Graphene after-finishing agent as well as preparation method and application thereof

Through electrophoresis-assisted filter screening and additive combination, the problems of graphene composite fiber in somatosensory and washing properties are solved, and high adhesion and functional fabric preparation are achieved, avoiding the negative impact of metal impurities ions.

CN118979378APending Publication Date: 2024-11-19ZHEJIANG XIFANG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411065584.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing graphene composite fibers have rough texture in the wear sense, and the color has a great impact. The post-organization process has the problem of degradation of washing performance. The size control of graphene oxide raw materials is poor, easy to fall off, and contain impurity ions that are difficult to separate.

Method used

The graphene post-finishing agent preparation method using electrophoresis-assisted combined with detachable microporous filter membrane is carried out by uniformly mixing the graphene dispersion, chelating agent and pH adjusting agent to perform electrophoresis-assisted filter membrane screening treatment, and small-sized graphene is concentrated. Add additives to improve adhesion and functionality.

Benefits of technology

The adhesion of graphene rear finishing agent is significantly improved, and a fabric with high adhesion, antistatic, antibacterial and far-infrared composite functions is obtained, which avoids the negative impact of metal impurities and improves the anti-water washing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979378A_ABST
    Figure CN118979378A_ABST
Patent Text Reader

Abstract

The invention relates to a graphene after-finishing agent and a preparation method and application thereof, the preparation method of the graphene after-finishing agent comprises the following steps: (1) uniformly mixing a graphene dispersion liquid, a chelating agent and a first pH regulator to obtain a mixed liquid; and (2) carrying out electrophoresis-assisted filter membrane screening treatment on the mixed solution obtained in the step (1), and mixing the obtained graphene reaction solution with a cationic auxiliary agent, a cationic etherifying agent, organic silicone oil and a second pH regulator to obtain the graphene after-finishing agent. Electrophoresis-assisted filter membrane screening treatment is adopted for fine treatment of graphene, and the adhesive force of effective components of the after-finishing agent is remarkably improved; meanwhile, a graphene raw material which does not contain metal impurity ions and has a specific size and oxidation degree is selected, and the fabric with high adhesive force, antistatic property, antibacterial property, far infrared function and other composite functions is obtained by combining with the action of an auxiliary agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of textile technology, and in particular to a graphene finishing agent and a preparation method and application thereof. Background Art

[0002] Functional fibers and textiles refer to new fibers and textiles that have some special functions in addition to the physical and mechanical properties of general fibers and textiles, such as health care fibers and textiles, protective functional fibers and textiles, and comfortable functional fibers and textiles. At present, the various functions of functional fibers include antibacterial, UV protection, far-infrared absorption and emission, antistatic, and anti-electromagnetic radiation. Graphene is considered to be a textile additive with multiple functions, and there are many studies on its application in the textile field in China.

[0003] There are two main ways to prepare graphene functional fabrics. One is the in-situ composite technology, which is to composite graphene materials with textile fiber raw materials and add them during the weaving process to achieve the corresponding functions; the other is the post-finishing technology, which is to give the fibers the corresponding functions through post-finishing auxiliaries.

[0004] CN 104328653A discloses a method for multifunctional finishing of textiles using graphene oxide derivatives, comprising: impregnating a fabric with an aqueous solution of graphene oxide derivatives, drying the fabric, and reducing the fabric so that the surface of the fabric is covered with a layer of reduced graphene oxide derivatives; and then repeating the above steps to obtain a multifunctional fabric with excellent conductive, UV-resistant and water-repellent effects; CN 114502655A discloses a graphene composite antibacterial masterbatch and a preparation method and application thereof, wherein the raw materials for preparing the graphene composite antibacterial masterbatch include a combination of a specific number of silver-plated graphene quantum dots, a polymer matrix, dopamine and polyvinyl pyrrolidone, and the functional masterbatch is used for preparing functional fibers to prepare fiber materials with high transparency, long-term thermal insulation, broad-spectrum antibacterial and high resilience.

[0005] However, the fibers obtained by blending with graphene composite masterbatch have a rough texture when actually worn, and the addition of graphene affects the color of the fiber, resulting in the overall blackness of the fabric. If graphene and other fabrics are selected for blending, the above problems can be effectively improved, but once the content of graphene fiber is lower than the threshold, its overall performance will be significantly reduced; and although the post-finishing scheme is basically not affected by the raw materials, it is subject to the characteristics of the process and has the problem of reduced water washing performance. In addition, the graphene raw materials currently used in the textile field are mostly graphene oxide, which is a graphene derivative rich in oxygen functional groups. Because the graphene itself contains oxygen functional groups and has certain polymer characteristics, the commonly used graphene oxide raw materials cannot achieve precise size control, and there is a problem of poor sheet diameter uniformity. Graphene oxide that is too large is not conducive to attachment to the inside of the fiber and is prone to washing and falling off; in addition, there are impurity ions in graphene oxide that are difficult to separate, and they will eventually remain in the textile fibers.

[0006] CN 107723820A discloses a modified graphene oxide regenerated cellulose composite fiber and a preparation method thereof, wherein the regenerated cellulose composite fiber comprises: 85-99% regenerated cellulose pulp treatment liquid; 0.1-15% modified graphene oxide solution; the ratio of the solid content of cellulose in the regenerated cellulose pulp treatment liquid to the solid content of modified graphene oxide in the modified graphene oxide solution is 100:0.01-5. The modified graphene oxide solution is prepared, and the modified graphene oxide solution is treated with microcapsule technology to improve the dispersibility of the modified graphene oxide, and finally the regenerated cellulose spinning process is used for preparation. However, the water washing resistance of the composite fiber prepared by this method still needs to be improved.

[0007] Therefore, in view of the shortcomings of the prior art, there is an urgent need to provide a graphene finishing agent that enables the fabric to have high adhesion, antistatic, antibacterial and far-infrared composite functions. Summary of the invention

[0008] The purpose of the present invention is to provide a graphene finishing agent and a preparation method and application thereof. The graphene finishing agent is prepared by electrophoresis-assisted combined with a detachable microporous filter membrane, which effectively improves the adhesion of the auxiliary agent in the fabric finishing process, and is conducive to obtaining a fabric with high adhesion, antistatic, antibacterial and far-infrared composite functions.

[0009] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0010] In a first aspect, the present invention provides a method for preparing a graphene finishing agent, the preparation method comprising the following steps:

[0011] (1) uniformly mixing a graphene dispersion, a chelating agent, and a first pH adjuster to obtain a mixed solution;

[0012] (2) The mixed solution obtained in step (1) is subjected to an electrophoresis-assisted filter membrane screening treatment, and the obtained graphene reaction solution is mixed with a cationic auxiliary agent, a cationic etherifying agent, an organic silicone oil and a second pH adjusting agent to obtain the graphene finishing agent.

[0013] The preparation method of the graphene finishing agent provided by the present invention introduces an electric field effect through electrophoresis-assisted reaction, combines filtering and screening treatment with a filter membrane, concentrates graphene with few layers and small sizes in a reaction area, further screens reactive graphene with suitable performance parameters, ensures size uniformity, and significantly improves the adhesion of effective components of the finishing agent; at the same time, a variety of additives are added to obtain composite functions such as antistatic, antibacterial and far infrared.

[0014] Preferably, the iron impurity content of the graphene in the graphene dispersion of step (1) is less than 10 ppm, and the manganese impurity content is less than 5 ppm.

[0015] The iron impurity content of the graphene in the graphene dispersion is less than 10 ppm, for example, it can be 9 ppm, 8 ppm, 5 ppm, 3 ppm or 1 ppm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] The manganese impurity content of the graphene in the graphene dispersion is less than 5 ppm, for example, it can be 4 ppm, 3 ppm or 1 ppm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] Preferably, the graphene in the graphene dispersion in step (1) includes graphene produced by an electrochemical method.

[0018] Preferably, the median particle size D50 of the graphene in the graphene dispersion in step (1) is 1-5 μm, for example, 1 μm, 2 μm, 3 μm, 4 μm or 5 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the degree of oxidation of graphene in the graphene dispersion in step (1) is 5-25%, for example, 5%, 10%, 15%, 20% or 25%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0020] The oxidation degree of the graphene in the graphene dispersion needs to be controlled within a reasonable range. If the oxidation degree is too high, agglomeration will occur in the subsequent process, and ultimately the expected effect cannot be achieved.

[0021] In the present invention, graphene with a specific size and oxidation degree and substantially no metal impurity ions is selected as the raw material, which is conducive to obtaining a fabric with high adhesion, antistatic and antibacterial far-infrared composite functions, and also fundamentally avoids the negative effects of metal ions on textiles and the human body.

[0022] Preferably, the conductivity of the graphene dispersion in step (1) is 100-1000 μS / cm, for example, it can be 100 μS / cm, 300 μS / cm, 500 μS / cm, 800 μS / cm or 1000 μS / cm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] Preferably, the solid content of the graphene dispersion in step (1) is 0.2-1%, for example, 0.2%, 0.4%, 0.6%, 0.8% or 1%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, the dispersant in the graphene dispersion in step (1) includes any one of NMP, SDS, SDBS or PVP.

[0025] Preferably, the mass percentage of the chelating agent in step (1) is 2-5wt% of the mass percentage of the graphene dispersion, for example, it can be 2wt%, 3wt%, 4wt% or 5wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the chelating agent in step (1) comprises ethylenediaminetetraacetic acid.

[0027] The addition of the chelating agent can further eliminate the alkali metal ions in the graphene dispersion.

[0028] Preferably, the amount of the first pH adjuster in step (1) is such that the pH value of the mixed solution is 9-10, for example, 9, 9.5 or 10, but not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] Preferably, in step (1), the first pH adjuster comprises sodium hydroxide.

[0030] The addition of the first pH regulator can improve the overall dispersibility and maintain the activity of the auxiliary agent.

[0031] Preferably, the electrophoresis-assisted membrane screening treatment in step (2) is carried out in an electrophoresis reactor, which comprises a positive electrode tank and a negative electrode tank, wherein the positive electrode tank and the negative electrode tank are separated by a detachable microporous filter membrane, the positive electrode tank is provided with a stirring paddle, and the negative electrode tank is provided with an immersion ultrasonicator.

[0032] Preferably, a positive electrode is disposed in the positive electrode slot, and a negative electrode is disposed in the negative electrode slot.

[0033] Preferably, the electrophoresis-assisted voltage in step (2) is 150-200 V, for example, 150 V, 160 V, 180 V, 190 V or 200 V, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0034] Preferably, the time of the electrophoresis-assisted membrane screening treatment in step (2) is 2-3 hours, for example, 2 hours, 2.5 hours or 3 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0035] Preferably, the specific steps of the electrophoresis-assisted membrane screening treatment in step (2) include: the mixed solution enters the negative electrode tank and is subjected to ultrasonic treatment to obtain graphene with reduced size; the obtained graphene with reduced size migrates to the positive electrode tank through the detachable microporous filter membrane under the action of the electric field, and is stirred and dispersed in the positive electrode tank to obtain a graphene reaction solution.

[0036] Since graphene is usually negatively charged, it will migrate toward the positive electrode under the action of the internal electric field of the solution. The migration speed is related to the size and number of layers of the graphene. The smaller the size and the thinner the number of layers, the easier it is to migrate to the positive electrode. In the present invention, the large and small-sized graphene are spatially isolated in the form of an intermediate diaphragm, and the graphene is ultrasonically treated in the large-sized area, i.e., the negative electrode tank, to further reduce its size, and the small-sized area, i.e., the positive electrode tank, is fully stirred and dispersed.

[0037] Preferably, the volume power density of the ultrasonic treatment is 5-30 kW / m 3 , for example, it can be 5kW / m 3 , 10kW / m 3 , 15kW / m 3 , 20kW / m 3 or 30kW / m 3 , but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the pore size of the detachable microporous filter membrane is 0.5-5 μm, for example, 0.5 μm, 1 μm, 2 μm, 3 μm or 5 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Preferably, the stirring rate of the stirring and dispersing is 200-600 rpm, for example, 200 rpm, 300 rpm, 400 rpm, 500 rpm or 600 rpm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0040] Preferably, the specific steps of mixing in step (2) include: adding a cationic auxiliary agent to the graphene reaction solution for a first stirring, continuing to add a cationic etherifying agent and then heating the solution; then adding silicone oil for a second stirring, and then adding a second pH adjusting agent for a third stirring.

[0041] Preferably, the temperature of the graphene reaction solution is 30-40°C, for example, 30°C, 32°C, 35°C, 38°C or 40°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, the first stirring time is 0.5-1 h, and the speed is 100-300 rpm.

[0043] The first stirring time is 0.5-1 h, for example, 0.5 h, 0.8 h or 1 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0044] The first stirring rate is 100-300 rpm, for example, 100 rpm, 150 rpm, 200 rpm, 250 rpm or 300 rpm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0045] The first stirring rate is low, which can prevent local flocculation of graphene.

[0046] Preferably, the cationic etherifying agent is added at a rate of 0.05-0.2 wt% per minute, for example, 0.05 wt%, 0.1 wt% or 0.2 wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0047] The cationic etherifying agent is used to improve the adhesion performance of the auxiliary agent on the finished fabric.

[0048] Preferably, the temperature rising treatment is: heating to 55-70°C at a heating rate of 0.5-1°C / min, and keeping the temperature for 0.5-1h.

[0049] The heating rate is 0.5-1°C / min, for example, 0.5°C / min, 0.8°C / min or 1°C / min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0050] The end point of the temperature increase is 55-70°C, for example, 55°C, 60°C or 70°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0051] The insulation time is 0.5-1h, for example, 0.5h, 0.8h or 1h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0052] If the temperature during the heating process is too low, the viscosity of the entire system will be too high, and if the temperature is too high, the graphene sheets will agglomerate due to the heat, so it is necessary to control the temperature range and the heating rate.

[0053] Preferably, nitrogen gas is continuously introduced at a unit volume flow rate of 200-400 sccm / L during the temperature rising treatment, for example, 200 sccm / L, 300 sccm / L or 400 sccm / L, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0054] The introduction of nitrogen can prevent the auxiliary agent from being deactivated due to oxidation during high temperature reaction.

[0055] Preferably, the second stirring time is 0.5-1 h, the temperature is 50-60° C., and the speed is 300-400 rpm.

[0056] The second stirring time is 0.5-1 h, for example, 0.5 h, 0.8 h or 1 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0057] The temperature of the second stirring is 50-60°C, for example, 50°C, 55°C or 60°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0058] The second stirring rate is 300-400 rpm, for example, 300 rpm, 320 rpm, 350 rpm, 380 rpm or 400 rpm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0059] Preferably, the third stirring time is 0.5-1 h, and the stirring speed is 500-600 rpm.

[0060] The third stirring time is 0.5-1 h, for example, 0.5 h, 0.8 h or 1 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0061] The third stirring rate is 500-600 rpm, for example, 500 rpm, 520 rpm, 550 rpm, 580 rpm or 600 rpm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0062] Preferably, the mass percentage of the cationic auxiliary agent in step (2) is 0.5-2wt% of the mass percentage of the graphene reaction solution, for example, it can be 0.5wt%, 1wt% or 2wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0063] Preferably, the cationic auxiliary agent in step (2) includes at least one of hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide or octadecyldimethylbenzylammonium chloride.

[0064] The function of the cationic auxiliary agent is to neutralize some functional groups on the graphene and perform cationic treatment on the graphene to facilitate its combination with the fabric.

[0065] Preferably, the mass percentage of the cationic etherifying agent in step (2) is 1-2wt% of the mass percentage of the graphene reaction solution, for example, it can be 1wt%, 1.5wt% or 2wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0066] Preferably, the cationic etherifying agent in step (2) includes 3-chloro-2-hydroxypropyltrimethylammonium chloride and / or 2,3-epoxypropyltrimethylammonium chloride.

[0067] Preferably, the mass percentage of the organic silicone oil in step (2) is 2-5wt% of the mass percentage of the graphene reaction solution, for example, it can be 2wt%, 3wt% or 5wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0068] Preferably, the viscosity of the silicone oil in step (2) is 1000-10000 cP, for example, 1000 cP, 3000 cP, 5000 cP, 8000 cP or 10000 cP, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0069] Preferably, the organic silicone oil in step (2) includes at least one of hydroxy silicone oil, hydrogen silicone oil, amino silicone oil or block silicone oil.

[0070] Preferably, the hydroxy silicone oil comprises cationic hydroxy polysiloxane.

[0071] Preferably, the hydrogen-containing silicone oil comprises methyl hydrogen-containing polysiloxane.

[0072] Preferably, the amino silicone oil comprises aminopolysiloxane having an ammonium value of 0.3-0.6, for example, 0.3, 0.4, 0.5 or 0.6, but not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0073] Preferably, the amount of the second pH adjuster in step (2) is such that the pH value of the graphene finishing agent is 4.5-6.5, for example, 4.5, 5.5 or 6.5, but not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0074] Preferably, in step (2), the second pH adjuster comprises glacial acetic acid.

[0075] In a second aspect, the present invention provides a graphene finishing agent, which is prepared by the preparation method of the graphene finishing agent described in the first aspect.

[0076] The graphene finishing agent provided by the present invention has excellent performance parameters and uniform size, and its effective components have strong adhesion, which is conducive to obtaining fabrics with high adhesion, antistatic, antibacterial and far-infrared composite functions in fabric finishing.

[0077] In a third aspect, the present invention provides an application of the graphene finishing agent as described in the second aspect, wherein the graphene finishing agent is used in the finishing of fabrics, and the finishing includes sequentially performing impregnation, dehydration, pre-drying and drying.

[0078] By using the graphene finishing agent provided by the present invention to finish fabrics, fabrics with high adhesion, antistatic, antibacterial and far-infrared composite functions can be obtained.

[0079] Preferably, the mass percentage of the graphene finishing agent is 1-5wt% of the mass percentage of the fabric, for example, it can be 1wt%, 3wt% or 5wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0080] Preferably, the impregnation includes a first impregnation and a second impregnation performed sequentially.

[0081] Preferably, the temperature of the first impregnation is 20-25° C., the bath ratio is 1:(8-10), and the time is 0.5-1 h.

[0082] The temperature of the first dipping is 20-25°C, for example, 20°C, 22°C or 25°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0083] The bath ratio of the first impregnation is 1:(8-10), for example, 1:8, 1:9 or 1:10, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0084] The first immersion time is 0.5-1 h, for example, 0.5 h, 0.8 h or 1 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0085] Preferably, the second impregnation is carried out at a temperature of 35-40°C and for a time of 0.5-1 h.

[0086] The temperature of the second dipping is 35-40°C, for example, 35°C, 38°C or 40°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0087] The second immersion time is 0.5-1 h, for example, 0.5 h, 0.8 h or 1 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0088] Preferably, the pre-baking temperature is 50-80°C and the time is 35-60 minutes.

[0089] The pre-baking temperature is 50-80° C., for example, 50° C., 65° C. or 80° C., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0090] The pre-baking time is 35-60 minutes, for example, 35 minutes, 50 minutes or 60 minutes, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0091] Preferably, the drying temperature is 110-130° C. and the drying time is 20-60 seconds.

[0092] The drying temperature is 110-130° C., for example, 110° C., 120° C. or 130° C., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0093] The drying time is 20-60 seconds, for example, 20 seconds, 40 seconds or 60 seconds, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0094] Compared with the prior art, the present invention has the following beneficial effects:

[0095] The preparation method of the graphene finishing agent provided by the present invention introduces an electric field effect through electrophoresis-assisted reaction, combines filtering and screening treatment with a filter membrane, concentrates graphene with few layers and small sizes in a reaction area, further screens reactive graphene with suitable performance parameters, ensures size uniformity, and significantly improves the adhesion of effective components of the finishing agent; at the same time, graphene raw materials without metal impurity ions, specific sizes and oxidation degrees are selected, and combined with the effect of auxiliary agents, a fabric with composite functions such as antistatic, antibacterial and far infrared is obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0096] Figure 1 is a schematic structural diagram of an electrophoresis reactor provided in Example 1 of the present invention;

[0097] Wherein: 1, positive electrode tank; 2, negative electrode tank; 3, positive electrode; 4, negative electrode; 5, detachable microporous filter membrane; 6, stirring paddle; 7, immersion ultrasonic device. DETAILED DESCRIPTION

[0098] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0099] Example 1

[0100] This embodiment provides a graphene finishing agent, and the preparation method of the graphene finishing agent comprises the following steps:

[0101] (1) uniformly mixing the graphene dispersion, ethylenediaminetetraacetic acid and sodium hydroxide to obtain a mixed solution with a pH value of 9.5;

[0102] The graphene in the graphene dispersion has an iron impurity content of 5ppm and a manganese impurity content of 3ppm. The graphene is prepared by an electrochemical method, has a median particle size D50 of 3μm, and a degree of oxidation of 5%. The conductivity of the graphene dispersion is 500μS / cm, and the solid content is 0.5%. The mass percentage of ethylenediaminetetraacetic acid is 3wt% of the mass percentage of the graphene dispersion.

[0103] (2) subjecting the mixed solution obtained in step (1) to an electrophoresis-assisted membrane screening treatment for 2.5 h, with an electrophoresis-assisted voltage of 180 V, to obtain a graphene reaction solution;

[0104] The electrophoresis-assisted membrane screening process is carried out in an electrophoresis reactor, such as Figure 1As shown, the electrophoresis reactor comprises a positive electrode tank 1 and a negative electrode tank 2, wherein the positive electrode tank 1 is provided with a positive electrode 3, the negative electrode tank 2 is provided with a negative electrode 4, the positive electrode tank 1 and the negative electrode tank 2 are separated by a detachable microporous filter membrane 5, the positive electrode tank 1 is provided with a stirring paddle 6, and the negative electrode tank 2 is provided with an immersion ultrasonic device 7;

[0105] The specific steps of the electrophoresis-assisted membrane screening process include: the mixed solution enters the negative electrode tank 2, passes through a 15kW / m 3 The graphene with reduced size is obtained by ultrasonic treatment; the graphene with reduced size migrates to the positive electrode tank 1 through a detachable microporous filter membrane 5 with a pore size of 2 μm under the action of an electric field, and is dispersed in the positive electrode tank 1 by stirring at 400 rpm to obtain a graphene reaction solution;

[0106] Then, dodecyltrimethylammonium bromide was added to the graphene reaction solution at 35° C. and stirred for 0.8 h at 200 rpm for the first time, then 3-chloro-2-hydroxypropyltrimethylammonium chloride was added at a rate of 0.1 wt% per minute, and the temperature was raised to 60° C. at a heating rate of 0.8° C. / min, and the temperature was kept for 0.8 h, during which nitrogen gas with a unit volume flow rate of 300 sccm / L was continuously introduced; then, cationic hydroxy polysiloxane with a viscosity of 5000 cP was added and stirred for a second time at 55° C. and 350 rpm for 0.8 h, and then glacial acetic acid was added to make the pH value of the solution 5.5, and then stirred for a third time at 550 rpm for 0.8 h to obtain the graphene finishing agent;

[0107] The mass percentage of the dodecyltrimethylammonium bromide is 1wt% of the mass percentage of the graphene reaction solution; the mass percentage of the 3-chloro-2-hydroxypropyltrimethylammonium chloride is 1.5wt% of the mass percentage of the graphene reaction solution; and the mass percentage of the cationic hydroxypolysiloxane is 3wt% of the mass percentage of the graphene reaction solution.

[0108] The graphene finishing agent is used in the finishing of fabrics, and the mass percentage of the graphene finishing agent is 3wt% of the mass percentage of the fabric; the finishing comprises a first immersion at 22°C and a bath ratio of 1:9 for 0.8h, a second immersion at 38°C for 0.8h, dehydration, pre-baking at 65°C for 50min, and drying at 120°C for 40s.

[0109] Example 2

[0110] This embodiment provides a graphene finishing agent, and the preparation method of the graphene finishing agent comprises the following steps:

[0111] (1) uniformly mixing the graphene dispersion, ethylenediaminetetraacetic acid and sodium hydroxide to obtain a mixed solution with a pH value of 9;

[0112] The graphene in the graphene dispersion has an iron impurity content of 8 ppm and a manganese impurity content of 4 ppm. The graphene is prepared by an electrochemical method, has a median particle size D50 of 1 μm, and a degree of oxidation of 5%. The conductivity of the graphene dispersion is 100 μS / cm, and the solid content is 0.2%. The mass percentage of the ethylenediaminetetraacetic acid is 2 wt% of the mass percentage of the graphene dispersion.

[0113] (2) subjecting the mixed solution obtained in step (1) to an electrophoresis-assisted filter membrane screening treatment for 2 h, with an electrophoresis-assisted voltage of 200 V, to obtain a graphene reaction solution;

[0114] The electrophoresis-assisted membrane screening treatment is carried out in an electrophoresis reactor, which is the same as that in Example 1. The specific steps of the electrophoresis-assisted membrane screening treatment include: the mixed solution enters the negative electrode tank 2, passes through 5kW / m 3 The graphene with reduced size is obtained by ultrasonic treatment; the graphene with reduced size migrates to the positive electrode tank 1 through a detachable microporous filter membrane 5 with a pore size of 5 μm under the action of an electric field, and is dispersed in the positive electrode tank 1 by stirring at 600 rpm to obtain a graphene reaction solution;

[0115] Then, hexadecyltrimethylammonium bromide was added to the graphene reaction solution at 30° C. and stirred for 1 hour at 100 rpm, then 2,3-epoxypropyltrimethylammonium chloride was added at a rate of 0.05 wt% per minute, and the temperature was raised to 55° C. at a heating rate of 0.5° C. / min, and kept warm for 1 hour, during which nitrogen gas with a unit volume flow rate of 200 sccm / L was continuously introduced; then, methyl hydrogenated polysiloxane with a viscosity of 1000 cP was added and stirred for a second time at 50° C. and 300 rpm for 1 hour, and then glacial acetic acid was added to make the pH value of the solution 4.5, and then stirred for a third time at 500 rpm for 1 hour to obtain the graphene finishing agent;

[0116] The mass percentage of the hexadecyltrimethylammonium bromide is 0.5wt% of the mass percentage of the graphene reaction solution; the mass percentage of the 2,3-epoxypropyltrimethylammonium chloride is 1wt% of the mass percentage of the graphene reaction solution; and the mass percentage of the methyl hydrogen-containing polysiloxane is 2wt% of the mass percentage of the graphene reaction solution.

[0117] The graphene finishing agent is used in the finishing of fabrics, and the mass percentage of the graphene finishing agent is 1wt% of the mass percentage of the fabric; the finishing comprises a first immersion at 20°C and a bath ratio of 1:8 for 1h, a second immersion at 35°C for 1h, dehydration, pre-baking at 50°C for 60min, and drying at 110°C for 60s.

[0118] Example 3

[0119] This embodiment provides a graphene finishing agent, and the preparation method of the graphene finishing agent comprises the following steps:

[0120] (1) uniformly mixing the graphene dispersion, ethylenediaminetetraacetic acid and sodium hydroxide to obtain a mixed solution with a pH value of 10;

[0121] The graphene in the graphene dispersion has an iron impurity content of 1 ppm and a manganese impurity content of 1 ppm, the graphene is graphene obtained by an electrochemical method, the median particle size D50 of the graphene is 5 μm, and the degree of oxidation is 25%; the conductivity of the graphene dispersion is 1000 μS / cm, and the solid content is 1%; the mass percentage of the ethylenediaminetetraacetic acid is 5wt% of the mass percentage of the graphene dispersion;

[0122] (2) subjecting the mixed solution obtained in step (1) to an electrophoresis-assisted membrane screening treatment for 3 h, with an electrophoresis-assisted voltage of 150 V, to obtain a graphene reaction solution;

[0123] The electrophoresis-assisted membrane screening treatment is carried out in an electrophoresis reactor, which is the same as that in Example 1. The specific steps of the electrophoresis-assisted membrane screening treatment include: the mixed solution enters the negative electrode tank 2, passes through 30kW / m 3 The graphene with reduced size is obtained by ultrasonic treatment; the graphene with reduced size migrates to the positive electrode tank 1 through a detachable microporous filter membrane 5 with a pore size of 0.5 μm under the action of an electric field, and is dispersed in the positive electrode tank 1 by stirring at 200 rpm to obtain a graphene reaction solution;

[0124] Then, dodecyl trimethyl ammonium bromide is added to the graphene reaction solution at 40° C. and stirred for a first time at 300 rpm for 0.5 h, then 3-chloro-2-hydroxypropyl trimethyl ammonium chloride is added at a rate of 0.2 wt% per minute, and the temperature is raised to 70° C. at a heating rate of 1° C. / min, and the temperature is kept for 0.5 h, during which nitrogen with a unit volume flow rate of 400 sccm / L is continuously introduced; then, aminopolysiloxane with a viscosity of 10000 cP and an ammonium value of 0.4 is added and stirred for a second time at 60° C. and 400 rpm for 0.5 h, and then glacial acetic acid is added to make the pH value of the solution 6.5, and then stirred for a third time at 600 rpm for 0.5 h to obtain the graphene finishing agent;

[0125] The mass percentage of the dodecyltrimethylammonium bromide is 2wt% of the mass percentage of the graphene reaction solution; the mass percentage of the 3-chloro-2-hydroxypropyltrimethylammonium chloride is 2wt% of the mass percentage of the graphene reaction solution; and the mass percentage of the aminopolysiloxane is 5wt% of the mass percentage of the graphene reaction solution.

[0126] The graphene finishing agent is used in the finishing of fabrics, and the mass percentage of the graphene finishing agent is 5wt% of the mass percentage of the fabric; the finishing comprises a first immersion at 25°C and a bath ratio of 1:10 for 0.5h, a second immersion at 40°C for 0.5h, dehydration, pre-baking at 80°C for 35min, and drying at 130°C for 20s.

[0127] Example 4

[0128] This embodiment provides a graphene finishing agent, which is different from Embodiment 1 in that the mass of graphene in the graphene dispersion in step (1) is replaced by graphene oxide, the particle size range of the graphene oxide is 10-20 μm, the degree of oxidation is 40%, and the rest is the same as Embodiment 1.

[0129] Example 5

[0130] This embodiment provides a graphene finishing agent, which is different from embodiment 1 in that the volume power density of the ultrasonic treatment in step (2) is adjusted to 2 kW / m 3 , the rest are the same as in Example 1.

[0131] Example 6

[0132] This embodiment provides a graphene finishing agent, which is different from embodiment 1 in that the volume power density of the ultrasonic treatment in step (2) is adjusted to 35 kW / m 3 , the rest are the same as in Example 1.

[0133] Example 7

[0134] This embodiment provides a graphene finishing agent, which differs from Embodiment 1 in that the end point of the temperature rise treatment in step (2) is adjusted to 50° C., and the rest is the same as Embodiment 1.

[0135] Example 8

[0136] This embodiment provides a graphene finishing agent, which differs from Embodiment 1 in that the end point of the temperature rise treatment in step (2) is adjusted to 80° C., and the rest is the same as Embodiment 1.

[0137] Comparative Example 1

[0138] This comparative example provides a graphene finishing agent, which differs from Example 1 in that step (2) does not include the step of electrophoresis-assisted filter membrane screening treatment, and the rest is the same as Example 1.

[0139] Comparative Example 2

[0140] This comparative example provides a graphene finishing agent, which differs from Example 1 in that dodecyltrimethylammonium bromide is not added in step (2), and the rest is the same as Example 1.

[0141] The graphene finishing agents provided in Examples 1-8 and Comparative Examples 1 and 2 were used for fabric finishing respectively. The prepared fabrics were tested for far infrared performance according to GB / T 30127-2013, and the results are shown in Table 1. The antibacterial rate of Escherichia coli was tested according to GB / T 20944.3-2008, and the results are shown in Table 1. The surface resistivity of the fabric was tested according to GB / T 12703.4-2010, and the results are shown in Table 1.

[0142] After the fabrics prepared in Examples 1-8 and Comparative Examples 1 and 2 were washed 50 times, the far-infrared performance, Escherichia coli antibacterial rate and fiber surface resistivity were tested again according to the above method or equipment to characterize the anti-washing performance of the fabrics. The results are shown in Table 2.

[0143] Table 1

[0144]

[0145] Table 2

[0146]

[0147]

[0148] It can be seen from Table 1 and Table 2 that the fabric prepared by using the graphene finishing agent provided by the present invention for finishing of the fabric has good far infrared, antibacterial and antistatic properties; and after the graphene raw material is refined by the electrophoresis-assisted filter membrane screening process, the water washing resistance of the fabric is greatly improved;

[0149] By comparing Example 1 with Example 4, it can be seen that the water washing resistance of the fabric is reduced by using graphene oxide as the raw material; by comparing Example 1 with Examples 5 and 6, it can be seen that the volume power density of the ultrasonic treatment is too low or too high, the size uniformity of the obtained graphene is reduced, which is not conducive to the attachment to the inside of the fiber, thereby affecting the water washing resistance of the fabric, and the antibacterial property is also reduced; by comparing Example 1 with Examples 7 and 8, it can be seen that if the terminal temperature of the heating treatment is too low, the viscosity of the whole system will be higher, and if the temperature is too high, the graphene sheets will be agglomerated by heat, affecting the adhesion;

[0150] By comparing Example 1 with Comparative Example 1, it can be seen that compared with the preparation of graphene finishing agents by traditional means, the fine treatment of graphene raw materials by electrophoresis-assisted membrane screening process can greatly improve the water washing resistance of the fabric; by comparing Example 1 with Comparative Example 2, it can be seen that not adding cationic additives is not conducive to the adhesion of graphene to the fabric, thereby reducing the water washing resistance of the fabric.

[0151] In summary, the preparation method of the graphene finishing agent provided by the present invention introduces an electric field effect through electrophoresis-assisted reaction, combines the filtering and screening treatment of the filter membrane, concentrates the graphene with few layers and small sizes in the reaction area, further screens the reaction graphene with suitable performance parameters, ensures the uniformity of size, and significantly improves the adhesion of the effective components of the finishing agent; at the same time, a graphene raw material without metal impurity ions, a specific size and oxidation degree is selected, and combined with the effect of the auxiliary agent, a fabric with composite functions such as antistatic, antibacterial and far infrared is obtained.

[0152] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a graphene finishing agent, characterized in that: The preparation method comprises the following steps: (1) uniformly mixing a graphene dispersion, a chelating agent, and a first pH adjuster to obtain a mixed solution; (2) The mixed solution obtained in step (1) is subjected to an electrophoresis-assisted filter membrane screening treatment, and the obtained graphene reaction solution is mixed with a cationic auxiliary agent, a cationic etherifying agent, an organic silicone oil and a second pH adjusting agent to obtain the graphene finishing agent.

2. The preparation method according to claim 1, characterized in that: The iron impurity content of the graphene in the graphene dispersion of step (1) is less than 10 ppm, and the manganese impurity content is less than 5 ppm; Preferably, the graphene in the graphene dispersion in step (1) comprises graphene produced by an electrochemical method; Preferably, the median particle size D50 of the graphene in the graphene dispersion in step (1) is 1-5 μm; Preferably, the oxidation degree of graphene in the graphene dispersion in step (1) is 5-25%; Preferably, the conductivity of the graphene dispersion in step (1) is 100-1000 μS / cm; Preferably, the solid content of the graphene dispersion in step (1) is 0.2-1%.

3. The preparation method according to claim 1 or 2, characterized in that: The mass percentage of the chelating agent in step (1) is 2-5wt% of the mass percentage of the graphene dispersion; Preferably, the chelating agent in step (1) comprises ethylenediaminetetraacetic acid; Preferably, the amount of the first pH adjuster in step (1) is such that the pH value of the mixed solution is 9-10; Preferably, in step (1), the first pH adjuster comprises sodium hydroxide.

4. The preparation method according to any one of claims 1 to 3, characterized in that The electrophoresis-assisted membrane screening treatment in step (2) is carried out in an electrophoresis reactor, wherein the electrophoresis reactor comprises a positive electrode tank and a negative electrode tank, wherein the positive electrode tank and the negative electrode tank are separated by a detachable microporous filter membrane, the positive electrode tank is provided with a stirring paddle, and the negative electrode tank is provided with an immersion ultrasonicator; Preferably, the electrophoresis-assisted voltage in step (2) is 150-200 V; Preferably, the electrophoresis-assisted membrane screening treatment in step (2) is performed for 2-3 hours.

5. The preparation method according to claim 4, characterized in that: The specific steps of the electrophoresis-assisted membrane screening treatment in step (2) include: the mixed solution enters the negative electrode tank, and is subjected to ultrasonic treatment to obtain graphene with reduced size; the obtained graphene with reduced size migrates to the positive electrode tank through the detachable microporous filter membrane under the action of the electric field, and is stirred and dispersed in the positive electrode tank to obtain a graphene reaction solution; Preferably, the volume power density of the ultrasonic treatment is 5-30 kW / m 3 ; Preferably, the pore size of the detachable microporous filter membrane is 0.5-5 μm; Preferably, the stirring rate of the stirring and dispersing is 200-600 rpm.

6. The preparation method according to any one of claims 1 to 5, characterized in that: The specific steps of mixing in step (2) include: adding a cationic auxiliary agent to the graphene reaction solution for a first stirring, continuing to add a cationic etherifying agent and then heating the mixture; then adding silicone oil for a second stirring, and then adding a second pH adjusting agent for a third stirring; Preferably, the temperature of the graphene reaction solution is 30-40°C; Preferably, the first stirring time is 0.5-1h, and the speed is 100-300rpm; Preferably, the cationic etherifying agent is added at a rate of 0.05-0.2 wt % per minute; Preferably, the temperature rising treatment is: heating to 55-70°C at a heating rate of 0.5-1°C / min, and keeping the temperature for 0.5-1h; Preferably, nitrogen gas with a unit volume flow rate of 200-400 sccm / L is continuously introduced during the temperature raising treatment; Preferably, the second stirring time is 0.5-1h, the temperature is 50-60°C, and the speed is 300-400rpm; Preferably, the third stirring time is 0.5-1 h, and the stirring speed is 500-600 rpm.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The mass percentage of the cationic auxiliary agent in step (2) is 0.5-2wt% of the mass percentage of the graphene reaction solution; Preferably, the cationic auxiliary agent in step (2) includes at least one of hexadecyltrimethylammonium bromide, dodecyltrimethylammonium bromide or octadecyldimethylbenzylammonium chloride; Preferably, the mass percentage of the cationic etherifying agent in step (2) is 1-2wt% of the mass percentage of the graphene reaction solution; Preferably, the cationic etherifying agent in step (2) includes 3-chloro-2-hydroxypropyltrimethylammonium chloride and / or 2,3-epoxypropyltrimethylammonium chloride; Preferably, the mass percentage of the organic silicone oil in step (2) is 2-5wt% of the mass percentage of the graphene reaction solution; Preferably, the viscosity of the silicone oil in step (2) is 1000-10000 cP; Preferably, the organic silicone oil in step (2) comprises at least one of hydroxy silicone oil, hydrogen silicone oil, amino silicone oil or block silicone oil; Preferably, the amount of the second pH adjuster in step (2) is such that the pH value of the graphene finishing agent is 4.5-6.5; Preferably, in step (2), the second pH adjuster comprises glacial acetic acid.

8. A graphene finishing agent, characterized in that: The graphene finishing agent is prepared by the preparation method of the graphene finishing agent according to any one of claims 1 to 7.

9. An application of the graphene finishing agent as claimed in claim 8, characterized in that: The graphene finishing agent is used in the finishing of fabrics, and the finishing comprises sequentially performing impregnation, dehydration, pre-drying and drying.

10. The use according to claim 9, characterized in that: The mass percentage of the graphene finishing agent is 1-5wt% of the mass percentage of the fabric; Preferably, the impregnation includes a first impregnation and a second impregnation performed sequentially; Preferably, the temperature of the first dipping is 20-25°C, the bath ratio is 1:(8-10), and the time is 0.5-1h; Preferably, the temperature of the second impregnation is 35-40°C and the time is 0.5-1h; Preferably, the pre-baking temperature is 50-80°C and the time is 35-60min; Preferably, the drying temperature is 110-130° C. and the drying time is 20-60 seconds.