Method for recovering metallic silver in crystalline silicon assembly
Through the methods of pyrolysis treatment and electrolytic purification, the problems of low recovery rate of metal silver and complex process in photovoltaic modules are solved, and the recycling of high-purity silver is realized and the process flow is simplified, with low energy consumption and environmental protection.
Patent Information
- Application Number
- CN202410934937.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-19
AI Technical Summary
When the prior art recovers metal silver in photovoltaic modules, the recovery rate is low and the process is complicated, and it is especially unable to effectively remove the interference of aluminum, affecting the high purity refining of silver.
The battery cells were separated by pyrolysis treatment, soaked the alkali solution to remove aluminum, then dissolved in the nitric acid solution and added metal copper powder and ferric chloride solution, and finally electrolytic purification was performed to obtain high-purity metal silver.
It improves the recovery rate and purity of metal silver, simplifies the process flow, has low equipment requirements, low energy consumption, and is environmentally friendly.
Smart Images

Figure CN118979284A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal recovery, and in particular to a method for recovering metallic silver in a crystalline silicon component. Background Art
[0002] Photovoltaic modules are made of cells, solder strips for connecting cells, EVA films, glass and back panels, and are hot pressed. Their service life is about 25-30 years. In the next few years, photovoltaic modules installed around 2000 will be retired. If not properly handled, they will cause serious environmental damage. At the same time, the components that make up photovoltaic modules all have recycling value. Among them, silver has the highest recycling value.
[0003] The traditional method of recovering silver is to use nitric acid to dissolve silver, and then use chloride ions to precipitate to obtain silver chloride, but this method has a low recovery rate of silver (about 90%), and silver chloride needs to be further dissolved and refined to obtain high-purity silver. At the same time, the back electrode of the battery cell is sintered by aluminum and glass, and silver cannot be directly leached out with nitric acid.
[0004] In view of this, we propose a silver recovery method which eliminates the interference of aluminum, can improve the silver recovery rate, and shorten the process flow. Summary of the invention
[0005] The object of the present invention is to provide a method for recovering metallic silver in a crystalline silicon component to solve the problems raised in the above background technology.
[0006] To achieve the above object, the present invention provides the following technical solutions:
[0007] A method for recovering metallic silver in a crystalline silicon component comprises the following steps:
[0008] S1. After removing the frame and junction box from the crystalline silicon module, pyrolysis treatment is performed to obtain a cell, and then the cell is immersed in a sufficient amount of alkaline solution to remove aluminum after sufficient reaction, and the silver-containing cell is obtained after filtering;
[0009] S2, dissolving the obtained silver-containing battery sheet in a nitric acid solution, filtering, and obtaining a silver-containing solution;
[0010] S3, adding a sufficient amount of metallic copper powder to the obtained silver-containing solution, filtering, and obtaining silver and copper solids;
[0011] S4, adding a sufficient amount of ferric chloride solution to the obtained silver and copper solids, filtering, and obtaining crude silver;
[0012] S5. The obtained crude silver is electrolytically purified to obtain high-purity metallic silver.
[0013] Preferably, in step S1, the pyrolysis treatment temperature is 180-220° C., and the pyrolysis treatment time is 5-10 min.
[0014] Preferably, in step S1, the alkali solution is a NaOH or KOH solution, the concentration of the alkali solution is 0.5-4 mol / L, the soaking time is 10-60 min, and after the soaking is completed, it is fully stirred and filtered to obtain a silver-containing solid.
[0015] Preferably, in step S2, the concentration of the nitric acid solution is 0.5-5 mol / L, and the mass ratio of the added amount of the nitric acid solution to the silver-containing solid is 2-20 mL: 1 g.
[0016] Preferably, in step S3, the particle size of the metal copper powder is less than 10 μm, and the ratio of the amount of the metal copper powder added to the volume of the silver-containing solution is 0.05-0.5 g:1 mL.
[0017] Preferably, in step S4, the concentration of the ferric chloride solution is 0.2-2 mol / L, and the mass ratio of the added amount of the ferric chloride solution to the silver and copper solids is 10-100 mL: 1 g.
[0018] Preferably, in step S5, the anode for electrolytic purification is crude silver, the cathode is high-purity metallic silver, and the electrolyte is a silver nitrate solution.
[0019] Preferably, the content of silver ions in the electrolyte is 50-150 g / L.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] 1. The method for recovering metallic silver in a crystalline silicon component comprises the following steps: heating the crystalline silicon component, separating the back plate from the battery cell, and then immersing the battery cell in a sufficient amount of alkali solution, filtering after sufficient reaction to obtain a silver-containing solid; dissolving the obtained silver-containing solid in a nitric acid solution, filtering to obtain a silver-containing solution; adding a sufficient amount of metallic copper to the obtained silver-containing solution, filtering to obtain silver and copper solids, adding a sufficient amount of ferric chloride solution to the obtained silver and copper solids, filtering to obtain crude silver; electrolyzing and purifying the obtained crude silver to obtain high-purity metallic silver; the present application recovers and purifies metallic silver in a crystalline silicon component by room temperature reaction and electrolysis, has low equipment requirements, low energy consumption, and is green and environmentally friendly.
[0022] 2. The method for recovering metallic silver in the crystalline silicon component is simple to operate, eliminates the interference of aluminum, and purifies the crude silver by electrolysis, and the purity of the metallic silver finally obtained reaches more than 99%. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The present invention is a flow chart of the method for recovering metallic silver in a crystalline silicon component. DETAILED DESCRIPTION
[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] like Figure 1 As shown, the present application provides a method for recovering metallic silver in a crystalline silicon component, comprising the following steps S1-S5, which are specifically as follows:
[0026] S1. After removing the frame and junction box of the crystalline silicon component, the battery cell is obtained by pyrolysis treatment, and then the battery cell is immersed in a sufficient amount of alkaline solution. After sufficient reaction, the aluminum is removed and the silver-containing battery cell is obtained after filtering.
[0027] In some embodiments, the pyrolysis treatment temperature is 180-220°C, for example, 180°C, 200°C, 210°C, 220°C, and the pyrolysis treatment time is 5-10 min, for example, 5 min, 6 min, 8 min, 10 min.
[0028] In some embodiments, the alkali solution is a NaOH or KOH solution, and the concentration of the alkali solution is 0.5-4 mol / L, for example, 0.5 mol / L, 1 mol / L, 2 mol / L, 4 mol / L. The immersion time of the crystalline silicon component in the alkali solution is 10-60 min, for example, 10 min, 20 min, 40 min, 60 min. After the immersion, it is fully stirred and filtered to obtain a silver-containing solid.
[0029] In this step S1, the crystalline silicon component is heated to separate the back plate and the battery cell, and the aluminum in the battery cell is removed by using a sufficient amount of alkaline solution NaOH or KOH, and a solid mainly containing silver is obtained after filtering.
[0030] S2. Dissolve the obtained silver-containing battery cell in a nitric acid solution, filter, and obtain a silver-containing solution.
[0031] In some embodiments, the concentration of the nitric acid solution is 0.5-5 mol / L, for example, 0.5 mol / L, 1 mol / L, 3 mol / L, 5 mol / L, and the ratio of the amount of nitric acid solution added to the mass of the silver-containing solid is 2-20 mL: 1 g, for example, 2 mL: 1 g, 5 mL: 1 g, 10 mL: 1 g, 20 mL: 1 g.
[0032] In this step S2, the silver-containing battery cell obtained in step S1 is dissolved by a nitric acid solution, and insoluble impurities are removed by filtration to obtain a silver nitrate solution.
[0033] S3. Add sufficient amount of metallic copper powder to the obtained silver-containing solution, filter, and obtain silver and copper solids.
[0034] In some embodiments, the particle size of the metallic copper powder is less than 10 μm, and the ratio of the amount of metallic copper powder added to the volume of the silver-containing solution is 0.05-0.5 g:1 mL, for example, 0.05 g:1 mL, 0.1 g:1 mL, 0.2 g:1 mL, 0.5 g:1 mL.
[0035] In this step S3, a sufficient amount of metallic copper powder is added to cause a replacement reaction with the silver nitrate solution to completely replace the metallic silver element, and the silver and copper solids are obtained by filtering.
[0036] S4. Add sufficient amount of ferric chloride solution to the obtained silver and copper solids, filter and obtain crude silver.
[0037] In some embodiments, the concentration of the ferric chloride solution is 0.2-2 mol / L, for example, 0.2 mol / L, 0.5 mol / L, 1 mol / L, 2 mol / L, and the mass ratio of the added amount of the ferric chloride solution to the silver and copper solids is 10-100 mL: 1 g, for example, 10 mL: 1 g, 20 mL: 1 g, 50 mL: 1 g, 100 mL: 1 g.
[0038] In this step S3, the metallic copper in the silver and copper solids undergoes an oxidation-reduction reaction with the ferric chloride solution to generate cupric chloride and ferrous chloride solutions, while the silver does not undergo a chemical reaction with the ferric chloride solution and remains in a solid form. The crude silver is filtered to obtain.
[0039] S5. The obtained crude silver is electrolytically purified to obtain high-purity metallic silver.
[0040] In some embodiments, the anode of electrolytic purification is crude silver, the cathode is high-purity metallic silver, the electrolyte is silver nitrate solution, and the silver ion content in the electrolyte is 50-150g / L, for example, 50g / L, 80g / L, 100g / L, 150g / L.
[0041] In this step S5, crude silver is continuously dissolved at the anode, and high-purity metallic silver is precipitated at the cathode.
[0042] The present application is further described in detail below in conjunction with specific embodiments. The following embodiments are only used to illustrate the present application and are not used to limit the scope of the present application.
[0043] Example 1
[0044] A method for recovering metallic silver in a crystalline silicon component comprises the following steps:
[0045] S1. After removing the frame and junction box from the crystalline silicon component, pyrolysis treatment is performed to obtain the battery cell. The pyrolysis treatment temperature is 180°C and the pyrolysis treatment time is 10 min. The back plate and the battery cell are separated. Then, the battery cell is immersed in a sufficient amount of alkaline solution for 10 min. The alkaline solution is a NaOH solution with an alkaline concentration of 0.5 mol / L. After sufficient reaction, aluminum is removed and the silver-containing battery cell is obtained after filtration.
[0046] S2, dissolving the obtained silver-containing battery cell in a nitric acid solution, wherein the concentration of the nitric acid solution is 0.5 mol / L, and the mass ratio of the added nitric acid solution to the silver-containing solid is 20 mL: 1 g, and filtering to obtain a silver-containing solution;
[0047] S3, adding a sufficient amount of metallic copper powder to the obtained silver-containing solution, wherein the particle size of the metallic copper powder is less than 10 μm, and the volume ratio of the added amount of the metallic copper powder to the silver-containing solution is 0.05 g: 1 mL, filtering to obtain silver and copper solids;
[0048] S4. Add a sufficient amount of ferric chloride solution to the obtained silver and copper solids, wherein the concentration of the ferric chloride solution is 0.2 mol / L, and the mass ratio of the added amount of the ferric chloride solution to the silver and copper solids is 100 mL: 1 g, and filter to obtain crude silver;
[0049] S5. The obtained crude silver is subjected to electrolytic purification, wherein the anode of the electrolytic purification is crude silver, the cathode is high-purity metallic silver, the electrolyte is silver nitrate solution, the content of silver ions in the electrolyte is 50 g / L, and metallic silver with a purity of 99.2% is obtained.
[0050] Example 2
[0051] A method for recovering metallic silver in a crystalline silicon component comprises the following steps:
[0052] S1. After removing the frame and junction box from the crystalline silicon component, pyrolysis treatment is performed to obtain the battery cell. The pyrolysis treatment temperature is 200°C and the pyrolysis treatment time is 8 minutes. The back plate and the battery cell are separated. Then, the battery cell is immersed in a sufficient amount of alkaline solution for 20 minutes. The alkaline solution is a NaOH solution with an alkaline solution concentration of 2 mol / L. After sufficient reaction, aluminum is removed and the silver-containing battery cell is obtained after filtration.
[0053] S2, dissolving the obtained silver-containing battery cell in a nitric acid solution, wherein the concentration of the nitric acid solution is 1 mol / L, and the mass ratio of the added nitric acid solution to the silver-containing solid is 10 mL: 1 g, and filtering to obtain a silver-containing solution;
[0054] S3, adding a sufficient amount of metallic copper powder to the obtained silver-containing solution, wherein the particle size of the metallic copper powder is less than 10 μm, and the volume ratio of the added amount of the metallic copper powder to the silver-containing solution is 0.1 g: 1 mL, filtering to obtain silver and copper solids;
[0055] S4. Add a sufficient amount of ferric chloride solution to the obtained silver and copper solids, wherein the concentration of the ferric chloride solution is 0.5 mol / L, and the mass ratio of the added amount of the ferric chloride solution to the silver and copper solids is 50 mL: 1 g, and filter to obtain crude silver;
[0056] S5. The obtained crude silver is subjected to electrolytic purification, wherein the anode of the electrolytic purification is crude silver, the cathode is high-purity metallic silver, the electrolyte is silver nitrate solution, the content of silver ions in the electrolyte is 80 g / L, and metallic silver with a purity of 99.4% is obtained.
[0057] Example 3
[0058] A method for recovering metallic silver in a crystalline silicon component comprises the following steps:
[0059] S1. After removing the frame and junction box from the crystalline silicon component, pyrolysis treatment is performed to obtain the battery cell. The pyrolysis treatment temperature is 210° C. and the pyrolysis treatment time is 6 min. The back plate and the battery cell are separated. Then, the battery cell is immersed in a sufficient amount of alkaline solution for 40 min. The alkaline solution is a NaOH solution with an alkaline solution concentration of 4 mol / L. After sufficient reaction, aluminum is removed and the silver-containing battery cell is obtained after filtration.
[0060] S2, dissolving the obtained silver-containing battery cell in a nitric acid solution, wherein the concentration of the nitric acid solution is 3 mol / L, and the mass ratio of the added nitric acid solution to the silver-containing solid is 5 mL:1 g, and filtering to obtain a silver-containing solution;
[0061] S3, adding a sufficient amount of metallic copper powder to the obtained silver-containing solution, wherein the particle size of the metallic copper powder is less than 10 μm, and the volume ratio of the added amount of the metallic copper powder to the silver-containing solution is 0.2 g: 1 mL, filtering to obtain silver and copper solids;
[0062] S4. Add a sufficient amount of ferric chloride solution to the obtained silver and copper solids, wherein the concentration of the ferric chloride solution is 1 mol / L, and the mass ratio of the added amount of the ferric chloride solution to the silver and copper solids is 20 mL: 1 g, and filter to obtain crude silver;
[0063] S5. The obtained crude silver is subjected to electrolytic purification, wherein the anode of the electrolytic purification is crude silver, the cathode is high-purity metallic silver, the electrolyte is silver nitrate solution, the content of silver ions in the electrolyte is 100 g / L, and metallic silver with a purity of 99.6% is obtained.
[0064] Example 4
[0065] A method for recovering metallic silver in a crystalline silicon component comprises the following steps:
[0066] S1. After removing the frame and junction box from the crystalline silicon component, pyrolysis treatment is performed to obtain the battery cell. The pyrolysis treatment temperature is 220° C. and the pyrolysis treatment time is 5 min. The back plate and the battery cell are separated. Then, the battery cell is immersed in a sufficient amount of alkaline solution for 60 min. The alkaline solution is a KOH solution with an alkaline solution concentration of 2 mol / L. After sufficient reaction, aluminum is removed and the silver-containing battery cell is obtained after filtration.
[0067] S2, dissolving the obtained silver-containing battery cell in a nitric acid solution, wherein the concentration of the nitric acid solution is 5 mol / L, and the mass ratio of the added nitric acid solution to the silver-containing solid is 2 mL: 1 g, and filtering to obtain a silver-containing solution;
[0068] S3, adding a sufficient amount of metallic copper powder to the obtained silver-containing solution, wherein the particle size of the metallic copper powder is less than 10 μm, and the volume ratio of the added amount of the metallic copper powder to the silver-containing solution is 0.5 g: 1 mL, filtering to obtain silver and copper solids;
[0069] S4. Add a sufficient amount of ferric chloride solution to the obtained silver and copper solids, wherein the concentration of the ferric chloride solution is 2 mol / L, and the mass ratio of the added amount of the ferric chloride solution to the silver and copper solids is 10 mL: 1 g, and filter to obtain crude silver;
[0070] S5. The obtained crude silver is subjected to electrolytic purification, wherein the anode of the electrolytic purification is crude silver, the cathode is high-purity metallic silver, the electrolyte is silver nitrate solution, the content of silver ions in the electrolyte is 150 g / L, and metallic silver with a purity of 99.4% is obtained.
[0071] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for recovering metallic silver from crystalline silicon components, It is characterized in that The following steps are involved: S1. After removing the frame and junction box from the crystalline silicon module, pyrolysis treatment is performed to obtain a cell, and then the cell is immersed in a sufficient amount of alkaline solution to remove aluminum after sufficient reaction, and the silver-containing cell is obtained after filtering; S2, dissolving the obtained silver-containing battery sheet in a nitric acid solution, filtering, and obtaining a silver-containing solution; S3, adding a sufficient amount of metallic copper powder to the obtained silver-containing solution, filtering, and obtaining silver and copper solids; S4, adding a sufficient amount of ferric chloride solution to the obtained silver and copper solids, filtering, and obtaining crude silver; S5. The obtained crude silver is electrolytically purified to obtain high-purity metallic silver.
2. The method for recovering metallic silver in a crystalline silicon component according to claim 1, It is characterized in that In the step S1, the pyrolysis treatment temperature is 180-220° C., and the pyrolysis treatment time is 5-10 min.
3. The method for recovering metallic silver in crystalline silicon components according to claim 1, It is characterized in that In the step S1, the alkali solution is a NaOH or KOH solution, the concentration of the alkali solution is 0.5-4 mol / L, the soaking time is 10-60 min, and after the soaking is completed, the solution is fully stirred and filtered to obtain a silver-containing solid.
4. The method for recovering metallic silver in a crystalline silicon component according to claim 1, It is characterized in that In step S2, the concentration of the nitric acid solution is 0.5-5 mol / L, and the mass ratio of the added amount of the nitric acid solution to the silver-containing solid is 2-20 mL: 1 g.
5. The method for recovering metallic silver in crystalline silicon components according to claim 1, It is characterized in that In the step S3, the particle size of the metal copper powder is less than 10 μm, and the ratio of the amount of the metal copper powder added to the volume of the silver-containing solution is 0.05-0.5 g: 1 mL.
6. The method for recovering metallic silver in crystalline silicon components according to claim 1, It is characterized in that In the step S4, the concentration of the ferric chloride solution is 0.2-2 mol / L, and the mass ratio of the added amount of the ferric chloride solution to the silver and copper solids is 10-100 mL: 1 g.
7. The method for recovering metallic silver in crystalline silicon components according to claim 1, It is characterized in that In step S5, the electrolytically purified anode is crude silver, the cathode is high-purity metallic silver, and the electrolyte is a silver nitrate solution.
8. The method for recovering metallic silver in crystalline silicon components according to claim 7, It is characterized in that The content of silver ions in the electrolyte is 50-150 g / L.