Method for reducing wafer defects

By depositing a metal layer on the wafer surface and bombarding the inner wall of the opening with inert gas, the crystallization defects caused by gas residue after the passivation layer etching are solved, and wafer quality and device performance are improved.

CN118983213APending Publication Date: 2024-11-19SHANGHAI HUALI INTEGRATED CIRCUIT CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411038055.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

During the wafer manufacturing process, after the passivation layer etches, crystal defects are generated on the wafer surface due to the residue of etching gas, which affects the wafer quality and device performance.

Method used

The metal layer is deposited on the wafer surface and filled around it with a passivation layer, the passivation layer is etched to form an opening, expose the metal layer, and then bombard the inner wall of the opening with an inert gas such as argon to reduce etching gas residue.

Benefits of technology

By reducing etching gas residues, avoiding the chemical reaction between metal aluminum and air, the generation of crystallization defects is reduced, and wafer quality and device performance are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983213A_ABST
    Figure CN118983213A_ABST
Patent Text Reader

Abstract

The invention provides a method for reducing wafer defects, and belongs to the field of semiconductors. The method for reducing the wafer defects comprises the steps that a wafer is provided, a metal layer is deposited on the surface of the wafer, and the periphery of the metal layer is filled with a passivation layer; etching the passivation layer and stopping at the metal layer so as to form an opening in the metal layer and expose the metal layer; cleaning the wafer in which the opening is formed; and for the cleaned wafer, bombarding the inner wall of the opening by using inert gas. According to the method, after the passivation layer is etched, the argon is adopted to bombard the inner wall of the opening to reduce the concentration of the etching gas remaining on the inner wall of the opening, so that chemical reaction of the etching gas, metal aluminum and air can be avoided, crystal defects formed on the wafer can be reduced, and the quality and yield of the wafer are improved. And meanwhile, the performance of the device is also improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for reducing wafer defects. Background Art

[0002] In the process of wafer manufacturing, passivation is one of the last important steps, which occurs after the circuit is built and metallized and interconnected. The main purpose of passivation is to protect the integrated circuit from the external environment and reduce the surface state density inside the device, thereby improving the reliability and performance of the device. After the passivation step is completed, the wafer is ready to enter the next step, which is wafer-level packaging or cutting into individual chips, followed by chip-level packaging or traditional packaging.

[0003] Currently in the large-scale wafer manufacturing process, after the wafers have completed the passivation step and have been packaged and stored for more than a month, electron microscope inspection has revealed crystallization. The specific reason is that the etching of the passivation layer is the last step to form the aluminum lead part. Because CF4 / CHF3 containing "F" is used to etch the passivation layer in the etching step, and the passivation layer is a stacked structure of silicon oxide and silicon nitride, even with wet etching and cleaning, there will be F residues on the surface of the wafer. If the wafers are not packaged in time and have been stored in the warehouse, after the passivation layer is etched, the "F" gas and the polymers remaining on the surface of the wafer will react with metal aluminum when encountering water vapor in the atmosphere to form crystals. The specific reaction formula is Al+HF+H2O->AlOxFy. Figure 1 As shown, Figure 1 This is an electronic scanning image of the wafer. It can be seen from the image that there are crystal defects in the wafer growth. Crystal defects seriously affect the quality of the wafer, thereby affecting the wafer yield and reducing the performance of the device.

[0004] It should be noted that the information disclosed in the background technology section of the invention is only intended to deepen the understanding of the general background technology of the invention, and should not be regarded as an admission or suggestion in any form that the information constitutes prior art already known to those skilled in the art. Summary of the invention

[0005] The object of the present invention is to provide a method for reducing wafer defects, so as to solve the problem that when etching a passivation layer, the residual etching gas causes crystal defects to be generated on the surface of the wafer.

[0006] In order to solve the above technical problems, the present invention provides a method for reducing wafer defects, comprising:

[0007] Providing a wafer, depositing a metal layer on the surface of the wafer, and filling a passivation layer around the metal layer;

[0008] Etching the passivation layer and stopping at the metal layer to form an opening in the metal layer to expose the metal layer;

[0009] cleaning the wafer having the opening formed thereon;

[0010] For the cleaned wafer, an inert gas is used to bombard the inner wall of the opening.

[0011] Preferably, the passivation layer includes a silicon nitride layer and a silicon oxide layer.

[0012] Preferably, the metal layer is an aluminum metal layer.

[0013] Preferably, the ratio of the area of ​​the opening to the area of ​​the wafer is less than 10%.

[0014] Preferably, cleaning the wafer with the opening formed therein comprises:

[0015] The wafer having the opening formed therein is cleaned by wet cleaning.

[0016] Preferably, the inert gas is argon.

[0017] Preferably, the flow rate of the argon gas is 1000 scmm, and the pressure of the argon gas bombarding the inner wall of the opening is 500 mtorr.

[0018] Preferably, a mixed gas of CF4 and CHF3 is used to etch the passivation layer.

[0019] Preferably, after bombarding the surface of the opening of the cleaned wafer with argon gas, the method for reducing wafer defects further comprises:

[0020] Use oxygen to push the top of the opening to expand the process window at the top of the opening.

[0021] Preferably, the thickness of the metal aluminum deposition is 6 μm.

[0022] Compared with the prior art, the method for reducing wafer defects of the present invention has the following advantages:

[0023] The present invention provides a wafer, deposits a metal layer on the surface of the wafer, and a passivation layer is filled around the metal layer. The passivation layer is etched and stopped at the metal layer to form an opening in the metal layer to expose the metal layer. The wafer with the opening is cleaned. For the cleaned wafer, the inner wall of the opening is bombarded with an inert gas. Therefore, the method for reducing wafer defects provided by the present invention uses argon gas to bombard the inner wall of the opening after etching the passivation layer to reduce the concentration of the etching gas remaining on the inner wall of the opening, thereby avoiding chemical reactions between the etching gas, metal aluminum and air, thereby reducing the formation of crystal defects in the wafer and improving the wafer quality and yield. At the same time, the performance of the device is also improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is an electronic scan of the wafer;

[0025] Figure 2 is a schematic diagram of a structure in which a crystal is grown on an aluminum lead opening formed in one embodiment of the present invention;

[0026] Figure 3 is a flow chart of a method for reducing wafer defects in one embodiment of the present invention;

[0027] Figure 4 is a schematic diagram of a structure in which aluminum leads are formed on a wafer surface in one embodiment of the present invention;

[0028] Figure 5 This is a schematic diagram of electronic scanning of wafer defects in one embodiment of the present invention without using the method for reducing wafer defects provided by the present invention;

[0029] Figure 6 This is a schematic diagram of electronic scanning of wafer defects using the method for reducing wafer defects provided by the present invention in one embodiment of the present invention;

[0030] Figure 7 is a graph showing the relationship between the F content and the reduced thickness of aluminum tested in one embodiment of the present invention;

[0031] In the figure,

[0032] 100-wafer; 110-metal copper;

[0033] 120-titanium nitride layer; 130-crystallization;

[0034] 200-silicon oxide layer; 300-silicon nitride layer;

[0035] 400-aluminum metal layer; 500-opening;

[0036] 600-passivation layer. DETAILED DESCRIPTION

[0037] In order to make the purpose, advantages and features of the present invention clearer, the method for reducing wafer defects proposed by the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the drawings are all in a very simplified form and use non-precise proportions, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. It should be understood that the drawings in the specification do not necessarily show the specific structure of the present invention in proportion, and the illustrative features used to illustrate certain principles of the present invention in the drawings in the specification will also adopt a slightly simplified drawing method. The specific design features of the present invention disclosed herein include, for example, specific dimensions, directions, positions and shapes, which will be determined in part by the specific environment to be applied and used. And, in the embodiments described below, sometimes the same figure mark is used in common between different drawings to represent the same part or a part with the same function, and its repeated description is omitted. In this specification, similar numbers and letters are used to represent similar items, so once an item is defined in one drawing, it does not need to be further discussed in subsequent drawings.

[0038] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0039] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0040] like Figure 2As shown, in the process of wafer manufacturing, passivation is one of the last important steps. An aluminum metal layer 400 is deposited on the surface of the wafer. In the last step, a passivation layer 600 is deposited on the surface of the wafer. The passivation layer 600 completely wraps the aluminum metal layer 400. Next, the passivation layer 600 is etched to form an opening 500 to expose the aluminum metal layer. When etching the passivation layer 600, a large amount of "F" gas is gathered at the opening 500. The "F" gas reacts chemically with the metal aluminum and substances in the air, thereby generating the following on the inner wall of the opening 500: Figure 1 He Ru Figure 2 The crystallization 130. Crystallization defects seriously affect the quality of the wafer, thereby affecting the wafer yield and reducing the performance of the device.

[0041] The core idea of ​​the present invention is to provide a method for reducing wafer defects, which can reduce the formation of crystal defects in the wafer and improve the wafer quality and yield.

[0042] In order to realize the above idea, the present invention provides a method for reducing wafer defects. Figures 3 to 7 A specific implementation of a method for reducing wafer defects disclosed herein includes the following steps S1 to S4.

[0043] Step S1: providing a wafer 100 , depositing a metal layer on the surface of the wafer 100 , and filling a passivation layer 600 around the metal layer.

[0044] Specifically, refer to Figure 3 and Figure 4 As shown, wafer 100 is a finished wafer that has completed testing. After the passivation step of the wafer is completed, it is ready to be packaged or cut into individual chips, and then chip-level packaging or traditional packaging is performed. The metal layer deposited on the surface of wafer 100 is an aluminum metal layer 400. The thickness of the aluminum metal deposition is 6μm. The aluminum metal layer 400 is filled with a passivation layer 600. The passivation layer 600 completely wraps the aluminum metal layer 400 to play an isolation role. In this embodiment, the passivation layer 600 includes a silicon nitride layer 300 and a silicon oxide layer 200. The silicon nitride layer 300 is deposited on the surface of the silicon oxide layer 200. The thickness of the deposited silicon nitride layer 300 is The thickness of the deposited silicon oxide layer 200 is It should be noted that, in this embodiment, a copper metal 110 is also disposed below the aluminum metal layer 400 to realize the metal interconnection of the chip. In addition, a titanium nitride layer 120 is disposed between the copper metal 110 and the aluminum metal layer 400 as a dielectric layer to realize an isolation layer between the aluminum metal and the copper metal 110. Since the copper metal 110 and the titanium nitride layer 120 are not the inventive point of this embodiment, they are not described here.

[0045] Step S2: etching the passivation layer 600 and stopping at the metal layer to form an opening 500 in the metal layer to expose the metal layer.

[0046] Specifically, refer to Figure 3 and Figure 4 As shown, a mixed gas of CF4 and CHF3 is used to etch the passivation layer 600. The etching stops at the aluminum metal layer 400, so that an opening 500 can be formed in the aluminum metal layer 400 to expose the aluminum metal so as to perform metal interconnection on the chip. The ratio of the area of ​​the opening 500 to the area of ​​the wafer 100 is less than 10%. The opening 500 can be of any shape as long as interconnection can be achieved.

[0047] Step S3: cleaning the wafer 100 with the opening 500 formed thereon.

[0048] Specifically, refer to Figure 3 and Figure 4 As shown, the wafer 100 with the opening 500 is cleaned by wet cleaning to remove the polymer on the wafer 100 and the inner wall of the opening 500. The cleaning agent of the wet cleaning can be a cleaning solution such as hydrofluoric acid, sulfuric acid, etc.

[0049] Step S4: bombarding the inner wall of the opening 500 with an inert gas on the cleaned wafer 100 .

[0050] Specifically, refer to Figure 3 and Figure 4 As shown. The inner wall of the opening 500 is physically bombarded with an inert gas. The inert gas may be nitrogen, argon, etc. Since argon is commonly used in the manufacturing process, in order to save costs, in this embodiment, the inert gas is preferably argon. Preferably, the flow rate of argon is 1000 scmm, and the pressure of argon bombarding the inner wall of the opening 500 is 500 mtorr. When argon is used to physically bombard the inner wall of the opening 500, the residual gas containing "F" can be reduced.

[0051] Furthermore, after the cleaned wafer 100 is bombarded with argon gas on the surface of the opening 500, the method for reducing wafer defects further includes: using oxygen to push the top of the opening 500 to expand the process window at the top of the opening 500. This facilitates the interconnection of the aluminum lead with other metals.

[0052] 5 and Figure 6 As shown, Figure 5 A schematic diagram of electronic scanning of wafer defects when the method for reducing wafer defects provided in this embodiment is not used. Figure 6 The method for reducing wafer defects provided by this embodiment is used, and the electronic scanning diagram of wafer defects is shown. It can be seen from the two electronic scanning diagrams that Figure 5The number of crystal defects on the wafer surface is significantly higher than Figure 6 Therefore, it can be shown that by adopting the method for reducing wafer defects provided by this embodiment, the number of crystal defects formed on the wafer 100 can be reduced, and the quality and yield of the wafer 100 can be improved.

[0053] Ginseng Figure 7 As shown, Figure 7 is a graph showing the relationship between the F content and the reduced thickness of aluminum as measured by Auger Electron Spectroscopy (AES). Figure 7 It can be seen that Figure 7 It is a relationship diagram of the tested F content and the reduced thickness of the aluminum metal layer under different conditions. In this embodiment, four different conditions are selected, and after the wafer 100 is subjected to the final passivation treatment, the F content and the reduced thickness of the aluminum metal layer are tested by Auger testing to obtain four relationship diagrams. The four corresponding conditions are: Condition 1, bombarding the inner wall of the opening 500 with argon gas and treating it with rapid thermal annealing. That is, using the method for reducing wafer defects disclosed in this embodiment, bombarding the inner wall of the opening 500 with argon gas, and then treating the wafer with a rapid thermal annealing process. Condition 2, standard 1. That is, the wafer is not passivated using the method for reducing wafer defects disclosed in this embodiment. Condition 3, bombarding the inner wall of the opening 500 with argon gas. That is, the wafer is passivated using the method for reducing wafer defects disclosed in this embodiment, but the wafer 100 is treated with a rapid thermal annealing process in Condition 1 is removed. Condition 4, standard 2. As with condition 2, the wafer was not passivated using the method for reducing wafer defects disclosed in this embodiment. It can be seen from conditions 1 and 3 that after the wafer was passivated using the method for reducing wafer defects provided in this embodiment, when the aluminum metal layer was reduced by 2.3nm, the F content was significantly reduced. When the aluminum metal layer was reduced by 4.4nm, the F content was 0. Therefore, argon gas was used to bombard the inner wall of the opening 500, and a high-energy electron beam was used as an excitation source to interact with the surface of the material after injection. After extracting the concentration data of surface F atoms and analyzing it, it was found that when the thickness of the aluminum metal layer on the surface was reduced by 2.3nm), the concentration of the F content could be reduced to a minimum, and the performance on the product was 30-50%. After adding the step of bombarding the inner wall of the opening 500 with argon gas, the source of the F element was reduced, and the generation of crystal defects was hindered to the greatest extent.

[0054] Therefore, the method for reducing wafer defects provided in this embodiment uses argon gas to bombard the inner wall of the opening 500 after etching the passivation layer 600 to reduce the concentration of the etching gas remaining on the inner wall of the opening 500, thereby avoiding chemical reactions between the etching gas, metal aluminum and air, thereby reducing the formation of crystal defects on the wafer 100, improving the quality and yield of the wafer 100. At the same time, the performance of the device is also improved.

[0055] In summary, the above embodiments provide detailed descriptions of different configurations of the method for reducing wafer defects. Of course, the above description is only a description of the preferred embodiments of the present invention, and is not any limitation to the scope of the present invention. The present invention includes but is not limited to the configurations listed in the above embodiments. Those skilled in the art can draw inferences based on the contents of the above embodiments. Any changes and modifications made by ordinary technicians in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.

Claims

1. A method for reducing wafer defects, It is characterized in that include: Providing a wafer, depositing a metal layer on the surface of the wafer, and filling a passivation layer around the metal layer; Etching the passivation layer and stopping at the metal layer to form an opening in the metal layer to expose the metal layer; cleaning the wafer formed with the opening; For the cleaned wafer, an inert gas is used to bombard the inner wall of the opening.

2. The method for reducing wafer defects according to claim 1, It is characterized in that The passivation layer includes a silicon nitride layer and a silicon oxide layer.

3. The method for reducing wafer defects according to claim 1, It is characterized in that The metal layer is an aluminum metal layer.

4. The method for reducing wafer defects according to claim 1, It is characterized in that The ratio of the area of ​​the opening to the area of ​​the wafer is less than 10%.

5. The method for reducing wafer defects according to claim 1, It is characterized in that Cleaning a wafer having an opening formed therein includes: The wafer having the opening formed therein is cleaned by wet cleaning.

6. The method for reducing wafer defects according to claim 1, It is characterized in that The inert gas is argon.

7. The method for reducing wafer defects according to claim 6, It is characterized in that The flow rate of the argon gas is 1000 scmm, and the pressure of the argon gas bombarding the inner wall of the opening is 500 mtorr.

8. The method for reducing wafer defects according to claim 1, It is characterized in that Using CF 4 and CHF 3 The mixed gas etches the passivation layer.

9. The method for reducing wafer defects according to claim 1, It is characterized in that After the cleaned wafer is bombarded with argon gas on the surface of the opening, the method for reducing wafer defects further comprises: Use oxygen to push the top of the opening to expand the process window at the top of the opening.

10. The method for reducing wafer defects according to claim 3, It is characterized in that The thickness of the metal aluminum deposition is 6 μm.