°C, measure the pH value and specific gravity, the composition and content of the prepared gold plating solution are: Au (in the form of potassium citrate gold) 8g / L, pH 5.0 under the condition of temperature 25°C.
[0078] (1) Wet sandblasting: Place the processed high-silicon aluminum electronic packaging shell parts into the sandblasting room, adjust the pressure of the sandblasting machine to 0.15Mpa, select 200-mesh glass beads, aim the spray gun at the surface of the parts and turn on the equipment. During the sandblasting process, the angle between the spray gun and the parts needs to be adjusted to ensure that the surface of the parts is evenly sprayed. After sandblasting, take out the parts and rinse them with deionized water, and observe whether there are any missed locations on the surface of the parts.
[0079] (2) Ultrasonic degreasing: Place the sandblasted parts into the prepared ultrasonic degreasing cleaning solution, ultrasonically clean them for 5 minutes at a solution temperature of 60°C, then take them out, rinse them thoroughly in running deionized water, and then take them out and dry them.
[0080] (3) Vacuum coating: Place the pre-treated parts on the turntable in the vacuum chamber, parallel nickel (Ni) palladium in the vacuum chamber of magnetron sputtering, control the turntable speed to 15rpm, adjust the distance between the substrate and the target to 8cm, and the vacuum in the vacuum chamber to 10 -4The working atmosphere is pure argon, the argon flow rate is controlled to be 10 sccm, and the gas pressure is maintained at 0.25 Pa.
[0081] The substrate temperature was adjusted to 350°C, and ion beam cleaning was started with a cleaning voltage of 1500V, a bias voltage of 1500V, a bias duty cycle of 5%, and a cleaning time of 20min. After the ion beam cleaning was completed, the nickel sputtering process was started directly with a nickel (Ni) palladium current of 2A, a negative bias voltage of 200V, and a reactive sputtering time of 30min. A pure nickel (Ni) bonding layer was deposited on the surface of the part. After the sputtering reaction was completed and the substrate temperature dropped to room temperature, the part was taken out and dried for storage.
[0082] (4) Activation treatment: Place the parts that have been vacuum coated into the prepared activation solution, soak them for 15 seconds at a solution temperature of 30°C, take them out and rinse them with water.
[0083] (5) Nickel electroplating: Place the activated parts into the prepared nickel plating solution for nickel plating, with a cathode current density of 1A / dm 2 The reaction temperature is 30℃, pH is 5.0, the reaction time is 20min, and the plate is taken out and cleaned.
[0084] (6) Gold plating: Use the platinum titanium mesh as the anode and the nickel-plated parts as the cathode. Perform gold plating on the nickel-plated parts according to the conventional pure gold plating method. The current density is 0.5A / dm 2 , reaction temperature 62 ℃, pH 5.0, reaction time 13min, take out and clean.
[0085] (7) Performance testing: After the parts are gold-plated according to the above method, the gold layer has fine crystals and uniform color. The coating thickness is tested with an X-ray coating thickness gauge, where the Ni layer is 5.05μm and the Au layer is 2.38μm. The parts are placed in a muffle furnace. When the furnace temperature rises to about 250°C, the coating begins to peel, bubble, and fall off.
[0086] Comparative Example 2:
[0087] The design of the coating system and the optimization of the plating process parameters are one of the main difficulties that the present invention needs to overcome. This comparative example adopts the method of Example 1 to perform surface modification on an electronic packaging shell with a silicon content of 50%, except that the setting of the plating process parameters is not within the range required by the present invention. The specific process is as follows:
[0088] Prepare ultrasonic degreasing cleaning solution: weigh sodium hydroxide, sodium carbonate and sodium phosphate according to the formula and prepare a solution. The composition and content of the prepared cleaning solution are: NaOH 10g / L, Na2CO3 40g / L, Na3PO4 50g / L and deionized water 1L.
[0089] Prepare activation solution: Pour one-third of deionized water into the plating tank, slowly add the measured sulfuric acid into the plating tank, stir thoroughly, add deionized water to the working liquid level, cool to room temperature for use. The composition and content of the prepared activation solution are: 50ml / L sulfuric acid.
[0090] Prepare nickel plating solution: inject one-third of deionized water into the plating tank, add weighed nickel sulfate and fully dissolve it, dissolve weighed nickel chloride separately and add it to the plating tank, dissolve weighed sodium dodecyl sulfate separately and add it to the plating tank, and then dissolve weighed boric acid separately with hot deionized water under boiling and add it to the plating tank, add deionized water to the working liquid level, and adjust the pH value to the required range of the formula with dilute sodium hydroxide solution. The composition and content of the prepared nickel plating solution are: nickel sulfate 180g / L, sodium chloride 50g / L, boric acid 30g / L, sodium dodecyl sulfate 0.08g / L, pH 5.0 at 25℃.
[0091] Preparation of gold plating solution: put the calculated amount of Temperex 9500 pre-bottle liquid into the plating tank and heat it to 65°C, add the calculated amount of gold salt while stirring, stir until the gold salt is completely dissolved, take 500mL of plating solution from the plating tank and cool it to 25°C, measure the pH value and specific gravity, the composition and content of the prepared gold plating solution are: Au (in the form of potassium citrate gold) 8g / L, pH 5.0 under the condition of temperature 25°C.
[0092] (1) Wet sandblasting: Place the processed high-silicon aluminum electronic packaging shell parts into the sandblasting room, adjust the pressure of the sandblasting machine to 0.15Mpa, select 200-mesh glass beads, aim the spray gun at the surface of the parts and turn on the equipment. During the sandblasting process, the angle between the spray gun and the parts needs to be adjusted to ensure that the surface of the parts is evenly sprayed. After sandblasting, take out the parts and rinse them with deionized water, and observe whether there are any missed locations on the surface of the parts.
[0093] (2) Ultrasonic degreasing: Place the sandblasted parts into the prepared ultrasonic degreasing cleaning solution, ultrasonically clean them for 5 minutes at a solution temperature of 60°C, then take them out, rinse them thoroughly in running deionized water, and then take them out and dry them.
[0094] (3) Vacuum coating: The pre-treated parts are placed on a turntable in a vacuum chamber. Titanium (Ti) palladium and copper (Cu) palladium are placed in parallel in the vacuum chamber of magnetron sputtering. The turntable speed is controlled to 15 rpm, and the distance between the substrate and the target is adjusted to 8 cm. The vacuum in the vacuum chamber reaches 10 -4 The working atmosphere is pure argon, the argon flow rate is controlled to be 10 sccm, and the gas pressure is maintained at 0.25 Pa.
[0095] The substrate temperature was adjusted to 200°C, and ion beam cleaning was started with a cleaning voltage of 1500V, a bias voltage of 1500V, a bias duty cycle of 5%, and a cleaning time of 10min. After the ion beam cleaning was completed, the titanium sputtering process was started directly with a titanium (Ti) palladium current of 0.05A, a negative bias voltage of 100V, and a reactive sputtering time of 10min to deposit a pure titanium (Ti) bonding layer on the surface of the part. After the titanium plating process was completed, the copper sputtering process was started directly with a copper (Cu) palladium current of 4A, a bias voltage of 500V, a bias duty cycle of 85%, and a reactive sputtering time of 30min. After the sputtering reaction was completed and the substrate temperature dropped to room temperature, the product was taken out and dried for storage.
[0096] (4) Activation treatment: Place the parts that have been vacuum coated into the prepared activation solution, soak them for 8 seconds at a solution temperature of 30°C, take them out and rinse them with water.
[0097] (5) Nickel electroplating: Place the activated parts into the prepared nickel plating solution for nickel plating, with a cathode current density of 1A / dm 2 The reaction temperature is 33℃, pH is 5.0, the reaction time is 20min, and the plate is taken out and cleaned.
[0098] (6) Gold plating: Use the platinum titanium mesh as the anode and the nickel-plated parts as the cathode. Perform gold plating on the nickel-plated parts according to the conventional pure gold plating method. The current density is 0.5A / dm 2 , reaction temperature 62 ℃, pH 5.0, reaction time 12min, take out and clean.
[0099] (7) Performance testing: After the parts are gold-plated according to the above method, the gold layer has fine crystals and uniform color. The coating thickness is tested with an X-ray coating thickness gauge, where the Ti layer is 0.28μm, the Cu layer is 1.35μm, the Ni layer is 3.32μm, and the Au layer is 2.18μm. The parts are placed in a muffle furnace and the temperature is raised to about 350°C. There is no obvious change in the appearance of the coating. When the temperature exceeds 400°C, the coating begins to peel, bubble, and fall off.
[0100] Comparative Example 3:
[0101] This comparative example uses the gold plating method for high-silicon aluminum composite materials disclosed in Chinese invention patent CN201310553767.2 to modify the surface of an electronic packaging shell with a silicon content of 50%, and the bonding strength of the modified coating meets the 450°C thermal shock assessment requirements. The difference between this comparative example and the present invention is that the method adopted in this comparative example can only meet the surface modification of aluminum-silicon composite materials with a silicon content of ≤50%, the higher the silicon content of the base material, the greater the difficulty of wet electroplating, and the process parameters cannot cover the full range of high-silicon aluminum substrates. In addition, due to the presence of chemical nickel plating and other plating processes in the electroplating process, the hydrogen content inside the shell is too high, which easily causes hydrogen poisoning in the electronic chip.
[0102] Performance comparison test:
[0103] Plating adhesion test: According to the standards specified in Appendix A of GJB 1420A-1999 "General Specification for Semiconductor Integrated Circuit Housings", the modified electronic packaging shell material is placed in a muffle furnace for high-temperature thermal shock testing.
[0104] Hydrogen content test: The hydrogen content of each comparative sample was tested according to the test method of 1018.1 “Internal water vapor content” in GJB 548B-2005.
[0105] Table 1 is a performance comparison of high silicon aluminum composite electronic packaging shell samples after surface modification by the embodiment and the comparative example method:
[0106]
[0107] The above description is only a preferred embodiment of the present invention, which is only illustrative and not restrictive of the present invention. Those skilled in the art understand that many changes, modifications, and even equivalences may be made to the present invention within the spirit and scope defined by the claims of the present invention, but all of them will fall within the scope of protection of the present invention.
Claims
1. A surface modification method for a high silicon aluminum composite material for an electronic packaging shell, characterized in that: The following steps are involved: S1, sandblasting the surface of the high silicon aluminum composite material by wet sandblasting; S2, ultrasonically degreasing and cleaning the high silicon aluminum composite material after sandblasting, rinsing it with water, and drying and storing it; S3, magnetron reactive sputtering titanium-copper metal film on the surface of pre-treated high silicon-aluminum composite material; S4, put the parts after magnetron sputtering treatment into the activation solution, soak for 5-10 seconds at a temperature of 20-35°C, take out and rinse with water; S5, placing the activated parts into a nickel plating solution for nickel plating, and taking them out and cleaning them; S6, use pure gold plate or platinum titanium mesh as anode and high silicon aluminum composite material as cathode, and gold-plate the nickel-plated parts according to the conventional pure gold plating method, and then take them out and clean them.
2. The surface modification method of a high silicon aluminum composite material for an electronic packaging shell according to claim 1, characterized in that: In the step S1, the wet sandblasting uses glass beads of 150-250 meshes, and the sandblasting pressure is set to 0.15-0.2 MPa.
3. The surface modification method of a high silicon aluminum composite material for an electronic packaging shell according to claim 1, characterized in that: In step S2, the ultrasonic degreasing cleaning solution is prepared from 5-10 g / L sodium hydroxide, 30-40 g / L sodium carbonate, 40-50 g / L sodium phosphate and deionized water, the temperature of the ultrasonic degreasing cleaning solution is 55-65° C., and the cleaning time is 3-5 min.
4. The surface modification method of a high silicon aluminum composite material for an electronic packaging shell according to claim 1, characterized in that: In the step S3, during the magnetron sputtering coating process, the substrate temperature is always maintained at 350°C, and the thickness of the Ti layer obtained on the surface of the high-silicon-aluminum composite material is 0.5-1 μm, and the thickness of the Cu layer is 1-3 μm.
5. The surface modification method of a high silicon aluminum composite material for an electronic packaging shell according to claim 1, characterized in that: In the step S3, during the magnetron sputtering coating process, a titanium target and a copper target are arranged in parallel in the vacuum chamber of the magnetron sputtering, a high silicon aluminum composite material is placed on a turntable in the vacuum chamber, the turntable speed is controlled to 15 rpm, the distance between the substrate and the target is adjusted to 8 to 12 cm, and the vacuum in the vacuum chamber reaches 10 -4 The working atmosphere is pure argon, the argon flow rate is controlled at 10-30 sccm, and the gas pressure is maintained at 0.25-0.45 Pa.
6. The surface modification method of a high silicon aluminum composite material for an electronic packaging shell according to claim 1, characterized in that: In step S4, the activation solution is a 50-100 mol / L dilute sulfuric acid solution.
7. The surface modification method of a high silicon aluminum composite material for an electronic packaging shell according to claim 1, characterized in that: In step S5, during the nickel plating process, the cathode current density is 0.5 to 1 A / dm 2 , reaction temperature is 20-35°C, pH is 4.6-5.2, reaction time is 15-25min, and nickel plating layer thickness is 2-5μm.
8. The surface modification method of a high silicon aluminum composite material for an electronic packaging shell according to claim 1, characterized in that: In step S6, during the gold plating process, the current density is 0.2 to 0.8 A / dm 2 , the reaction temperature is 55-70°C, the pH is 4.5-5.5, the reaction time is 10-15min, and the thickness of the gold layer is 2-3μm.
Citation Information
Patent Citations
Gold-plating method of high silicon-aluminum composite material
CN103540935A