Preparation method of halogen-free insulating plate with CTI value greater than 600V
Through the combination of ZIF-8@Al(OH)3 filler and halogen-free epoxy resin, the CTI value and heat resistance of the insulating plate are improved, and the insufficient CTI value of the existing halogen-free insulating plates and poor interface bonding strength are solved. The problem of the high-performance insulating plate is realized.
Patent Information
- Application Number
- CN202411039394.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The existing halogen-free insulating plates have insufficient CTI value, poor heat resistance and interface bonding strength, which limits its application in humid environments.
ZIF-8@Al(OH)3 is used as filler, and the insulating plate is made by combining the metal organic framework material ZIF-8 with aluminum hydroxide, combined with halogen-free epoxy resin adhesive, and baking and hot pressing. Improve the CTI value and interface binding strength.
A insulation board with a CTI value greater than 600V has been achieved. The interface bonding strength of the surface is high, the heat resistance is good, and there is no need to add a coupling agent. The compatibility between the filler and the epoxy resin is good, which solves the uneven distribution of aluminum hydroxide filler. The problem.
Smart Images

Figure CN118983154A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a halogen-free insulating plate with a CTI value greater than 600V, belonging to the technical field of insulating plates. Background Art
[0002] In the field of insulation boards, laminated boards are one of the common insulation boards. The production process of laminated boards is as follows:
[0003] First, the glass fiber cloth is impregnated with resin glue and baked to be semi-dry to form a prepreg. Then several prepregs are placed in a mold and heat-pressed and cured using a hot press to form a laminate.
[0004] On the one hand, halogen-containing laminates will release highly toxic substances such as hydrogen halides due to the large amount of smoke they produce during combustion. Therefore, halogen-free laminates have been a development trend in recent years.
[0005] On the other hand, in order to improve the safety and reliability of electronic products, especially for the safety and reliability of insulating materials (such as motors, electrical appliances, etc.) used in humid environments, developing high-insulation products to ensure the safety and reliability of electronic products has been an important development direction in recent years. The CTI value (Comparative Tracking Index) of insulating materials refers to the highest voltage value that the surface of the material can withstand 50 drops of electrolyte (0.1% ammonium chloride aqueous solution) without forming leakage traces. It measures the insulation safety performance of the material to a certain extent. The higher this value, the better the insulation of the material. Therefore, high CTI insulating boards have become a research and development trend in the electronics industry.
[0006] Current halogen-free insulation boards usually utilize a dicyandiamide-cured halogen-free epoxy system, and the CTI is mainly improved by adding aluminum hydroxide. However, the heat resistance of the laminated board of this system is poor; if it is compounded with other materials, the interface bonding strength of its surface is limited, all of which restrict its application.
[0007] Based on this, the present invention is proposed. Summary of the invention
[0008] In view of the shortcomings of the prior art, the present invention provides a method for preparing a halogen-free insulating board with a CTI value greater than 600V. The specific technical scheme is as follows:
[0009] A method for preparing a halogen-free insulating board with a CTI value greater than 600V comprises the following steps:
[0010] Step 1: Synthesis of ZIF-8@Al(OH)3
[0011] The metal organic framework material ZIF-8 and aluminum hydroxide are dispersed in water, ultrasonicated, centrifuged, filtered, dried in an oven, and ground to obtain ZIF-8@Al(OH)3;
[0012] Step 2: Preparation of epoxy resin adhesive
[0013] The halogen-free epoxy resin, meline amide, curing agent, accelerator, solvent and ZIF-8@Al(OH)3 are mixed and stirred uniformly to obtain epoxy resin adhesive;
[0014] Step 3: Stacking and hot pressing
[0015] The epoxy resin adhesive is coated on the glass fiber cloth and baked to form a semi-cured sheet; after stacking a plurality of semi-cured sheets, they are sent to a hot press for hot pressing, and after the hot pressing is completed, they are cooled to obtain the halogen-free insulating board with a CTI value greater than 600V.
[0016] In a further improvement, the curing agent is dicyandiamide.
[0017] In a further improvement, the accelerator is 2-methylimidazole.
[0018] In a further improvement, the solvent is one of acetone, butanone, cyclohexanone, methanol, ethanol, toluene and xylene.
[0019] As a further improvement, in step one, the mass ratio of the metal organic framework material ZIF-8 to aluminum hydroxide is 2:5, ultrasonic cleaning is performed for 30 to 60 minutes, and centrifugation is performed for 10 to 15 minutes.
[0020] As a further improvement, in step 2, the mass ratio of halogen-free epoxy resin, melinamide, curing agent, accelerator, solvent, and ZIF-8@Al(OH)3 is 100:13:(2-2.5):(0.07-0.1):(80-100):(55-70).
[0021] As a further improvement, in step three, the glass fiber cloth coated with the epoxy resin adhesive is baked at 170-180° C. for 1-5 minutes to obtain a prepreg.
[0022] As a further improvement, in step three, the stacked prepreg is placed in a mold and hot-pressed at 180-200° C. and 3.5-5 MPa for 1-2 hours, then cooled to room temperature and demolded.
[0023] Beneficial effects of the present invention:
[0024] The insulating board made by the present invention does not contain halogen, has a CTI value greater than 600V, has high interface bonding strength on the surface of the insulating board, is easy to be hot-pressed and composited with other materials, and has high heat resistance. Aluminum hydroxide is composited with a metal organic framework material ZIF-8 to form ZIF-8@Al(OH)3. Since the metal organic framework material ZIF-8 has a three-dimensional pore structure, the metal ions are used as connection points, and the organic ligands are used as support to form a 3D extension of the space. Therefore, the new filler can form a coating material with Al(OH)3, and since it contains organic ligands, the compatibility between the metal organic framework material ZIF-8 and the epoxy resin is very good, and the problems of agglomeration and uneven distribution caused by excessive aluminum hydroxide filler are finally solved. In addition, there is no need to add a coupling agent, and the bonding between the inorganic filler and the epoxy resin is also good. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a photo of the halogen-free insulating board with a CTI value greater than 600V described in Example 1;
[0026] Figure 2 This is a photo of the halogen-free insulating board with a CTI value greater than 600V described in Example 2;
[0027] Figure 3 This is a photo of the halogen-free insulating board with a CTI value greater than 600V described in Example 3. DETAILED DESCRIPTION
[0028] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0029] Example 1
[0030] Step 1: Synthesis of ZIF-8@Al(OH)3
[0031] Dispersing metal organic framework material ZIF-8 and aluminum hydroxide in water, with the mass ratio of metal organic framework material ZIF-8 to aluminum hydroxide being 2:5, ultrasonicating for 30 minutes in an ultrasonic cleaner, centrifuging for 10 minutes, filtering, drying in an oven, and grinding to obtain ZIF-8@Al(OH)3;
[0032] Step 2: Preparation of epoxy resin adhesive
[0033] Halogen-free epoxy resin, melinamide, dicyandiamide, 2-methylimidazole, butanone, and ZIF-8@Al(OH)3 were mixed and stirred in a mass ratio of 100:13:2:0.07:80:55 to obtain an epoxy resin adhesive;
[0034] Step 3: Stacking and hot pressing
[0035] The epoxy resin adhesive is coated on the glass fiber cloth and baked at 170°C for 5 minutes to form a prepreg; after stacking multiple prepregs, the stacked prepregs are placed in a mold and hot-pressed at 180°C and 5MPa for 2 hours, then cooled to room temperature and demolded to obtain the halogen-free insulation board with a CTI value greater than 600V. The actual photo is shown in Figure 1 .
[0036] Example 2
[0037] Step 1: Synthesis of ZIF-8@Al(OH)3
[0038] The metal organic framework material ZIF-8 and aluminum hydroxide are dispersed in water, the mass ratio of the metal organic framework material ZIF-8 to aluminum hydroxide is 2:5, ultrasonicated by an ultrasonic cleaner for 50 minutes, centrifuged for 12 minutes, filtered, dried in an oven, and ground to obtain ZIF-8@Al(OH)3;
[0039] Step 2: Preparation of epoxy resin adhesive
[0040] Halogen-free epoxy resin, melinamide, dicyandiamide, 2-methylimidazole, butanone, and ZIF-8@Al(OH)3 were mixed and stirred in a mass ratio of 100:13:2.2:0.08:90:60 to obtain an epoxy resin adhesive;
[0041] Step 3: Stacking and hot pressing
[0042] The epoxy resin adhesive is coated on the glass fiber cloth and baked at 175°C for 3 minutes to form a prepreg; after stacking multiple prepregs, the stacked prepregs are placed in a mold and hot-pressed at 190°C and 4MPa for 1.5 hours, then cooled to room temperature and demolded to obtain the halogen-free insulation board with a CTI value greater than 600V. The actual photo is shown in Figure 2 .
[0043] Example 3
[0044] Step 1: Synthesis of ZIF-8@Al(OH)3
[0045] The metal organic framework material ZIF-8 and aluminum hydroxide are dispersed in water, the mass ratio of the metal organic framework material ZIF-8 to aluminum hydroxide is 2:5, ultrasonicated by an ultrasonic cleaner for 60 minutes, centrifuged for 15 minutes, filtered, dried in an oven, and ground to obtain ZIF-8@Al(OH)3;
[0046] Step 2: Preparation of epoxy resin adhesive
[0047] Halogen-free epoxy resin, melinamide, dicyandiamide, 2-methylimidazole, butanone, and ZIF-8@Al(OH)3 were mixed and stirred in a mass ratio of 100:13:2.5:0.1:100:70 to obtain an epoxy resin adhesive;
[0048] Step 3: Stacking and hot pressing
[0049] The epoxy resin adhesive is coated on the glass fiber cloth and baked at 180°C for 1 minute to form a prepreg; after stacking multiple prepregs, the stacked prepregs are placed in a mold and hot-pressed at 200°C and 3.5MPa for 1 hour, then cooled to room temperature and demolded to obtain the halogen-free insulation board with a CTI value greater than 600V. The actual photo is shown in Figure 3 .
[0050] Comparative Example 1
[0051] The only difference between this example and Example 1 is that Al(OH)3 is used in the epoxy resin adhesive of this example to replace ZIF-8@Al(OH)3, and the rest remains unchanged.
[0052] Comparative Example 2
[0053] The difference between this example and Example 1 is that the epoxy resin adhesive in this example uses a mixture of metal organic framework material ZIF-8 and Al(OH)3 to replace ZIF-8@Al(OH)3, and the rest remains unchanged. Among them, the mixture of metal organic framework material ZIF-8 and Al(OH)3 is prepared by mixing metal organic framework material ZIF-8 and aluminum hydroxide in a mass ratio of 2:5.
[0054] Comparative Example 3
[0055] The only difference between this example and Example 1 is that this example uses Al(OH)3 instead of Mg(OH)2 to finally produce ZIF-8@Mg(OH)2. In this example, ZIF-8@Mg(OH)2 is used in the epoxy resin adhesive instead of ZIF-8@Al(OH)3, and the rest remains unchanged.
[0056] Comparative Example 4
[0057] The only difference between this example and Example 1 is that the epoxy resin adhesive in this example is prepared by mixing and evenly stirring halogen-free epoxy resin, dicyandiamide, 2-methylimidazole, butanone, and ZIF-8@Al(OH)3 in a mass ratio of 113:2:0.07:80:55, and the rest remain unchanged.
[0058] Comparative Example 5
[0059] The only difference between this example and Example 1 is that 4,4'-diaminodiphenyl ether is used to replace meline amide in this example, and the rest remains unchanged.
[0060] 《Insulation board performance characterization test》
[0061] 1. The interfacial bonding strength of the insulating board surface is characterized by the glass strength of the copper clad laminate. The copper clad laminate sample is made by laying copper foil (1OZ) on the upper and lower layers of the stacked semi-cured sheet during the stacking and hot pressing steps. After the hot pressing is completed, the copper foil and the insulating board are hot-pressed into one. The peel strength of the copper foil is measured to characterize the interfacial bonding strength of the insulating board surface.
[0062] 2. Test CTI and glass transition temperature according to IPC-TM-650. It should be noted that since the upper limit of the CTI test is 600V, if no leakage trace is found when the CTI value reaches 600V, it means that the CTI value of the insulation board is greater than 600V.
[0063] 3. Inspection of filler uniformity
[0064] Cut the insulating board into a test board of 5cm×5cm×0.3cm, immerse the test board in 300℃ tin liquid, keep it for a while, then take it out and observe whether the test board has bubbling, stratification and other phenomena. For insulating boards with high aluminum hydroxide content, since aluminum hydroxide is easy to decompose at a high temperature of 300℃, when multiple bubbles appear locally but no stratification occurs, it means that the filler is unevenly distributed; if stratification caused by large bubbles (usually the bubble diameter is greater than 2cm) occurs, it means that the uniformity is good. In addition, when testing, after approaching the critical value, take it out immediately for observation after immersing in tin for 1s.
[0065] The insulation board properties corresponding to Examples 1 to 3 and Comparative Examples 1 to 5 are shown in Table 1:
[0066] Table 1
[0067] Peel strength (lb / in) CTI value (V) Glass transition temperature(℃) Packing uniformity Example 1 10.5 >600 164 Immersion tin for 350s without blistering or delamination Example 2 10.7 >600 165 Immersion tin for 350s without blistering or delamination Example 3 10.9 >600 168 Immersion tin for 350s without blistering or delamination Comparative Example 1 8.1 >600 163 Immersion tin 203s bubbling but no stratification Comparative Example 2 8.3 500 164 Immersion tin 186s bubbling but no stratification Comparative Example 3 10.6 500 162 Immersion tin for 350s without blistering or delamination Comparative Example 4 10.1 >600 151 Immersion tin for 350s without blistering or delamination Comparative Example 5 10.2 >600 154 Immersion tin for 350s without blistering or delamination
[0068] It can be seen from Comparative Example 1 that if the aluminum hydroxide content is too high, although the CTI value can reach 600V, it will significantly affect the peel strength and filler uniformity.
[0069] It can be seen from Comparative Example 2 that the mixture of metal organic framework materials ZIF-8 and Al(OH)3 is equivalent to directly adding metal organic framework materials ZIF-8 and Al(OH)3, the two are not compounded, the dispersion of the filler is not good, especially the distribution between two different types of fillers is poor.
[0070] It can be seen from Comparative Example 3 that the CTI value of the composite of magnesium hydroxide and metal organic framework material ZIF-8 cannot reach 600V.
[0071] It can be seen from Comparative Example 4 that adding melinamide to epoxy resin can significantly improve heat resistance and glass transition temperature.
[0072] In the above embodiments, the halogen-free epoxy resin is purchased from Hongchang Electronic Materials Co., Ltd., and its trade name is GEBR589K75.
[0073] The metal organic framework material ZIF-8 can be purchased from outside or made by oneself. The method of making by oneself is as follows:
[0074] 2-Methylimidazole and zinc nitrate hexahydrate react in water to generate the metal organic framework material ZIF-8.
[0075] When mixing halogen-free epoxy resin, meline amide, dicyandiamide, 2-methylimidazole, butanone, and ZIF-8@Al(OH)3, dicyandiamide and 2-methylimidazole can be first dissolved in 10 times (by mass) butanone to prepare a curing accelerator liquid, and then the remaining butanone and the curing accelerator liquid are added to the halogen-free epoxy resin and meline amide, and finally ZIF-8@Al(OH)3 is added in batches and stirred evenly.
[0076] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a halogen-free insulating board with a CTI value greater than 600V, characterized in that: The following steps are involved: Step 1: Synthesis of ZIF-8@Al(OH)3 The metal organic framework material ZIF-8 and aluminum hydroxide are dispersed in water, ultrasonicated, centrifuged, filtered, dried in an oven, and ground to obtain ZIF-8@Al(OH)3; Step 2: Preparation of epoxy resin adhesive The halogen-free epoxy resin, meline amide, curing agent, accelerator, solvent and ZIF-8@Al(OH)3 are mixed and stirred uniformly to obtain epoxy resin adhesive; Step 3: Stacking and hot pressing The epoxy resin adhesive is coated on the glass fiber cloth and baked to form a semi-cured sheet; after stacking a plurality of semi-cured sheets, they are sent to a hot press for hot pressing, and after the hot pressing is completed, they are cooled to obtain the halogen-free insulating board with a CTI value greater than 600V.
2. The method for preparing a halogen-free insulating board with a CTI value greater than 600V according to claim 1, characterized in that: The curing agent is dicyandiamide.
3. The method for preparing a halogen-free insulating board with a CTI value greater than 600V according to claim 1, characterized in that: The accelerator is 2-methylimidazole.
4. The method for preparing a halogen-free insulating board with a CTI value greater than 600V according to claim 1, characterized in that: The solvent is one of acetone, butanone, cyclohexanone, methanol, ethanol, toluene and xylene.
5. The method for preparing a halogen-free insulating board with a CTI value greater than 600V according to claim 1, characterized in that: In step 1, the mass ratio of the metal organic framework material ZIF-8 to aluminum hydroxide is 2:5, and the product is ultrasonicated by an ultrasonic cleaner for 30 to 60 minutes and centrifuged for 10 to 15 minutes.
6. The method for preparing a halogen-free insulating board with a CTI value greater than 600V according to claim 1, characterized in that: In step 2, the mass ratio of halogen-free epoxy resin, melinamide, curing agent, accelerator, solvent, and ZIF-8@Al(OH)3 is 100:13:(2-2.5):(0.07-0.1):(80-100):(55-70).
7. The method for preparing a halogen-free insulating board with a CTI value greater than 600V according to claim 1, characterized in that: In step three, the glass fiber cloth coated with the epoxy resin adhesive is baked at 170-180° C. for 1-5 minutes to obtain a prepreg.
8. The method for preparing a halogen-free insulating board with a CTI value greater than 600V according to claim 1, characterized in that: In step three, the stacked prepreg is placed in a mold and hot-pressed at 180-200° C. and 3.5-5 MPa for 1-2 hours, then cooled to room temperature and demolded.
Citation Information
Cited By
Low-temperature curing epoxy adhesive and preparation method thereof
CN119709079A