Iron-based A-type lattice molecular catalyst as well as preparation method and application thereof
By designing the non-planar structure and synthesis method of iron-based A-type molecular catalyst, the problems of insufficient activity, selectivity and stability in electrochemical reduction of carbon dioxide are solved, and the effect of efficient methanol generation is achieved, which significantly improves the performance of the catalyst.
Patent Information
- Application Number
- CN202411053175.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
Prior Art In the electrochemical reduction process of carbon dioxide, the activity, selectivity and stability of the catalyst are insufficient, especially when there are kinetic limitations in the production of methanol, making it difficult to efficiently reduce CO2 to methanol.
Develop an iron-based A-type molecular catalyst with a non-planar molecular structure. Through specific synthesis steps and ligand design, its electronic structure and steric hindrance are adjusted to form high activity, high selectivity, and high stability. Catalyst, used for electrochemical reduction of CO2 to produce methanol.
It has achieved efficient catalytic electrochemical reduction of CO2 to produce methanol, which has improved the activity and selectivity of the catalyst, solved the problems of poor activity, poor selectivity and poor stability in the prior art, and has better market application prospects.
Smart Images

Figure CN118979269A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of catalytic technology, and in particular to an iron-based A-type lattice molecular catalyst and a preparation method and application thereof. Background Art
[0002] In recent years, the increasing consumption of fuels has led to a continuous increase in the concentration of carbon dioxide in the atmosphere. The electrochemical reduction of carbon dioxide into high-value-added chemical raw materials using renewable but intermittent electricity from wind, solar and tidal energy can effectively reduce the concentration of carbon dioxide in the atmosphere and produce fuels or value-added chemicals. However, due to the high kinetic inertness and thermodynamic stability of carbon dioxide, coupled with the competitive hydrogen evolution reaction, its conversion is limited. In addition, during the electrocatalytic reduction of carbon dioxide, the thermodynamic redox potentials of different products are similar, so the selectivity is low. Therefore, it remains a severe challenge to develop efficient and stable catalysts to achieve the selective conversion of carbon dioxide into desired products.
[0003] At present, researchers have developed a series of electrocatalysts for electrocatalytic carbon dioxide reduction, including metal-based catalysts, metal-free carbon-based catalysts, molecular catalysts, etc. Among them, molecular catalysts have significant advantages, and the primary and secondary coordination spheres can be adjusted by manipulating the coordination environment and the stereo and electronic effects of the ligands. Therefore, by rationally optimizing the ligand structure, the catalytic efficiency and product selectivity can be adjusted. In addition, the unique atomic configuration of molecular catalysts limits the effective binding of *H to the central metal, forcing the HER to proceed through the high-energy barrier Volmer-Heyrovsky pathway to improve the efficiency of CO2 reduction reaction. Since the first report of CO2's reducing ability in 1974, molecular catalysts have made rapid progress in the field of CO2 reduction reaction (CO2RR) in recent years. Among them, porphyrins, phthalocyanines, and their derivatives centered on cobalt (Co), iron (Fe), and nickel (Ni) have become the most widely studied molecular catalysts. However, these catalysts mainly reduce CO2 to two-electron CO or HCOOH. So far, the only metals that can catalyze CO2 electroreduction to produce multi-electron products with considerable activity and selectivity are cobalt and copper. The six-electron product methanol from deep reduction is more popular due to its high energy density and liquid fuel properties that are easy to store and transport. However, the electrochemical reduction of CO2 to CH3OH involves multiple proton-coupled electron transfer processes, which makes the reaction limited by slow kinetics. In this context, it is of great significance to design efficient and stable molecular catalysts to selectively produce methanol.
[0004] Highly dispersed active centers are essential for the electrochemical reduction of CO2 to CH3OH. Loading planar molecules on substrate materials is a common method to achieve highly dispersed active centers. In the process of electrochemical reduction of CO2 to methanol, multiple intermediates and transition states are involved, which significantly change the activity and selectivity. Based on the Sabatier principle, the adsorption strength of CO intermediates is widely believed to play a key role in the selectivity of electrochemical CO2 reduction. Therefore, regulating the adsorption strength between electrocatalysts and CO intermediates by adjusting the local electronic structure of electrocatalysts is crucial for the formation of CH3OH. Nanolattice molecules are a class of closed-loop molecules that use fluorene or fluorene-like structures as the basic modules for building lattices and are assembled through the concept of multi-molecule integrated design. These molecules can regulate their aggregation structure by adjusting the steric hindrance. In addition, nanolattice molecules have the dual advantages of the modifiability of organic molecules and the size scalability of framework materials.
[0005] Therefore, it is of great significance to develop a catalyst based on the lattice strategy and use it to efficiently produce methanol. Summary of the invention
[0006] Purpose of the invention: The technical problem to be solved by the present invention is to provide an iron-based A-type lattice molecular catalyst and its preparation method and application in view of the deficiencies in the prior art. Based on the unique chemical structure of the molecular catalyst, CO2 can be reduced to methanol with high activity, high selectivity and high stability, providing some theoretical and technical guidance for promoting CO2 emission reduction and resource utilization.
[0007] In order to solve the above technical problems, the present invention discloses an iron-based A-type lattice (FeAG) molecular catalyst, the molecular structure of which is non-planar, and the general structural formula is as follows:
[0008]
[0009] The present invention also discloses a method for preparing an iron-based A-type lattice molecular catalyst.
[0010] The specific preparation steps are as follows:
[0011] S1. Add 2-bromofluorenone solution to the reaction vessel, slowly add phenylmagnesium bromide solution under nitrogen protection at room temperature, then heat to 80-90°C and react for 4-10 hours. After the reaction, quench the reaction with saturated ammonium chloride solution, remove tetrahydrofuran solvent by rotary evaporation, then add a large amount of water to precipitate the solid, and stir to remove inorganic salts. Filter and wash with a large amount of deionized water to obtain a crude product. The crude product is eluted through a column to obtain 2-bromo-9-phenyl-9H-fluorenol;
[0012] S2. Add 2-bromo-9-phenyl-9H-fluorenol, bipyraclostrobin, [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride and potassium acetate into a sealed reaction vessel, evacuate and blow nitrogen for 3 times, inject dry 1,4-dioxane under nitrogen protection to form a first mixed solution, control the temperature at 100-110° C. to react for 8-15 hours, extract, dry, filter and evaporate the solvent under reduced pressure to obtain a crude product after the reaction is completed, and pass the crude product through a column to obtain 9-phenyl-2-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-9H-fluorenol;
[0013] S3. 3,6-dibromocarbazole, ethyl bromide, sodium hydroxide, tetrabutylammonium bromide and acetone are added to a reaction vessel to form a second mixed solution, and the temperature is controlled to be 60-70° C. and refluxed with stirring for 1.5-3 hours. After the reaction, the crude product is extracted, dried, filtered, and evaporated under reduced pressure to obtain a crude product, and the crude product is eluted through a column to obtain 3,6-dibromoethylcarbazole;
[0014] S4. 3,6-dibromoethylcarbazole, 9-phenyl-2-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-9H-fluorenol and Pd(PPh3)4 are added to a reaction vessel in a light-proof state. Subsequently, the reaction system is evacuated and replaced with nitrogen several times to ensure an oxygen-free environment. A toluene / tetrahydrofuran mixture bubbled with nitrogen is injected, and then a K2CO3 / KF aqueous solution is injected to obtain a third mixed solution. The reaction system is sealed and connected to a nitrogen balloon. The temperature is controlled at 90 to 100°C and stirred for 1.5 to 3 hours. After the reaction is completed, the crude product is extracted, dried, filtered, and the solvent is evaporated under reduced pressure to obtain a crude product. The crude product is eluted through a column to obtain type A synthon AOH;
[0015] S5. Add BF3·Et2O to the 4-methyl-N,N-diphenylaniline solution, slowly dropwise add the A-type synthon AOH solution, stir and react for 5-10 minutes after the dropwise addition, add water to quench the reaction after the reaction, extract, dry, filter, evaporate the solvent under reduced pressure to obtain a crude product, and elute the crude product through a column to obtain the A-type lattice molecule AG;
[0016] S6. Evenly mix the A-type lattice molecule AG solution and the FeCl3 solution, and stir the reaction at room temperature for 10 to 15 hours. After the reaction is completed, evaporate the solvent under reduced pressure, wash with deionized water, and remove the unreacted FeCl3 by centrifugation to obtain the iron-based A-type lattice molecule FeAG.
[0017] Wherein, in step S1, the molar ratio of 2-bromofluorenone to phenylmagnesium bromide is 1:(1.5-3.5); the concentration of the 2-bromofluorenone solution is 0.2-0.6 mol / L; the concentration of the phenylmagnesium bromide solution is 1-4 mol / L; the solvent of the 2-bromofluorenone solution and the phenylmagnesium bromide solution is tetrahydrofuran;
[0018] Wherein, in step S2, the molar ratio of 2-bromo-9-phenyl-9H-fluorenol, bipyraclostrobin, [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride and potassium acetate is 1:(1-2):(0.05-0.15):(2-3.5); the solvent of the first mixed solution is 1,4-dioxane; the concentration of the 2-bromo-9-phenyl-9H-fluorenol is 0.1-0.3M;
[0019] Wherein, in step S3, the molar ratio of 3,6-dibromocarbazole, ethyl bromide, sodium hydroxide and tetrabutylammonium bromide is 1:(1-1.5):(0.5-1.5):(0.05-0.2); the solvent of the second mixed solution is acetone; the concentration of the 3,6-dibromocarbazole is 0.1-0.3M;
[0020] Wherein, in step S4, the molar ratio of 3,6-dibromoethylcarbazole, 9-phenyl-2-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-9H-fluorenol and Pd(PPh3)4, K2CO3, and KF is 1:(2-4):(0.05-0.2):(2.5-5):(2.5-5); the solvent in the third mixed solution is toluene and tetrahydrofuran, and the volume ratio is 1:1; the concentration of the 3,6-dibromoethylcarbazole is 0.1-0.3M; the concentration of the K2CO3 / KF aqueous solution is 1.5-3M;
[0021] Wherein, in step S5, the molar ratio of BF3·Et2O, 4-methyl-N,N-diphenylaniline and type A synthon AOH is (5-15):(1-2):1; the solvent of the 4-methyl-N,N-diphenylaniline solution is dichloromethane, and the concentration is 0.001-0.003 mol / L; the solvent of the type A synthon AOH solution is dichloromethane, and the concentration is 0.001-0.003 mol / L; the dropwise addition rate of the type A synthon AOH solution is 0.78-2.4 mL / min, and the dropwise addition time is 1.5-2 h;
[0022] Among them, in step S6, the molar ratio of type A lattice molecule AG to FeCl3 is 1:(1.5~2); the solvent of the type A lattice molecule AG solution is dichloromethane; the solvent of the FeCl3 solution is ethanol; the volume ratio of dichloromethane to ethanol is (1~2.5):1.
[0023] Specifically, in some embodiments of the present invention, the working electrode is prepared using the iron-based A-type lattice molecule FeAG, and the specific steps are:
[0024] S1. Add the iron-based A-type lattice molecule FeAG to ethanol, then add the Nafion solution, and ultrasonicate for 30 minutes to fully disperse it;
[0025] S2. Take the solution prepared in step S1 and evenly drop it on a piece of carbon paper, and then dry it naturally to obtain the working electrode of iron-based A-type lattice molecule FeAG.
[0026] Specifically, in some embodiments of the present invention, a working electrode prepared with iron-based A-type lattice molecules FeAG electrocatalyzes CO2 reduction to produce methanol in an electrochemical experiment.
[0027] Beneficial effects:
[0028] 1. The iron-based A-type lattice molecules disclosed in the present invention have non-planar and large steric hindrance characteristics. The non-planar and large steric hindrance molecular structure effectively inhibits the aggregation of molecules, is conducive to the high exposure of active sites, and promotes the efficient transfer of electrons.
[0029] 2. The iron-based A-type lattice molecular catalyst disclosed in the present invention can efficiently catalyze the electrochemical reduction of CO2 to produce methanol, solving the problems of poor activity, poor selectivity and poor stability of molecular electrocatalysts in the production of methanol by carbon dioxide reduction, and has better market application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.
[0031] Figure 1 It is a transmission electron microscope (TEM) image of the iron-based A-type lattice molecular catalyst in the embodiment of the present invention;
[0032] Figure 2 This is an energy dispersive X-ray (EDX) elemental spectrum of the iron-based A-type lattice molecular catalyst in the embodiment of the present invention;
[0033] Figure 3 is an X-ray photoelectron spectrometer (XPS) diagram of the iron-based A-type lattice molecular catalyst in an embodiment of the present invention;
[0034] Figure 4 is the X-ray absorption spectrum (XAS) of the iron-based A-type lattice molecular catalyst in the embodiment of the present invention;
[0035] Figure 5 This is a Faraday efficiency distribution diagram of CO2 reduction products of the iron-based A-type lattice molecular catalyst at different potentials in an embodiment of the present invention;
[0036] Figure 6 This is a test diagram of selectivity of CO2 reduction to produce methanol using an iron-based A-type lattice molecular catalyst in an embodiment of the present invention;
[0037] Figure 7 This is a test diagram of the CO2 reduction stability of the iron-based A-type lattice molecular catalyst in an embodiment of the present invention. DETAILED DESCRIPTION
[0038] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0039] Example 1: Preparation of FeAG-based A-type lattice molecular catalyst
[0040] The following figure shows the synthesis route of the iron-based A-type lattice molecule FeAG in this example:
[0041]
[0042] The specific synthesis steps are as follows:
[0043] S1. Synthesis of 2-bromo-9-phenyl-9H-fluorenol:
[0044] 2-Bromofluorenone 1 (5.2 g, 20 mmol) was placed in a sealed flask, and vacuumed and nitrogen-filled for 3 times. Dry tetrahydrofuran (50 mL) was added to the flask under nitrogen protection. A dry tetrahydrofuran solution (18 mL) of phenylmagnesium bromide 2 (9 g, 50 mmol) was slowly added to the flask under nitrogen protection at room temperature, and then the temperature was raised to 85°C and reacted for 6 hours. After the reaction was completed, the reaction was quenched with a saturated ammonium chloride solution, the tetrahydrofuran solvent was removed by rotary evaporation, and then a large amount of water was added to precipitate the solid, and the inorganic salt was removed by stirring. The crude product was filtered and washed with a large amount of deionized water to obtain a crude product. The crude product was separated and purified by column chromatography using 200-300 mesh silica gel, and a mixed solution of petroleum ether and dichloromethane (volume ratio of 4:1) was used as the eluent to obtain 2-bromo 9-phenyl-9H-fluorenol.
[0045] S2. Synthesis of 9-phenyl-2-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-9H-fluorenol:
[0046] 2-Bromo-9-phenyl-9H-fluorenol 3 (2.9 g, 8.5 mmol) synthesized in step S1, biboric acid pinacol ester 4 (2.6 g, 10.2 mmol), [1,1'-bis(diphenylphosphino)ferrocene] palladium dichloride (Pd(dppf)Cl2) (617 mg, 0.85 mmol) and potassium acetate (2 g, 20.4 mmol) were placed in a flask and sealed, and vacuumed and nitrogen-filled for 3 times. Dry 1,4-dioxane (50 mL) was injected into the flask under nitrogen protection and reacted at 105°C for 12 h. After the reaction was completed, the organic phase was extracted with dichloromethane. Then it was dried with anhydrous sodium sulfate, filtered, and the solvent was evaporated under reduced pressure. The crude product was separated and purified by column chromatography using 200-300 mesh silica gel and a mixed solution of petroleum ether and dichloromethane (volume ratio of 1:1) as an eluent to obtain 9-phenyl-2-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-9H-fluorenol 5.
[0047] S3. Synthesis of 3,6-dibromoethylcarbazole:
[0048] 3,6-dibromocarbazole 6 (15 g, 46.2 mmol), bromoethane 7 (5 g, 46.2 mmol), sodium hydroxide (1.8 g, 46.2 mmol) and tetrabutylammonium bromide (1.5 g, 4.62 mmol) were added to a three-necked flask, followed by acetone (308 mL), and the mixture was stirred under reflux in an oil bath at 65 °C for 2 hours. After the reaction, the organic phase was extracted with dichloromethane. The mixture was then dried over anhydrous sodium sulfate, filtered, and the solvent was evaporated under reduced pressure. The crude product was separated and purified by column chromatography using 200-300 mesh silica gel with petroleum ether as the eluent to obtain 3,6-dibromoethylcarbazole 8.
[0049] S4. Synthesis of Compound A-type Synthon AOH:
[0050] 3,6-dibromoethylcarbazole 8 (3 g, 8.5 mmol) synthesized in step S3, 9-phenyl-2-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-9H-fluorenol 5 (11.4 g, 29.75 mmol) synthesized in step S2 and Pd(PPh3)4 catalyst (1 g, 0.85 mmol) (protected from light) were added to a three-necked flask. Subsequently, the reaction system was evacuated and replaced with nitrogen several times to ensure an anaerobic environment. A nitrogen-bubbled toluene / tetrahydrofuran mixture (volume ratio 1:1, 42.5 mL) and a K2CO3 / KF aqueous solution (K2CO3 / KF molar ratio 1:1, 2 M, 29.75 mL) were injected into the flask through a syringe. The reaction system was sealed and connected to a nitrogen balloon. The reaction was stirred in an oil bath at 95°C for 2 hours. After the reaction, the organic phase was extracted with dichloromethane. The crude product was then dried over anhydrous sodium sulfate, filtered, and the solvent was evaporated under reduced pressure. The crude product was separated and purified by column chromatography using 200-300 mesh silica gel and a mixed solution of petroleum ether, dichloromethane and ethyl acetate (ratio 6:1:1) as eluent to obtain Type A synthon AOH.
[0051] S5. Synthesis of compound A-type lattice molecule AG:
[0052] 4-Methyl-N,N-diphenylaniline 9 (73.3 mg, 0.283 mmol) was placed in a reaction bottle, dichloromethane (142 mL) was added to dissolve and stir, and then BF3·Et2O (401.7 mg, 2.83 mmol) was added. AOH (200 mg, 0.283 mmol) synthesized in step S4 was dissolved in dichloromethane solution (142 mL) and placed in a constant pressure dropping funnel, and the AOH solution was slowly added dropwise to the reaction bottle at a dropping rate of 0.78-2.4 mL / min, and the dropping time was about 2 hours. After the addition was completed, stirring was continued for 5 minutes. After the reaction was completed, water was added to quench the reaction, and the organic phase was extracted with dichloromethane. Then it was dried with anhydrous sodium sulfate, filtered, and the solvent was evaporated under reduced pressure. The crude product was separated and purified by column chromatography with 200-300 mesh silica gel, and a mixed solution of petroleum ether and dichloromethane (volume ratio of 3:1) was used as the eluent to obtain the A-type lattice molecule AG.
[0053] S6. Synthesis of iron-based A-type lattice molecules FeAG:
[0054] Take the A-type lattice molecule AG (100.0 mg, 0.108 mmol) synthesized in step S5 and add it to a flask, followed by 50 mL of dichloromethane. Then FeCl3 (35.0 mg, 0.216 mmol) was dissolved in 25 mL of ethanol and added to the flask. The reaction mixture was stirred at room temperature for 12 hours. After the reaction was completed, the solvent was evaporated under reduced pressure. Then, it was washed with deionized water and centrifuged to remove the unreacted FeCl3 to obtain the iron-based A-type lattice molecule FeAG.
[0055] Example 2: Preparation of working electrode using iron-based A-type lattice molecule FeAG
[0056] S1. The iron-based A-type lattice molecule FeAG complex (2 mg) was added to ethanol (200 μL), followed by a 5 wt.% Nafion solution (20 μL), and ultrasonicated for 30 minutes to fully disperse it;
[0057] S2. Take 100 μL of the solution prepared in step S1 and evenly drop it on a piece of carbon paper (1×1 square centimeter), and then dry it naturally to obtain the working electrode of iron-based A-type lattice molecule FeAG.
[0058] Example 3: Electrochemical reduction of CO2 test
[0059] For the H-type electrolytic cell test, Ag / AgCl and platinum sheet were used as reference electrode and counter electrode respectively, and the electrode prepared by S2 in Example 2 was used as working electrode. The cathode and anode were separated by Nafion 117 proton exchange membrane. Each chamber was equipped with 20 ml of 0.5M KHCO3 solution electrolyte. Before all electrochemical measurements, CO2 was introduced into the cathode chamber for half an hour to saturate the dissolution of CO2 in the electrolyte. During the electrolysis process, the flow rate of CO2 was controlled to be 20sccm. The electrochemical measurements were controlled and recorded using a CHI 650E potentiometer. The gas products were monitored by online gas chromatography (GC 7890B, Agilent), and the liquid products after the reaction were measured by nuclear magnetic resonance (600MHz 1 H NMR, Bruker Advance).
[0060] Example 4: Characterization and performance testing
[0061] 1. Characterization of FeAG: The iron-based A-type lattice molecule FeAG obtained in Example 1 was characterized by transmission electron microscopy (TEM), X-ray photoelectron spectrometer (XPS) and X-ray absorption spectroscopy (XAS).
[0062] The characterization results are as follows Figures 1 to 4 shown. Figure 1 TEM image of FeAG obtained in Example 1; Figure 1As can be seen from 1a, FeAG presents a nanosheet structure, which is conducive to the uniform distribution of active sites and the rapid transfer of multiple electrons; as can be seen from 1b, there are no Fe clusters or particles on FeAG, which is conducive to electrochemical CO2 reduction. Figure 2 is the energy dispersive X-ray (EDX) elemental spectrum of FeAG obtained in Example 1; Figure 2 It can be seen that the elements Fe, C, N, and Cl are evenly distributed on FeAG, which is crucial for efficient CO2 electrochemical reduction. Figure 3 is the XPS graph of FeAG obtained in Example 1; Figure 3 a It can be seen that the valence state of Fe atoms in FeAG is between +2 and +3; Figure 3 b It can be seen that there are CC / C=C, CN and Fe-C bonds in FeAG; Figure 3 c It can be seen that there are pyrrolic nitrogen, graphitic nitrogen and Fe-N bonds in FeAG; Figure 3 d It can be seen that there are Cl atoms in FeAG. Figure 4 is the X-ray absorption spectrum (XAS) of FeAG obtained in Example 1; Figure 4 a It can be seen that the valence state of Fe atoms in FeAG is between +2 and +3; Figure 4 b It can be seen that there are Fe-C / N and Fe-Cl bonds in FeAG, but no Fe-Fe bonds.
[0063] 2. Test of FeAG catalytic effect:
[0064] Figure 5 This is the Faraday efficiency distribution diagram of CO2 reduction products of FeAG catalyst obtained in Example 1 at different potentials. It can be seen from the figure that methanol is the only liquid product, and the Faraday efficiency is the highest at -0.8V, reaching 49.4%;
[0065] Figure 6 This is a test diagram of the selectivity of CO2 reduction to methanol produced by the FeAG catalyst obtained in Example 1. It can be seen from the figure that the selectivity of CO2 converted to methanol is 96.8% at -0.8V;
[0066] Figure 7 This is a test graph of the CO2 reduction stability of the FeAG catalyst obtained in Example 1 at -0.8V. It can be seen from the figure that the catalyst can work stably for 20 hours.
[0067] The present invention provides an iron-based A-type lattice molecular catalyst and its preparation method and application. There are many methods and ways to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements can be made without departing from the principle of the present invention. These improvements should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.
Claims
1. An iron-based A-type lattice molecular catalyst, characterized in that: The molecular structure is non-planar, and the general structure is as follows:
2. The method for preparing an iron-based A-type lattice molecular catalyst according to claim 1, characterized in that: The specific preparation steps are as follows: S1. Add 2-bromofluorenone solution into a reaction vessel, slowly add phenylmagnesium bromide solution under nitrogen protection at room temperature, then raise the temperature to 80-90°C, react for 4-10 hours, and obtain 2-bromo-9-phenyl-9H-fluorenol; S2. Add 2-bromo-9-phenyl-9H-fluorenol, bipyraclostrobin, [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride and potassium acetate into a reaction vessel, inject dry 1,4-dioxane to form a first mixed solution, control the temperature at 100-110° C. to react for 8-15 hours to obtain 9-phenyl-2-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-9H-fluorenol; S3. 3,6-dibromocarbazole, ethyl bromide, sodium hydroxide, tetrabutylammonium bromide and acetone are added to a reaction vessel to form a second mixed solution, and the temperature is controlled to 60 to 70° C. for 1.5 to 3 hours to obtain 3,6-dibromoethylcarbazole; S4. 3,6-dibromoethylcarbazole, 9-phenyl-2-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-9H-fluorenol and Pd(PPh3)4 are added to a reaction vessel, a nitrogen-bubbled toluene / tetrahydrofuran mixed solution is injected, and then a K2CO3 / KF aqueous solution is injected to obtain a third mixed solution, and the temperature is controlled at 90-100°C for reaction for 1.5-3h to obtain type A synthon AOH; S5. Add BF3·Et2O to the 4-methyl-N,N-diphenylaniline solution, slowly dropwise add the A-type synthon AOH solution, and stir the reaction at room temperature for 5 to 10 minutes after the dropwise addition to obtain the A-type lattice molecule AG; S6. Evenly mix the A-type lattice molecule AG solution and the FeCl3 solution, and stir the reaction at room temperature for 10 to 15 hours to obtain the A-type lattice molecule FeAG.
3. The preparation method according to claim 2, wherein in step S1, the molar ratio of 2-bromofluorenone to phenylmagnesium bromide is 1:(1.5-3.5); the concentration of the 2-bromofluorenone solution is 0.2-0.6 mol / L; the concentration of the phenylmagnesium bromide solution is 1-4 mol / L; and the solvent of the 2-bromofluorenone solution and the phenylmagnesium bromide solution is tetrahydrofuran.
4. The preparation method according to claim 2, wherein in step S2, the molar ratio of 2-bromo-9-phenyl-9H-fluorenol, bipyraclostrobin, [1,1'-bis(diphenylphosphino)ferrocene]palladium dichloride and potassium acetate is 1:(1-2):(0.05-0.15):(2-3.5); the solvent of the first mixed solution is 1,4-dioxane; and the concentration of the 2-bromo-9-phenyl-9H-fluorenol is 0.1-0.3M.
5. The preparation method according to claim 2, wherein in step S3, the molar ratio of 3,6-dibromocarbazole, ethyl bromide, sodium hydroxide and tetrabutylammonium bromide is 1:(1-1.5):(0.5-1.5):(0.05-0.2); the solvent of the second mixed solution is acetone; and the concentration of the 3,6-dibromocarbazole is 0.1-0.3M.
6. The preparation method according to claim 2, wherein in step S4, the molar ratio of 3,6-dibromoethylcarbazole, 9-phenyl-2-(4,4,5,5-tetramethyl-1,3,2-dioxaborolan-2-yl)-9H-fluorenol and Pd(PPh3)4, K2CO3, and KF is 1:(2-4):(0.05-0.2):(2.5-5):(2.5-5); the solvent in the third mixed solution is toluene and tetrahydrofuran in a volume ratio of 1:1; the concentration of 3,6-dibromoethylcarbazole is 0.1-0.3M; and the concentration of the K2CO3 / KF aqueous solution is 1.5-3M.
7. The preparation method according to claim 2, wherein in step S5, the molar ratio of BF3·Et2O, 4-methyl-N,N-diphenylaniline and type A synthon AOH is (5-15):(1-2):1; the solvent of the 4-methyl-N,N-diphenylaniline solution is dichloromethane, and the concentration is 0.001-0.003 mol / L; the solvent of the type A synthon AOH solution is dichloromethane, and the concentration is 0.001-0.003 mol / L; the dropping rate of the type A synthon AOH solution is 0.78-2.4 mL / min, and the dropping time is 1.5-2 h.
8. The preparation method according to claim 2, wherein in step S6, the molar ratio of type A lattice molecule AG to FeCl3 is 1:(1.5-2); the solvent of the type A lattice molecule AG solution is dichloromethane; the solvent of the FeCl3 solution is ethanol; and the volume ratio of the dichloromethane to the ethanol is (1-2.5):
1.
9. Use of the iron-based A-type lattice molecular catalyst according to claim 1 in the preparation of an electrocatalytic working electrode.
10. Use of the iron-based A-type lattice molecular catalyst according to claim 1 in the production of methanol by electrocatalytic CO2 reduction.