Digestion method of titanium-containing oxide in sodium battery positive electrode material and titanium content detection method

By combining the sintering of barium carbonate with sodium-ion cathode materials and hydrochloric acid dissolution with ICP technology, the complexity and inaccuracy of titanium extraction and detection have been solved, achieving efficient, low-cost, and safe titanium content detection.

CN118980565AActive Publication Date: 2024-11-19TIANJIN ZHONGDIAN NEW ENERGY RES INST CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410996617.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-19
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

Existing technologies for the extraction and detection of titanium in sodium-ion cathode materials suffer from problems such as cumbersome procedures, long analysis cycles, poor precision, high costs, and significant safety risks. In particular, the use of sulfuric acid and strong alkaline substances can easily introduce interfering elements, affecting the accuracy of detection.

Method used

Barium carbonate and sodium-ion battery cathode material are mixed and sintered at 500–800℃ to generate BaTiO3, which is then dissolved in hydrochloric acid. Combined with ICP technology, the titanium content is detected by establishing a standard curve method, avoiding the use of sulfuric acid and strong alkali, thus reducing experimental costs and safety risks.

Benefits of technology

This technology enables efficient conversion and accurate detection of titanium, improving detection efficiency and accuracy, reducing experimental costs and safety risks, and simplifying experimental equipment requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention provides a method for digesting titaniferous oxide in a sodium battery positive electrode material and a method for detecting titanium content, which comprises the following steps of: uniformly mixing the sodium battery positive electrode material with barium carbonate to obtain a material before sintering; sintering the material before sintering in a heating box to obtain a digestion sample I; dissolving the first digestion sample with an acid solution to obtain a second digestion sample; the sintering temperature is 500-800 DEG C, and the sintering time is 1-2 hours; and diluting the digested sample II, fixing the volume, and detecting the titanium content in the digested sample II by utilizing an ICP technology and a standard curve method. According to the preparation method, barium carbonate and the titanium-containing oxide in the sodium battery positive electrode material are mixed and sintered for melting reaction, so that effective conversion of the titanium-containing oxide is realized, convenience is provided for subsequent digestion and titanium extraction, and the yield of the titanium element is improved; the use of sulfuric acid and sodium-containing strong base is avoided, so that the efficiency and the accuracy of detecting the titanium content by utilizing the ICP technology are improved; compared with the prior art, the method has the advantages that the requirements on experimental containers are greatly reduced, and the experimental economy and safety are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sodium battery positive electrode material detection and analysis, in particular to a method for digesting titanium oxides in sodium battery positive electrode materials and a method for detecting titanium content. Background Art

[0002] As a new type of energy storage technology, sodium-ion batteries have attracted much attention in recent years due to their abundant resources, low cost and excellent performance. In sodium-ion batteries, the performance of the positive electrode material has an important impact on the overall performance of the battery. The industry usually uses titanium to inhibit the migration of Fe and Cr, thereby increasing the charging voltage to improve the performance of sodium-based positive electrode materials. Therefore, doping and coating titanium is a key means to improve the electrochemical properties, cycle stability and energy storage efficiency of sodium-based positive electrode materials. Furthermore, the addition and coating of titanium and the precise control of the ratio are crucial to ensure the performance of sodium-ion batteries, which leads to the accurate detection of the titanium content in sodium-based positive electrode materials becoming an urgent problem to be solved.

[0003] Titanium dioxide is a common titanium source. Its unique crystal structure and chemical properties give it unique advantages in the preparation of sodium cathode materials. However, the extraction and detection technology of titanium in sodium cathode materials currently faces great challenges, such as cumbersome operation procedures, long analysis cycles, large workload, and poor precision.

[0004] Since titanium dioxide is soluble in concentrated sulfuric acid and hydrofluoric acid, technicians have tried to use this method to extract titanium from sodium cathode materials. However, the iron oxide in the sodium cathode material will react with sulfuric acid to form iron sulfate, which is insoluble in acid. A large amount of solid suspended matter is instantly generated in the reaction solution, making it difficult to remove impurities and use ICP technology to detect the titanium content.

[0005] In some literature, some technicians have tried to use alkaline substances such as sodium hydroxide or sodium borate as co-solvents to extract titanium from sodium positive electrode materials through high-temperature digestion to improve the yield. However, sodium hydroxide or sodium borate will introduce sodium elements, and in ICP (inductively coupled plasma technology) detection, easily ionized elements such as sodium will interfere with the content detection of the analyte and reduce the accuracy of the results. At the same time, substances such as sodium hydroxide and sodium borate are highly alkaline and have a strong corrosive effect on equipment and containers. Generally, expensive platinum crucibles are required, and the digestion temperature is high (above 800°C), which increases laboratory test costs and experimental safety risks.

[0006] In summary, although the existing measurement methods can measure the titanium content in sodium-ion positive electrode materials to a certain extent, there are still some problems and challenges. Therefore, it is necessary to explore more efficient, accurate and low-cost measurement methods to promote the further development of sodium-ion battery technology. Summary of the invention

[0007] The purpose of the present invention is to provide a method for digesting titanium oxides in sodium-based positive electrode materials and a method for detecting the titanium content, so as to extract the titanium element in the sodium-based positive electrode materials and detect the content thereof more efficiently, accurately and at a low cost.

[0008] One of the technical solutions of the present invention is: a method for digesting titanium oxide in a sodium positive electrode material, which comprises the steps of:

[0009] The sodium positive electrode material and barium carbonate are mixed to obtain a material before sintering;

[0010] The material before sintering is placed in a heating box for sintering to obtain a digestion sample 1;

[0011] Dissolve digestion sample 1 with acid to obtain digestion sample 2.

[0012] Furthermore, the mass ratio of barium carbonate to titanium dioxide in the sodium positive electrode material is greater than 2.5:1.

[0013] Furthermore, the sintering temperature is 500-800° C., and the sintering time is 1 h-2 h.

[0014] Furthermore, the acid solution is hydrochloric acid or aqua regia.

[0015] Another technical solution of the present invention is: a method for detecting titanium content in a sodium battery positive electrode material, comprising the steps of:

[0016] Take the digestion sample 2 obtained by the digestion method of the titanium oxide in the sodium positive electrode material, dilute it with pure water or ultrapure water, and make it constant to volume to obtain a solution to be tested;

[0017] Establishing a standard curve: preparing a series of standard solutions containing titanium, measuring the spectral line intensity of the titanium element in the series of standard solutions under the set working conditions of the inductively coupled plasma atomic emission spectrometer, taking the solution concentration of the titanium element in each standard solution as the abscissa and the spectral line intensity of the titanium element in each standard solution as the ordinate, and fitting a standard curve of solution concentration-spectral line intensity of the titanium element using the standard curve method;

[0018] Under the same working conditions of the inductively coupled plasma atomic emission spectrometer as those for establishing the standard curve, the spectral line intensity of the solution to be tested is measured, and the solution concentration of the titanium element in the solution to be tested is calculated using the standard curve of the titanium element's solution concentration-spectral line intensity. Then, based on the solution concentration of the titanium element in the solution to be tested, the mass proportion of the titanium element in the sodium battery positive electrode material is calculated.

[0019] Furthermore, when establishing the standard curve, the wavelength of the most sensitive analytical line of titanium was 336.121 nm.

[0020] Furthermore, when establishing the standard curve, the working conditions of the inductively coupled plasma atomic emission spectrometer were set as follows: the RF generator power was 1150 W, the pump speed was 50 r / min, and the integration time was 30 s.

[0021] Further, the mass proportion of titanium in the sodium positive electrode material = the mass proportion of titanium in the material before sintering / the mass proportion of the sodium positive electrode material in the material before sintering, and the mass proportion of titanium in the material before sintering w = c*a;

[0022] Wherein: c is the mass proportion of titanium element in digestion sample 1, and a is the sintering mass ratio of sodium battery positive electrode material and barium carbonate.

[0023] Further, c = (solution concentration of titanium element in digestion sample 2 × volume of digestion sample 2) / mass of digestion sample 1; solution concentration of titanium element in digestion sample 2 = solution concentration of titanium element in the test solution × dilution multiple of digestion sample 2.

[0024] Further, a = (M3 - M1) / (M2 - M1);

[0025] Wherein: M1 is the mass of the sintering container, M2 is the total mass of the sodium cathode material, barium carbonate and the sintering container before sintering; M3 is the total mass of the digestion sample 1 and the sintering container after sintering.

[0026] The invention has the beneficial effects of: mixing barium carbonate with titanium-containing oxides in sodium positive electrode materials and sintering them, and performing a melting reaction to convert the titanium-containing oxides into substances that are easily soluble in hydrochloric acid, which not only realizes the effective conversion of the titanium-containing oxides, but also provides convenience for subsequent digestion and titanium extraction, thereby improving the yield of the titanium element; and by avoiding the use of sulfuric acid and sodium-containing strong alkali, the efficiency and accuracy of detecting the titanium content using the ICP technology are improved; compared with the traditional technology, the method greatly reduces the requirements for the experimental container, thereby improving the economic efficiency and safety of the experiment. DETAILED DESCRIPTION

[0027] The present invention will be further described below in conjunction with embodiments:

[0028] Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and comparative examples, and are not intended to limit the scope of protection of the present invention. It should be particularly noted that there may be multiple names for the same organic structure, as long as the structure is within the scope of this patent, it belongs to the protection object of this patent.

[0029] Unless otherwise defined, the raw materials, reagents, etc. in the following examples can be purchased from the market or prepared according to reported methods.

[0030] This embodiment provides a method for digesting titanium oxides in sodium battery positive electrode materials and a method for detecting titanium content, which specifically includes: a stage of extracting titanium from the sodium battery positive electrode material and a stage of detecting the content of the titanium after extraction.

[0031] In the extraction stage of titanium element in the sodium positive electrode material, the above digestion method is used to digest the sodium positive electrode material, and the specific steps include:

[0032] (A1) Mixing a sodium positive electrode material and barium carbonate to obtain a pre-sintering material.

[0033] (A2) The material before sintering is placed in a heating box for sintering to obtain digestion sample 1.

[0034] In this step, titanium dioxide in the sodium positive electrode material reacts with barium carbonate as follows: TiO2+BaCO3==BaTiO3+CO2↑. Therefore, the obtained digestion sample 1 contains BaTiO3 generated by the reaction and other substances in the sodium positive electrode material except titanium dioxide. The BaTiO3 in the digestion sample 1 is soluble in hydrochloric acid. This reaction not only realizes the effective conversion of titanium dioxide, but also facilitates the subsequent digestion and titanium extraction.

[0035] The selected barium carbonate will not introduce easily ionized sodium elements, which can improve the accuracy of ICP detection results of titanium elements; barium carbonate has weak alkalinity and is non-corrosive, and can be contained in ordinary infrared carbon-sulfur crucibles, reducing experimental costs; the temperature required for the reaction of titanium dioxide and barium carbonate is relatively low. Generally speaking, sintering at a temperature of 500-800°C for 1h-2h can make the two fully react, reducing experimental costs and safety risks.

[0036] In this step, the temperature and time of the sintering treatment are critical. When the sintering temperature is 650°C and the sintering time is 1 hour, the reactants can fully melt and react, and the reaction proceeds fully to obtain the ideal product and titanium element yield.

[0037] In order to improve the accuracy of detecting the titanium content in the sodium battery positive electrode material, the barium carbonate that should be added should be able to fully react with the titanium dioxide in the sodium battery positive electrode material. Generally, during the preparation stage of the sodium battery positive electrode material, the titanium doping amount has a known range of values, and the amount of barium carbonate added can be calculated based on the range of values, and the mass ratio of barium carbonate to titanium dioxide in the sodium battery positive electrode material can be controlled to be greater than 2.5:1.

[0038] (A3) After the digestion sample 1 is cooled, the digestion sample 1 is dissolved with acid to obtain the digestion sample 2.

[0039] In this step, the BaTiO3 in the digestion sample 1 and other substances except titanium dioxide in the sodium positive electrode material react with acid solution to generate soluble substances, thereby converting the titanium element into a solution state for quantitative detection. In order to avoid the iron oxides in the sodium positive electrode material from reacting with the acid to generate suspended solids, which affects the detection, the acid solution is preferably hydrochloric acid or aqua regia to avoid the generation of ferric sulfate that is insoluble in acid. In addition, this method can avoid the use of hydrofluoric acid, avoid its corrosion to the glass instruments used in this experiment, and improve the safety of the experiment.

[0040] If the dissolution rate is too slow, it can be heated appropriately to increase the dissolution rate, but it needs to be cooled before the subsequent content detection steps. In order to avoid sampling close to or in contact with the crucible wall, which may introduce impurities and affect the test results, the sampling point of the digestion sample 1 can be controlled at the center of the material in the crucible, and the general sampling amount is 0.1g-0.5g.

[0041] After adding the positive electrode material to be tested to 5mL of hydrochloric acid solution and heating for 10 to 15 minutes, the appropriate hydrochloric acid concentration helps to accelerate the dissolution of the positive electrode material to be tested. In some embodiments, the mass percentage concentration of the hydrochloric acid solution is 5 to 20%; for example, it can be 5%, 15%, 20%, etc., without specific limitation. The mass volume ratio of the positive electrode material to be tested and the hydrochloric acid solution is 0.1g: (5 to 10)mL; for example, it can be 0.1g: 5mL, 0.1g: 6mL, 0.1g: 7mL, 0.1g: 8mL, 0.1g: 9mL or 0.1g: 11mL, etc., without specific limitation.

[0042] In the titanium content detection stage after extraction, ICP technology is used to detect the titanium content. The specific steps include:

[0043] (B1) preparing a series of standard solutions with different gradients: preparing a series of standard solutions with different gradients, wherein the standard solutions contain the element titanium, and measuring the spectral line intensity of the element titanium in the series of standard solutions under set working conditions of an inductively coupled plasma atomic emission spectrometer, taking the solution concentration of the element titanium in each standard solution as the horizontal coordinate and the spectral line intensity of the element titanium in each standard solution as the vertical coordinate, and using a standard curve method to fit a standard curve of the solution concentration of the element titanium - the spectral line intensity.

[0044] In this step, the working conditions of the inductively coupled plasma atomic emission spectrometer are set as follows: the power of the radio frequency generator is 1150 W, the pump speed is 50 r / min, the integration time is 30 s, and the wavelength of the optimal sensitive analysis line of titanium element is 336.121 nm.

[0045] In this step, the concentrations of titanium in the prepared series of gradient standard solutions are 0.5 mg / L, 1 mg / L, 2 mg / L, 5 mg / L and 10 mg / L, respectively. The blank solution (titanium concentration is 0 mg / L) and the titanium concentration in the standard solution are injected and tested in order from low to high to make a standard curve of titanium solution concentration-spectral line intensity.

[0046] (B2) Under the same working conditions of the inductively coupled plasma atomic emission spectrometer as those for establishing the standard curve, the spectral line intensity of the solution to be tested is measured, and the solution concentration of the titanium element in the solution to be tested is calculated using the standard curve of the solution concentration of the titanium element-the spectral line intensity, and then the mass percentage of the titanium element in the sodium battery positive electrode material is calculated based on the solution concentration of the titanium element in the solution to be tested.

[0047] In this step, the mass proportion of titanium in the sodium positive electrode material = the mass proportion of titanium in the material before sintering / the mass proportion of the sodium positive electrode material in the material before sintering, and the mass proportion of titanium in the material before sintering w = c*a;

[0048] The above-mentioned c is the mass proportion of titanium element in digestion sample one, and its calculation method is: c = (solution concentration of titanium element in digestion sample two × volume of digestion sample two) / mass of digestion sample one; solution concentration of titanium element in digestion sample two = solution concentration of titanium element in the test solution × dilution multiple of digestion sample two; the mass of digestion sample one mentioned here is the actual amount of digestion sample one taken when digestion sample one is dissolved in acid.

[0049] The above-mentioned a is the sintering mass ratio of the sodium positive electrode material and barium carbonate, and its calculation method is: a=(M3-M1) / (M2-M1), wherein M1 is the mass of the sintering container, M2 is the total mass of the sodium positive electrode material, barium carbonate and the sintering container before sintering; M3 is the total mass of the digestion sample and the sintering container after sintering.

[0050] Some specific examples are listed below. It should be pointed out that in these specific examples, a mixture of nickel, iron, manganese, sodium oxide and titanium dioxide with known accurate proportions is selected to simulate the sodium positive electrode material for titanium digestion and content detection, so as to calculate the titanium element yield and verify the technical effects of the digestion method and content detection method provided in this application.

[0051] Embodiment 1:

[0052] (1) using a high-speed mixer to uniformly mix barium carbonate, oxides of nickel, iron, manganese, and titanium dioxide to obtain a pre-sintering material, wherein the mass fractions of the substances are 26%, 64%, and 10%, respectively;

[0053] Use a carbon-sulfur crucible as the sintering container and weigh the mass M1 = 16.5546 g;

[0054] The above-mentioned material before sintering is placed in a carbon-sulfur crucible, and the weight M2 is 23.0541 g;

[0055] The carbon-sulfur crucible and the material before sintering were placed in a muffle furnace and sintered at 650°C for 1 hour to perform a melting reaction to obtain a digestion sample 1;

[0056] After cooling, weigh the mass of digestion sample 1 and carbon-sulfur crucible M3 = 22.8915 g;

[0057] The sintering mass ratio a=(M3-M1) / (M2-M1)=97.498% was calculated.

[0058] (2) Remove solution sample 1 from the part that is not in contact with the wall of the carbon-sulfur crucible, weigh 0.1 g and add it to a beaker, add 5 mL of hydrochloric acid to the beaker and place it in a heating furnace at 600° C. for digestion to obtain digestion sample 2, transfer digestion sample 2 to a 100 mL volumetric flask, dilute to volume, and obtain a solution to be tested;

[0059] (3) Based on the concentration of the sample to be tested, the concentrations of titanium in the prepared series of gradient standard solutions were 0.5 mg / L, 1 mg / L, 2 mg / L, 5 mg / L and 10 mg / L, respectively. The blank solution (titanium concentration was 0 mg / L) and the standard solution were injected and tested in the order of low to high titanium concentration to prepare a titanium solution concentration-spectral line intensity standard curve.

[0060] (4) Under the same working conditions of the inductively coupled plasma atomic emission spectrometer as those for establishing the standard curve, the spectral line intensity of the solution to be tested is measured, and the solution concentration of titanium in the solution to be tested is calculated using the standard curve of solution concentration-spectral line intensity of titanium. The working conditions of the inductively coupled plasma atomic emission spectrometer are set as follows: the RF generator power is 1150 W, the pump speed is 50 r / min, the integration time is 30 s, and the wavelength of the optimal sensitive analysis line of titanium is 336.121 nm.

[0061] According to the above formula, the mass proportion of titanium in the digested sample 1 is calculated to be c=6.133%, and the mass proportion of titanium in the material before sintering is further calculated to be w=5.9796%.

[0062] According to the mass proportion of titanium dioxide in the material before sintering being 10%, the mass proportion of titanium in the material before sintering is 5.993%, and the yield of titanium in the digestion method is further calculated to be 99.77%.

[0063] Embodiment 2:

[0064] (1) using a high-speed mixer to uniformly mix barium carbonate, oxides of nickel, iron, manganese, and titanium dioxide to obtain a material before sintering, wherein the mass fractions of the substances are 36%, 60%, and 4%, respectively;

[0065] Use a carbon-sulfur crucible as the sintering container, weighing the mass M1 = 15.0786g;

[0066] The above-mentioned material before sintering is placed in a carbon-sulfur crucible, and the weight M2 is weighed to be 21.6861 g;

[0067] The carbon-sulfur crucible and the material before sintering were placed in a muffle furnace and sintered at 650°C for 1 hour to perform a melting reaction to obtain a digestion sample 1;

[0068] After cooling, weigh the mass of digestion sample 1 and carbon-sulfur crucible M3 = 21.5434 g;

[0069] The sintering mass ratio a=(M3-M1) / (M2-M1)=97.840% was calculated.

[0070] (2) Remove sample 1 from the part that is not in contact with the wall of the carbon-sulfur crucible, weigh 0.1 g and add it to a beaker, add 5 mL of hydrochloric acid to the beaker and place it in a heating furnace at 600° C. to digest, and obtain digestion sample 2, transfer digestion sample 2 to a 100 mL volumetric flask, dilute to volume, and obtain a solution to be tested;

[0071] (3) Based on the concentration of the sample to be tested, the concentrations of titanium in the prepared series of gradient standard solutions were 0.5 mg / L, 1 mg / L, 2 mg / L, 5 mg / L and 10 mg / L, respectively. The blank solution (titanium concentration was 0 mg / L) and the standard solution were injected and tested in the order of low to high titanium concentration to prepare a titanium solution concentration-spectral line intensity standard curve.

[0072] (4) Under the same working conditions of the inductively coupled plasma atomic emission spectrometer as those for establishing the standard curve, the spectral line intensity of the solution to be tested was measured, and the solution concentration of the titanium element in the solution to be tested was calculated using the standard curve of the solution concentration of the titanium element - the spectral line intensity. Then, according to the above formula, the mass proportion of the titanium element in the digested sample 1 was calculated to be c = 2.430%, and then the mass proportion of the titanium element in the material before sintering was calculated to be w = 2.3775%.

[0073] According to the mass proportion of titanium dioxide in the material before sintering being 4%, the mass proportion of titanium in the material before sintering is 2.397%, and the yield of titanium in the digestion method is further calculated to be 99.17%.

[0074] Embodiment 3:

[0075] The difference from Example 1 and Example 2 is that after the nickel iron manganese sodium oxide and titanium dioxide are mixed in a mass ratio of 96:4, 0.1 g is weighed and 5 mL of hydrochloric acid is added thereto for dissolution and then filtered, the filtrate is transferred to a 100 mL volumetric flask, fixed to volume, and a test solution is obtained. The solution concentration of the titanium element in the test solution is detected by the same method as in Example 1 and Example 2, and the mass proportion of the titanium element in the material before dissolution with hydrochloric acid is calculated to be 1.44%, and then it is calculated that the yield of the titanium element in this embodiment is only 60%.

[0076] The above are preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.

Claims

1. A method for digesting titanium oxide in a sodium positive electrode material, characterized in that: Includes steps: The sodium positive electrode material and barium carbonate are mixed to obtain a material before sintering; The material before sintering is placed in a heating box for sintering to obtain a digestion sample 1; Dissolve digestion sample 1 with acid to obtain digestion sample 2.

2. The method for digesting titanium oxide in sodium positive electrode material according to claim 1, characterized in that: The mass ratio of barium carbonate to titanium dioxide in the sodium positive electrode material is greater than 2.5:

1.

3. The method for digesting titanium oxide in sodium positive electrode material according to claim 1, characterized in that: The sintering temperature is 500-800°C, and the sintering time is 1h-2h.

4. The method for digesting titanium oxide in sodium positive electrode material according to claim 1, characterized in that: The acid solution is hydrochloric acid or aqua regia.

5. A method for detecting titanium content in sodium positive electrode materials, characterized in that: Includes steps: Take the digestion sample 2 obtained by the digestion method of titanium oxide in the sodium positive electrode material according to any one of claims 1 to 4, dilute and fix the volume with pure water or ultrapure water to obtain a solution to be tested; Establishing a standard curve: preparing a series of standard solutions containing titanium, measuring the spectral line intensity of the titanium element in the series of standard solutions under the set working conditions of the inductively coupled plasma atomic emission spectrometer, taking the solution concentration of the titanium element in each standard solution as the abscissa and the spectral line intensity of the titanium element in each standard solution as the ordinate, and fitting a standard curve of the solution concentration-spectral line intensity of the titanium element using the standard curve method; Under the same working conditions of the inductively coupled plasma atomic emission spectrometer as those for establishing the standard curve, the spectral line intensity of the solution to be tested is measured, and the solution concentration of the titanium element in the solution to be tested is calculated using the standard curve of the titanium element's solution concentration-spectral line intensity. Then, based on the solution concentration of the titanium element in the solution to be tested, the mass proportion of the titanium element in the sodium battery positive electrode material is calculated.

6. The method for detecting titanium content in sodium positive electrode materials according to claim 5, characterized in that: When establishing the standard curve, the wavelength of the most sensitive analytical line of titanium was 336.121 nm.

7. The method for detecting titanium content in sodium positive electrode materials according to claim 5, characterized in that: When establishing the standard curve, the working conditions of the inductively coupled plasma atomic emission spectrometer were set as follows: the RF generator power was 1150 W, the pump speed was 50 r / min, and the integration time was 30 s.

8. The method for detecting titanium content in sodium battery positive electrode materials according to any one of claims 5 to 7, characterized in that: The mass proportion of titanium in the sodium positive electrode material = the mass proportion of titanium in the material before sintering / the mass proportion of the sodium positive electrode material in the material before sintering, the mass proportion of titanium in the material before sintering w = c * a; Wherein: c is the mass proportion of titanium element in digestion sample 1, and a is the sintering mass ratio of sodium battery positive electrode material and barium carbonate.

9. The method for detecting titanium content in sodium battery positive electrode material according to claim 8, characterized in that: c = (solution concentration of titanium element in digestion sample 2 × volume of digestion sample 2) / mass of digestion sample 1; solution concentration of titanium element in digestion sample 2 = solution concentration of titanium element in the test solution × dilution multiple of digestion sample 2.

10. The method for detecting titanium content in sodium battery positive electrode material according to claim 8, characterized in that: a=(M3-M1) / (M2-M1); Wherein: M1 is the mass of the sintering container, M2 is the total mass of the sodium cathode material, barium carbonate and the sintering container before sintering; M3 is the total mass of the digestion sample 1 and the sintering container after sintering.

Citation Information

Patent Citations

  • Processes for producing barium titanyl salt and barium titanate

    CN103459319A

  • Method for microwave-assisted preparation of barium calcium zirconate titanate powder

    CN107879750A

  • Method for determining manganese and titanium content in ferrophosphorus through microwave digestion ICP-AES method

    CN110174395A

  • X-ray fluorescence spectrum detection method for ferrotitanium and titanium alloy

    CN113866202A

  • Chemical analysis method for detecting silicon carbide-containing refractory material