Alloy oxide catalyst with hollow core-shell structure as well as preparation method and application of alloy oxide catalyst

By using the secondary reduction method to prepare iridium ruthenium alloy oxide catalyst with hollow core-shell structure in PEM electrolytic hydrogen production technology, the problems of large amount of precious metals and poor durability are solved, the efficiency and stability of the catalyst are improved, and the efficiency and stability of the catalyst are improved, and the Commercial application of technology.

CN118979278APending Publication Date: 2024-11-19山东国创燃料电池技术创新中心有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411054301.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the existing PEM electrolytic hydrogen production technology, the amount of precious metal materials is used in the catalyst, which leads to high cost and poor durability and low catalytic efficiency, making it difficult to achieve large-scale commercial application.

Method used

The secondary reduction method is used to prepare an iridium ruthenium alloy oxide catalyst with a hollow core-shell structure. The core structure is protected by forming a uniformly dense iridium-based oxide shell layer, which improves the structural stability and reactivity of the catalyst, and through the regulation group The nanostructured catalyst is formed by proportion and particle size.

Benefits of technology

It reduces the amount of precious metals, improves the catalytic efficiency and durability of the catalyst, reduces manufacturing costs, and maintains stability in high-temperature and high-pressure environments, significantly improving the stability of hydrogen production by electrolyzed water and the continuous operation ability of the system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979278A_ABST
    Figure CN118979278A_ABST
Patent Text Reader

Abstract

The invention provides an alloy oxide catalyst with a hollow core-shell structure as well as a preparation method and application of the alloy oxide catalyst. The method comprises the following steps: performing primary mixing on a first iridium-based precursor, a ruthenium-based precursor, a carrier material and a first solvent, and performing secondary heating treatment and primary reaction to obtain a first reaction solution; and mixing the first reaction solution, a second iridium-based precursor and a second solvent for the second time, and carrying out a second reaction and oxidation treatment to obtain the alloy oxide catalyst with the hollow core-shell structure. The alloy oxide catalyst with the hollow core-shell structure provided by the invention not only reduces the use amount of noble metal so as to reduce the cost, but also can improve the catalytic efficiency, structural stability and durability of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst materials, and in particular relates to an alloy oxide catalyst with a hollow core-shell structure and a preparation method and application thereof. Background Art

[0002] At present, proton exchange membrane (PEM) water electrolysis hydrogen production technology is a method for producing high-purity hydrogen with significant environmental advantages and application potential. However, despite its advantages in safety, reliability and flexibility in combination with renewable energy, its large-scale commercial application still faces some challenges: for example, compared with other water electrolysis hydrogen production technologies, PEM water electrolysis hydrogen production technology has a certain gap in manufacturing cost, hydrogen production efficiency and reliability. Therefore, overcoming the above problems is the key to achieving large-scale application of PEM water electrolysis hydrogen production technology.

[0003] The commercial catalysts in the PEM water electrolysis hydrogen production technology disclosed in the prior art need to use expensive precious metal materials (such as iridium, platinum, etc.), and the resources of the above precious metal materials are scarce. However, in order to ensure the good performance and durability of the membrane electrode, the amount of precious metal materials is relatively large. At present, the iridium metal loading of commercial membrane electrodes is mostly 1.5-3 mg / cm 2 , resulting in higher catalyst costs in the membrane electrode, making it difficult to reduce the manufacturing cost of the entire PEM water electrolysis hydrogen production process.

[0004] In order to solve the above problems, Chinese patent CN115896841A discloses a method for preparing a core-shell structure catalyst that improves the activity of an iridium-based electrolytic water catalyst and reduces the amount of iridium metal used, specifically including using metal oxides such as titanium dioxide as carriers of iridium-based catalysts, and loading iridium-based oxide electrolytic water catalysts on their surfaces. Although this method can reduce the amount of iridium precious metal used, titanium oxide itself has low electrical conductivity and does not have electrolytic water catalytic activity, the electrical conductivity and catalytic activity of the prepared catalyst are both low, and the particle size of the prepared catalyst is large, and the particle distribution is uneven, but the catalyst's own performance and electrical conductivity are greatly damaged.

[0005] In addition, the PEM water electrolysis hydrogen production catalyst used in the existing technology still has technical problems such as low catalytic efficiency and poor durability. At the same time, since the catalyst is in a corrosive environment of high temperature, high pressure and high potential for a long time during the water electrolysis hydrogen production process, the catalyst will fall off, degrade or deactivate during the subsequent operation process, thereby affecting the stability of water electrolysis hydrogen production and the continuous operation capability of the system.

[0006] Therefore, in this field, there is an urgent need to develop a technical means to reduce the amount of precious metals in the catalyst and improve the catalytic efficiency and durability of the catalyst, so as to realize the large-scale application of PEM water electrolysis hydrogen production technology. Summary of the invention

[0007] In view of the shortcomings of the prior art, the object of the present invention is to provide an alloy oxide catalyst with a hollow core-shell structure and a preparation method and application thereof. The alloy oxide catalyst with a hollow core-shell structure provided by the present invention not only reduces the amount of precious metals used to reduce costs, but also can improve the catalytic efficiency, structural stability and durability of the catalyst.

[0008] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing an alloy oxide catalyst having a hollow core-shell structure, the method comprising the following steps:

[0010] The first iridium-based precursor, the ruthenium-based precursor, the carrier material and the first solvent are mixed for the first time, and subjected to a secondary heating treatment and a first reaction to obtain a first reaction solution;

[0011] The first reaction solution, the second iridium-based precursor and the second solvent are mixed for a second time, and subjected to a second reaction and oxidation treatment to obtain the alloy oxide catalyst having a hollow core-shell structure.

[0012] First, compared with the conventional one-step reduction preparation method, the present invention adopts a secondary reduction method to prepare an alloy oxide catalyst with a hollow core-shell structure, which can not only form a uniform, dense and stable iridium-based oxide (IrO x ) shell structure, which is used to treat the alloy oxide (IrRuO x ) The core structure forms an effective protective effect, and can also effectively inhibit the loss of active components in the core structure, thereby improving the structural stability and durability of the catalyst; secondly, there is an obvious hollow structure between the core and shell of the catalyst in the present invention, which greatly increases the specific surface area of ​​the catalyst, promotes the generation of more catalytic active sites, and thus can improve the reaction activity and catalytic efficiency of the catalyst. In addition, the preparation method provided by the present invention can achieve a high yield without using an alkaline solution to adjust the pH value of the solution, is safe to operate, and does not pollute the environment.

[0013] Finally, the present invention optimizes the preparation method and then regulates the component ratio and particle size in the core-shell structure, and finally forms a nanostructured catalyst with an iridium-ruthenium alloy oxide as the core and an iridium-based oxide as the shell. On the one hand, the iridium-ruthenium alloy oxide core itself has sufficient corrosion resistance, and the layered iridium-based oxide shell has controllable proton exchange and charge balance capabilities, which can inhibit surface reconstruction and the formation of soluble iridium and ruthenium species during the catalytic process, thereby further improving the structural stability of the catalyst; on the other hand, the above catalyst not only reduces the amount of precious metal Ir used, saves costs, but also improves its surface electronic properties, thereby further improving the catalytic activity.

[0014] Preferably, the first iridium-based precursor includes any one of chloroiridic acid, ammonium chloroiridate, potassium chloroiridate, ammonium chloroiridate or potassium chloroiridate, or a combination of at least two of them.

[0015] Preferably, the ruthenium-based precursor includes ruthenium chloride and hydrates thereof.

[0016] Preferably, the mass ratio of iridium atoms in the first iridium-based precursor to ruthenium atoms in the ruthenium-based precursor is 1:(0.3-3), preferably 1:2, for example, it can be 1:0.3, 1:0.5, 1:0.8, 1:1, 1:1.2, 1:1.5, 1:1.8, 1:2, 1:2.2, 1:2.5, 1:2.8, 1:3, etc.

[0017] In the present invention, by regulating the mass ratio of iridium atoms in the first iridium-based precursor and ruthenium atoms in the ruthenium-based precursor, the alloy oxide catalyst has the best catalytic activity and durability. Too low a mass ratio will cause poor durability, and vice versa, it will lead to insufficient activity of the alloy oxide catalyst.

[0018] Preferably, the support material comprises an undoped or doped carbon support material.

[0019] Preferably, the doped element includes at least one of nitrogen, boron, sulfur or phosphorus.

[0020] Preferably, the carbon support material includes any one of carbon black, graphitized carbon, porous carbon, carbon nanotubes, carbon nanofibers, graphene or carbon aerogel, or a combination of at least two thereof.

[0021] In the present invention, the carbon support material is a commercially available material in the art, and the present invention is not limited thereto.

[0022] Preferably, the mass ratio of the total mass of the first iridium-based precursor and the ruthenium-based precursor to the carrier material is (1-10):1, preferably 5:1, for example, it can be 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, etc.

[0023] In the present invention, by regulating the mass ratio of the total mass of the first iridium-based precursor and the ruthenium-based precursor to the carrier material, an appropriate amount of iridium metal ions and ruthenium metal ions can be loaded onto the surface of the carrier material through electrostatic adsorption. If the mass ratio is too low, the adsorption amount will be too low, thereby reducing the effective loading capacity of the metal ions. Otherwise, it will cause redundancy of metal ions and fail to be completely adsorbed.

[0024] Preferably, the first solvent comprises a reducing alcohol solvent.

[0025] Preferably, the reducing alcohol solvent includes any one of ethanol, propanol, n-propanol, ethylene glycol, isopropanol or glycerol, or a combination of at least two thereof.

[0026] Preferably, the mass ratio of the total mass of the first iridium-based precursor and the ruthenium-based precursor to the first solvent is 1:(5-20), for example, it can be 1:5, 1:6, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, etc.

[0027] Preferably, the first surfactant is further added before the first mixing.

[0028] Preferably, the first surfactant comprises polyvinylpyrrolidone (PVP) and / or cetyltrimethylammonium bromide (CTAB).

[0029] Preferably, the mass ratio of the first surfactant to the first solvent is 1:(10-50), preferably 1:30, for example, it can be 1:10, 1:12, 1:15, 1:18, 1:20, 1:22, 1:25, 1:28, 1:30, 1:32, 1:35, 1:38, 1:40, 1:42, 1:45, 1:48, 1:50, etc.

[0030] In the present invention, the mass ratio of the first surfactant to the first solvent is adjusted to achieve the best dispersed particle size of the precursor. Too low a mass ratio will cause the precursor to agglomerate, whereas too high a mass ratio will cause the first surfactant content to be excessive, resulting in spontaneous polymerization.

[0031] Preferably, the first mixing comprises ultrasound and shearing treatment in sequence.

[0032] Preferably, the ultrasound time is 30-60 min, for example, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.

[0033] Preferably, the shearing treatment rate is 80000-150000 rpm, for example, 80000 rpm, 9000 rpm, 100000 rpm, 110000 rpm, 120000 rpm, 130000 rpm, 140000 rpm, 150000 rpm, etc.

[0034] Preferably, the secondary heating treatment comprises microwave heating or hydrothermal heating.

[0035] Preferably, the secondary heating treatment includes a first heating treatment and a second heating treatment in sequence.

[0036] Preferably, the temperature of the first heating treatment is 60-85°C, preferably 70-85°C, for example, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, etc.; the time is 10-60min, for example, 10min, 20min, 30min, 40min, 50min, 60min, etc.

[0037] Preferably, the heating rate of the first heating treatment is 1-20°C / min, preferably 5-10°C / min, for example, it can be 1°C / min, 2°C / min, 5°C / min, 8°C / min, 10°C / min, 12°C / min, 15°C / min, 18°C / min, 20°C / min, etc.

[0038] Preferably, the temperature of the second heating treatment is 100-145°C, preferably 130°C, for example, it can be 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, etc.

[0039] Preferably, the heating rate of the second heating treatment is 1-10°C / min, preferably 5-10°C / min, for example, 1°C / min, 2°C / min, 5°C / min, 8°C / min, 10°C / min, etc.

[0040] In the present invention, by adjusting the parameters of the first heating treatment and the second heating treatment, the precursor can achieve nanoscale nucleation and can effectively avoid large-scale agglomeration and growth.

[0041] Preferably, the temperature of the first reaction is 100-145°C, for example, it can be 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, etc.; the time is 10-120min, for example, it can be 10min, 20min, 30min, 50min, 80min, 100min, 110min, 120min, etc.

[0042] Preferably, the second iridium-based precursor includes any one of chloroiridic acid, ammonium chloroiridate, potassium chloroiridate, ammonium chloroiridate or potassium chloroiridate, or a combination of at least two of them.

[0043] Preferably, the mass ratio of iridium atoms in the second iridium-based precursor to iridium atoms in the first iridium-based precursor is (0.01-0.3):1, preferably (0.1-0.2):1, for example, it can be 0.01:1, 0.02:1, 0.05:1, 0.08:1, 0.1:1, 0.12:1, 0.15:1, 0.18:1, 0.2:1, 0.22:1, 0.25:1, 0.28:1, 0.3:1, etc.

[0044] Preferably, the second solvent comprises a reducing alcohol solvent.

[0045] Preferably, the reducing alcohol solvent includes any one of ethanol, propanol, n-propanol, ethylene glycol, isopropanol or glycerol, or a combination of at least two thereof.

[0046] Preferably, the mass ratio of the second iridium-based precursor to the second solvent is 1:(2-10), preferably 1:(5-7), for example, it can be 1:2, 1:3, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, etc.

[0047] Preferably, the second surfactant is further added before the second mixing.

[0048] Preferably, the second surfactant comprises polyvinyl pyrrolidone and / or cetyltrimethylammonium bromide.

[0049] Preferably, the mass ratio of the second surfactant to the second solvent is 1:(5-10), preferably 1:8, for example, it can be 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, etc.

[0050] Preferably, the second mixing comprises ultrasound and shearing treatment in sequence.

[0051] Preferably, the second reaction is carried out under an inert atmosphere.

[0052] In the present invention, the inert atmosphere exemplarily includes inert gases such as nitrogen, argon or helium, and the present invention is not limited thereto.

[0053] Preferably, the temperature of the second reaction is 110-145°C, for example, it can be 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C, 145°C, etc.; the time is 10-120min, for example, it can be 10min, 20min, 30min, 50min, 80min, 100min, 110min, 120min, etc.

[0054] Preferably, the oxidation treatment is performed by sintering in an oxygen atmosphere.

[0055] Preferably, the temperature of the oxidation treatment is 300-600°C, for example, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, etc.

[0056] Preferably, the oxidation treatment is followed by acid washing and water washing to remove unstable impurity components.

[0057] Preferably, the acid solution used for pickling includes any one of nitric acid, hydrochloric acid or sulfuric acid.

[0058] Preferably, the concentration of the acid solution is 0.01-0.1 mol / L, for example, it can be 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.04 mol / L, 0.05 mol / L, 0.06 mol / L, 0.07 mol / L, 0.08 mol / L, 0.09 mol / L, 0.1 mol / L, etc.

[0059] In a second aspect, the present invention provides an alloy oxide catalyst with a hollow core-shell structure, wherein the alloy oxide catalyst with a hollow core-shell structure comprises an alloy oxide core and an iridium-based oxide coating layer coated on the surface of the alloy oxide core, wherein there is a hollow structure between the alloy oxide core and the iridium-based oxide coating layer, and the alloy oxide catalyst with a hollow core-shell structure is prepared by the method for preparing an alloy oxide catalyst with a hollow core-shell structure according to the first aspect.

[0060] Preferably, the particle size of the alloy oxide core is 1.5-5 nm, for example, it can be 1.5 nm, 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm, 5 nm, etc.

[0061] Preferably, the thickness of the iridium-based oxide coating layer is 0.1-1.5 nm, for example, it may be 0.1 nm, 0.2 nm, 0.5 nm, 0.8 nm, 1 nm, 1.2 nm, 1.5 nm, etc.

[0062] Preferably, the mass ratio of iridium atoms in the iridium-based oxide coating layer to iridium atoms in the alloy oxide core is (0.01-0.3):1, preferably (0.1-0.2):1, for example, it can be 0.01:1, 0.02:1, 0.05:1, 0.08:1, 0.1:1, 0.12:1, 0.15:1, 0.18:1, 0.2:1, 0.22:1, 0.25:1, 0.28:1, 0.3:1, etc.

[0063] In a third aspect, the present invention provides an application of the alloy oxide catalyst with a hollow core-shell structure according to the second aspect in a proton exchange membrane water electrolysis hydrogen production technology.

[0064] Compared with the prior art, the present invention has the following beneficial effects:

[0065] The present invention provides a method for preparing an alloy oxide catalyst having a hollow core-shell structure. First, compared with the conventional one-time reduction preparation method, the present invention adopts a secondary reduction method to prepare an alloy oxide catalyst having a hollow core-shell structure, which can not only form a uniform, dense and stable iridium-based oxide (IrO x ) shell structure, which is used to treat the alloy oxide (IrRuO x ) The core structure forms an effective protective effect, and can also effectively inhibit the loss of active components in the core structure, thereby improving the structural stability and durability of the catalyst; secondly, there is an obvious hollow structure between the core and shell of the catalyst in the present invention, which greatly increases the specific surface area of ​​the catalyst, promotes the generation of more catalytic active sites, and thus can improve the reaction activity and catalytic efficiency of the catalyst. In addition, the preparation method provided by the present invention can achieve a high yield without using an alkaline solution to adjust the pH value of the solution, is safe to operate, and does not pollute the environment.

[0066] Finally, the present invention optimizes the preparation method and then regulates the component ratio and particle size in the core-shell structure, and finally forms a nanostructured catalyst with an iridium-ruthenium alloy oxide as the core and an iridium-based oxide as the shell. On the one hand, the iridium-ruthenium alloy oxide core itself has sufficient corrosion resistance, and the layered iridium-based oxide shell has controllable proton exchange and charge balance capabilities, which can inhibit surface reconstruction and the formation of soluble iridium and ruthenium species during the catalytic process, thereby further improving the structural stability of the catalyst; on the other hand, the above catalyst not only reduces the amount of precious metal Ir used, saves costs, but also improves its surface electronic properties, thereby further improving the catalytic activity. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] Figure 1 A schematic diagram of the structure of an alloy oxide catalyst having a hollow core-shell structure provided by the present invention;

[0068] Figure 2 This is a performance comparison chart of the catalysts provided in Example 1 and Comparative Examples 1-2;

[0069] Figure 3 This is a performance comparison diagram of the membrane electrode assembled with the catalysts provided in Example 1 and Comparative Examples 1-2;

[0070] Figure 4 This is a durability performance diagram of the membrane electrode assembled using the catalyst provided in Example 1. DETAILED DESCRIPTION

[0071] The technical solution of the present invention is further described below by combining the accompanying drawings and specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0072] Unless otherwise specified, the materials in the embodiments and comparative examples of the present invention are commercially available.

[0073] Example 1

[0074] This embodiment provides an alloy oxide catalyst having a hollow core-shell structure and a preparation method thereof, which comprises the following steps:

[0075] Preparation of the inner core: chloroiridic acid, ruthenium chloride, a porous carbon carrier material and an ethylene glycol solvent are mixed for the first time, wherein the mass ratio of iridium atoms in chloroiridic acid to ruthenium atoms in ruthenium chloride is 1:3, the mass ratio of the total mass of chloroiridic acid and ruthenium chloride to the porous carbon carrier material is 2:1, and the mass ratio of the total mass of chloroiridic acid and ruthenium chloride to the ethylene glycol solvent is 1:5; then a surfactant polyvinyl pyrrolidone (PVP) is added, the mass ratio of PVP to the ethylene glycol solvent is 1:50, ultrasonic treatment is performed for 30 minutes, and shearing is performed at a speed of 100,000 rpm for 1 hour. After uniform mixing, the mixture is first heated to 80°C at a heating rate of 5°C / min under a nitrogen atmosphere and kept at a constant temperature for 30 minutes, and then heated to 140°C at a heating rate of 5°C / min and reacted for 60 minutes to obtain a first reaction solution;

[0076] Preparation of the shell: The first reaction solution, chloroiridic acid and ethylene glycol solvent are mixed, wherein the mass ratio of chloroiridic acid to ethylene glycol solvent is 1:10, and the mass ratio of iridium atoms of chloroiridic acid in the shell to iridium atoms of chloroiridic acid in the core is 0.03:1; then a surfactant PVP is added, wherein the mass ratio of PVP to ethylene glycol solvent is 1:10, ultrasonic treatment is performed for 30 minutes, shearing is performed at a speed of 100,000 rpm for 1 hour, heating and stirring are performed at 135°C under an argon atmosphere for 20 minutes, washing and drying are performed, and further oxidation treatment is performed at 400°C under an oxygen atmosphere, and then a hydrochloric acid solution with a concentration of 0.1 mol / L is added for pickling for 2 hours, and then washed and dried with water to obtain the alloy oxide catalyst having a hollow core-shell structure.

[0077] from Figure 1 It can be seen that the alloy oxide catalyst with a hollow core-shell structure provided in this embodiment has an obvious hollow structure between the core structure and the shell structure, and thus has a higher specific surface area, and its specific surface area is 120-150m 2 / g, so the exposed catalytic active sites can be greatly increased, thereby further improving the reaction activity of the catalyst.

[0078] Example 2

[0079] This embodiment provides an alloy oxide catalyst having a hollow core-shell structure and a preparation method thereof, which comprises the following steps:

[0080] Preparation of the inner core: chloroiridic acid, ruthenium chloride, a porous carbon carrier material and an ethylene glycol solvent are mixed for the first time, wherein the mass ratio of iridium atoms in chloroiridic acid to ruthenium atoms in ruthenium chloride is 1:2, the mass ratio of the total mass of chloroiridic acid and ruthenium chloride to the porous carbon carrier material is 5:1, and the mass ratio of the total mass of chloroiridic acid and ruthenium chloride to the ethylene glycol solvent is 1:12; then a surfactant polyvinyl pyrrolidone (PVP) is added, the mass ratio of PVP to the ethylene glycol solvent is 1:30, ultrasonic treatment is performed for 40 minutes, and shearing is performed at a speed of 100,000 rpm for 1 hour. After uniform mixing, the mixture is first heated to 80°C at a heating rate of 8°C / min under a nitrogen atmosphere and kept at a constant temperature for 30 minutes by microwave heating, and then heated to 140°C at a heating rate of 8°C / min and reacted for 60 minutes to obtain a first reaction solution;

[0081] Preparation of the shell: The first reaction solution, chloroiridic acid and ethylene glycol solvent are mixed, wherein the mass ratio of chloroiridic acid to ethylene glycol solvent is 1:6, and the mass ratio of iridium atoms of chloroiridic acid in the shell to iridium atoms of chloroiridic acid in the core is 0.15:1; then a surfactant PVP is added, wherein the mass ratio of PVP to ethylene glycol solvent is 1:8, ultrasonic treatment is performed for 60 minutes, shearing is performed at 120,000 rpm for 1 hour, heating and stirring are performed at 135°C under an argon atmosphere for 20 minutes, washing and drying are performed, and further oxidation treatment is performed at 400°C under an oxygen atmosphere, and then a hydrochloric acid solution with a concentration of 0.1 mol / L is added for pickling for 2 hours, and then washed and dried with water to obtain the alloy oxide catalyst having a hollow core-shell structure.

[0082] Example 3

[0083] This embodiment provides an alloy oxide catalyst having a hollow core-shell structure and a preparation method thereof, which comprises the following steps:

[0084] Preparation of the inner core: chloroiridic acid, ruthenium chloride, a porous carbon carrier material and an ethylene glycol solvent are mixed for the first time, wherein the mass ratio of iridium atoms in chloroiridic acid to ruthenium atoms in ruthenium chloride is 1:2.5, the mass ratio of the total mass of chloroiridic acid and ruthenium chloride to the porous carbon carrier material is 6:1, and the mass ratio of the total mass of chloroiridic acid and ruthenium chloride to the ethylene glycol solvent is 1:15; then a surfactant polyvinyl pyrrolidone (PVP) is added, the mass ratio of PVP to the ethylene glycol solvent is 1:25, ultrasonic treatment is performed for 50 minutes, and shearing is performed at a speed of 100,000 rpm for 1 hour. After uniform mixing, the mixture is first heated to 80°C at a heating rate of 10°C / min under a nitrogen atmosphere and kept at a constant temperature for 30 minutes, and then heated to 140°C at a heating rate of 10°C / min and reacted for 60 minutes to obtain a first reaction solution;

[0085] Preparation of the shell: The first reaction solution, chloroiridic acid and ethylene glycol solvent are mixed, wherein the mass ratio of chloroiridic acid to ethylene glycol solvent is 1:7, and the mass ratio of iridium atoms of chloroiridic acid in the shell to iridium atoms of chloroiridic acid in the core is 0.1:1; then a surfactant PVP is added, the mass ratio of PVP to ethylene glycol solvent is 1:9, ultrasonic treatment is performed for 30 minutes, shearing is performed at 100,000 rpm for 1 hour, heating and stirring are performed at 135°C in an argon atmosphere for 20 minutes, washing and drying are performed, and further oxidation treatment is performed at 600°C in an oxygen atmosphere, and then a hydrochloric acid solution with a concentration of 0.1 mol / L is added for pickling for 2 hours, and then washed and dried to obtain the alloy oxide catalyst having a hollow core-shell structure.

[0086] Example 4

[0087] This embodiment provides an alloy oxide catalyst having a hollow core-shell structure and a preparation method thereof, which comprises the following steps:

[0088] Preparation of the inner core: chloroiridic acid, ruthenium chloride, a porous carbon carrier material and an ethylene glycol solvent are mixed for the first time, wherein the mass ratio of iridium atoms in chloroiridic acid to ruthenium atoms in ruthenium chloride is 1:3, the mass ratio of the total mass of chloroiridic acid and ruthenium chloride to the porous carbon carrier material is 10:1, and the mass ratio of the total mass of chloroiridic acid and ruthenium chloride to the ethylene glycol solvent is 1:20; then a surfactant polyvinyl pyrrolidone (PVP) is added, the mass ratio of PVP to the ethylene glycol solvent is 1:50, ultrasonic treatment is performed for 60 minutes, and shearing is performed at a speed of 150,000 rpm for 1 hour. After uniform mixing, the mixture is first heated to 85°C at a heating rate of 10°C / min under a nitrogen atmosphere and kept at a constant temperature for 60 minutes, and then heated to 100°C at a heating rate of 10°C / min and reacted for 60 minutes to obtain a first reaction solution;

[0089] Preparation of the shell: The first reaction solution, chloroiridic acid and ethylene glycol solvent are mixed, wherein the mass ratio of chloroiridic acid to ethylene glycol solvent is 1:10, and the mass ratio of iridium atoms of chloroiridic acid in the shell to iridium atoms of chloroiridic acid in the core is 0.3:1; then a surfactant PVP is added, wherein the mass ratio of PVP to ethylene glycol solvent is 1:10, ultrasonic treatment is performed for 10 minutes, shearing is performed at 80,000 rpm for 1 hour, heating and stirring are performed at 115°C in an argon atmosphere for 60 minutes, washing and drying are performed, and further oxidation treatment is performed at 300°C in an oxygen atmosphere, and then a hydrochloric acid solution with a concentration of 0.01 mol / L is added for pickling for 2 hours, and then washed and dried to obtain the alloy oxide catalyst having a hollow core-shell structure.

[0090] Example 5

[0091] The difference between this embodiment and embodiment 1 is that, during the preparation of the inner core, the mass ratio of iridium atoms in chloroiridic acid to ruthenium atoms in ruthenium chloride is 1:0.1, and the rest is the same as embodiment 1.

[0092] Example 6

[0093] The difference between this embodiment and embodiment 1 is that, during the preparation of the inner core, the mass ratio of iridium atoms in chloroiridic acid to ruthenium atoms in ruthenium chloride is 1:6, and the rest is the same as embodiment 1.

[0094] Example 7

[0095] The difference between this embodiment and embodiment 1 is that, during the preparation of the inner core, the mass ratio of the total mass of chloroiridic acid and ruthenium chloride to the mass of the porous carbon carrier material is 0.5:1, and the rest is the same as embodiment 1.

[0096] Example 8

[0097] The difference between this embodiment and embodiment 1 is that, during the preparation of the inner core, the mass ratio of the total mass of chloroiridic acid and ruthenium chloride to the mass of the porous carbon carrier material is 15:1, and the rest is the same as embodiment 1.

[0098] Example 9

[0099] The difference between this embodiment and embodiment 1 is that, during the preparation of the inner core, the mass ratio of PVP to ethylene glycol solvent is 7:50, and the rest is the same as embodiment 1.

[0100] Example 10

[0101] The difference between this embodiment and embodiment 1 is that, during the preparation process of the inner core, a single heating treatment is adopted, that is, microwave heating is performed at a heating rate of 5°C / min to 140°C under a nitrogen atmosphere for 60 minutes, and the rest is the same as embodiment 1.

[0102] Embodiment 11

[0103] The difference between this embodiment and embodiment 1 is that, during the preparation of the shell, the mass ratio of chloroiridic acid to ethylene glycol solvent is 1:0.5, and the rest is the same as embodiment 1.

[0104] Example 12

[0105] The difference between this embodiment and embodiment 1 is that, during the preparation of the shell, the mass ratio of chloroiridic acid to ethylene glycol solvent is 1:15, and the rest is the same as embodiment 1.

[0106] Example 13

[0107] The difference between this embodiment and embodiment 1 is that, during the preparation of the shell, the mass ratio of PVP to ethylene glycol solvent is 1:1, and the rest is the same as embodiment 1.

[0108] Comparative Example 1

[0109] This comparative example provides a commercial iridium oxide catalyst.

[0110] Comparative Example 2

[0111] This comparative example provides a commercial iridium oxide catalyst with a core-shell structure, wherein the component of the core is titanium dioxide, and the component of the shell is iridium oxide.

[0112] Comparative Example 3

[0113] The difference between this comparative example and Example 1 is that the shell is not prepared, and the other aspects are the same as Example 1.

[0114] Test conditions

[0115] The catalysts provided in Examples 1 to 13 and Comparative Examples 1 to 3 were subjected to performance tests, and the test methods were as follows:

[0116] (1) Catalyst overpotential test: Linear sweep voltammetry (LSV) test, scanning range 0 ~ 1.75V vs RHE (0.544 ~ 0.944V vs Hg2SO4), scanning rate 10mV / s, rotating disk electrode speed 1600rpm, comparison 10mA / cm 2 The potential at

[0117] (2) Characterization of membrane electrode performance: First, 10 mg of catalyst was dispersed in 10 mL of deionized water and ultrasonically dispersed for 30 min; then 200 μL of naphthol (mass fraction 0.05%) and 15 mL of isopropanol were added and ultrasonically dispersed for 30 min, and then they were uniformly sprayed on the N117 membrane using an ultrasonic sprayer; the prepared membrane electrode was assembled into a PEM water electrolyzer for performance evaluation. The gas diffusion layer was titanium felt, the test temperature was 80 ° C, and the active area was 5 cm 2 The Ir metal loading is 0.5 mg / cm 2 ;

[0118] (3) Durability characterization: The obtained membrane electrode was subjected to a durability test with a test time of 1000 h and a current density of 1 A / cm 2 .

[0119] The test results are shown in Table 1:

[0120] Table 1

[0121] <![CDATA[10mA / cm 2 Potential (mV)]]> 1000h durability attenuation (%) Example 1 1.468 0.6 Example 2 1.475 1 Example 3 1.477 1.2 Example 4 1.481 1.5 Example 5 1.478 1.3 Example 6 1.485 1.1 Example 7 1.479 2 Example 8 1.488 1.4 Example 9 1.477 1.6 Example 10 1.478 1.3 Embodiment 11 1.481 1.5 Example 12 1.483 1.1 Embodiment 13 1.488 1.4 Comparative Example 1 1.485 1.2 Comparative Example 2 1.5 1.3 Comparative Example 3 1.475 1.8

[0122] It can be seen from Table 1 that in the preparation process of the alloy oxide catalyst with a hollow core-shell structure, factors such as the metal atom content, the content of the porous carbon support material, the heating method, the PVP content, and the mass ratio of the iridium atoms in the iridium-based oxide coating layer to the iridium atoms in the alloy oxide core have a significant effect on the overall performance and durability of the catalyst. The technical solution of the present invention requires strict control of the preparation method and parameters of the above-mentioned alloy oxide catalyst with a hollow core-shell structure, so as to achieve the purpose of the alloy oxide catalyst with a hollow core-shell structure having both optimal reaction activity and durability.

[0123] By comparing Example 1 with Examples 5-6, it can be seen that the present invention enables the alloy oxide catalyst to have the best catalytic activity and durability by regulating the mass ratio of iridium atoms in chloroiridic acid and ruthenium atoms in ruthenium chloride.

[0124] By comparing Example 1 with Examples 7-8, it can be seen that the present invention enables the alloy oxide catalyst to have higher catalytic activity by regulating the mass ratio of the total mass of chloroiridic acid and ruthenium chloride to the porous carbon support material.

[0125] By comparing Example 1, Example 9 and Example 13, it can be seen that the present invention enables the precursor to be well dispersed and have uniform particle size by regulating the content of surfactant in the process of preparing the core and the shell.

[0126] Comparing Example 1 and Example 10, it can be seen that the comprehensive performance of the core material obtained by a single heating treatment is relatively poor.

[0127] By comparing Example 1 with Examples 11-12, it can be seen that the present invention enables the catalyst to have a higher catalytic efficiency by regulating the mass ratio of iridium atoms in the second iridium-based precursor to iridium atoms in the first iridium-based precursor.

[0128] By comparing Example 1 and Comparative Examples 1-2, it can be seen that the commercial iridium oxide catalyst disclosed in the prior art cannot achieve all the technical effects of the present invention; since Comparative Example 3 is not coated, the durability of the catalyst prepared is poor.

[0129] The half-cell performance obtained by assembling the alloy oxide catalyst with a hollow core-shell structure provided in Example 1 is as follows: Figure 2 Shown: At 10mA / cm 2 At the same current density, its overpotential is 20-40mV lower; the results of assembling it into a membrane electrode and testing the performance of a single cell are as follows Figure 3 and Figure 4 As shown, the catalyst loading on Ir metal is 0.5 mg / cm 2 The performance is significantly better than that of the commercial catalyst membrane electrode disclosed in the prior art in Comparative Examples 1-2, and after 1A / cm 2 After 1000h of durability test at constant current density, there is no obvious performance degradation.

[0130] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing an alloy oxide catalyst having a hollow core-shell structure, characterized in that: The method comprises the following steps: The first iridium-based precursor, the ruthenium-based precursor, the carrier material and the first solvent are mixed for the first time, and subjected to a secondary heating treatment and a first reaction to obtain a first reaction solution; The first reaction solution, the second iridium-based precursor and the second solvent are mixed for a second time, and subjected to a second reaction and oxidation treatment to obtain the alloy oxide catalyst having a hollow core-shell structure.

2. The method according to claim 1, characterized in that The first iridium-based precursor includes any one of chloroiridic acid, ammonium chloroiridate, potassium chloroiridate, ammonium chloroiridate or potassium chloroiridate, or a combination of at least two thereof; Preferably, the ruthenium-based precursor comprises ruthenium chloride and its hydrate; Preferably, the mass ratio of iridium atoms in the first iridium-based precursor to ruthenium atoms in the ruthenium-based precursor is 1:(0.3-3), preferably 1:2; Preferably, the support material comprises an undoped or doped carbon support material; Preferably, the doped element includes at least one of nitrogen, boron, sulfur or phosphorus; Preferably, the carbon support material comprises any one or a combination of at least two of carbon black, graphitized carbon, porous carbon, carbon nanotubes, carbon nanofibers, graphene or carbon aerogel; Preferably, the mass ratio of the total mass of the first iridium-based precursor and the ruthenium-based precursor to the support material is (1-10):1, preferably 5:1; Preferably, the first solvent comprises a reducing alcohol solvent; Preferably, the reducing alcohol solvent includes any one of ethanol, propanol, n-propanol, ethylene glycol, isopropanol or glycerol, or a combination of at least two thereof; Preferably, the mass ratio of the total mass of the first iridium-based precursor and the ruthenium-based precursor to the first solvent is 1:(5-20).

3. The method according to claim 1 or 2, characterized in that: The first mixing also includes adding a first surfactant; Preferably, the first surfactant comprises polyvinyl pyrrolidone and / or hexadecyltrimethylammonium bromide; Preferably, the mass ratio of the first surfactant to the first solvent is 1:(10-50), preferably 1:

30.

4. The method according to any one of claims 1 to 3, characterized in that The first mixing includes ultrasound and shearing treatment in sequence; Preferably, the ultrasound time is 30-60 min; Preferably, the shearing treatment rate is 80000-150000 rpm; Preferably, the secondary heating treatment comprises microwave heating or hydrothermal heating; Preferably, the secondary heating treatment includes a first heating treatment and a second heating treatment in sequence; Preferably, the temperature of the first heating treatment is 60-85°C, preferably 70-85°C, and the time is 10-60 minutes; Preferably, the heating rate of the first heating treatment is 1-20°C / min, preferably 5-10°C / min; Preferably, the temperature of the second heating treatment is 100-145°C, preferably 130°C; Preferably, the heating rate of the second heating treatment is 1-10°C / min, preferably 5-10°C / min; Preferably, the temperature of the first reaction is 100-145° C. and the time is 10-120 min.

5. The method according to any one of claims 1 to 4, characterized in that The second iridium-based precursor includes any one of chloroiridic acid, ammonium chloroiridate, potassium chloroiridate, ammonium chloroiridate or potassium chloroiridate, or a combination of at least two thereof; Preferably, the mass ratio of iridium atoms in the second iridium-based precursor to iridium atoms in the first iridium-based precursor is (0.01-0.3):1, preferably (0.1-0.2):1; Preferably, the second solvent comprises a reducing alcohol solvent; Preferably, the reducing alcohol solvent includes any one of ethanol, propanol, n-propanol, ethylene glycol, isopropanol or glycerol, or a combination of at least two thereof; Preferably, the mass ratio of the second iridium-based precursor to the second solvent is 1:(2-10), preferably 1:(5-7); Preferably, the second mixing further comprises adding a second surfactant; Preferably, the second surfactant comprises polyvinyl pyrrolidone and / or hexadecyltrimethylammonium bromide; Preferably, the mass ratio of the second surfactant to the second solvent is 1:(5-10), preferably 1:

8.

6. The method according to any one of claims 1 to 5, characterized in that The second mixing includes ultrasound and shearing treatment in sequence; Preferably, the second reaction is carried out under an inert atmosphere; Preferably, the temperature of the second reaction is 110-145°C and the time is 10-120min; Preferably, the oxidation treatment is sintering in an oxygen atmosphere; Preferably, the temperature of the oxidation treatment is 300-600°C.

7. The method according to any one of claims 1 to 6, characterized in that The oxidation treatment also includes pickling and water washing in sequence; Preferably, the acid solution used for pickling includes any one of nitric acid, hydrochloric acid or sulfuric acid; Preferably, the concentration of the acid solution is 0.01-0.1 mol / L.

8. An alloy oxide catalyst having a hollow core-shell structure, characterized in that: The alloy oxide catalyst with a hollow core-shell structure comprises an alloy oxide core and an iridium-based oxide coating layer coated on the surface of the alloy oxide core, wherein a hollow structure is provided between the alloy oxide core and the iridium-based oxide coating layer, and the alloy oxide catalyst with a hollow core-shell structure is prepared by the method for preparing an alloy oxide catalyst with a hollow core-shell structure according to any one of claims 1 to 7.

9. The alloy oxide catalyst having a hollow core-shell structure according to claim 8, characterized in that: The particle size of the alloy oxide core is 1.5-5 nm; Preferably, the thickness of the iridium-based oxide coating layer is 0.1-1.5 nm; Preferably, the mass ratio of iridium atoms in the iridium-based oxide coating layer to iridium atoms in the alloy oxide core is (0.01-0.3):1, preferably (0.1-0.2):

1.

10. Use of the alloy oxide catalyst with a hollow core-shell structure according to claim 8 or 9 in proton exchange membrane water electrolysis hydrogen production technology.