Method of forming epitaxial stack and substrate processing apparatus thereof
By performing multiple deposition cycles on the substrate at low pressure and low temperature, the Si1-xGex/Si epitaxial stacking is solved, and the device manufacturing efficiency and quality is improved.
Patent Information
- Application Number
- CN202410555407.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-05-07
- Publication Date
- 2024-11-19
AI Technical Summary
In three-dimensional transistors, especially in the manufacturing process of complementary field effect transistors (CFETs) based on vertical stacked nanosheets, it is difficult to obtain a defect-free fully strained silicon germanium-silicon epitaxial stack, resulting in the problem of channel degradation.
By performing multiple deposition cycles on the substrate, an epitaxial stack including Si1-xGex and Si epitaxial layers is formed, using a pressure value below 10 torr and a temperature below 600°C to reduce the formation of particles and defects and improve the formation of them and improve the Growth rate.
Achieves the formation of Si1-xGex/Si epitaxial stacks with reduced defects and particles at lower temperatures, suitable for the manufacture of surrounding gate field effect transistors (GAA-FETs) and complementary field effect transistors (CFETs) devices, reducing the process Risk of loss of output.
Smart Images

Figure CN118983216A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a method for forming an epitaxial stack and a substrate processing apparatus for forming an epitaxial stack. More specifically, the present disclosure relates to a method for forming a silicon / silicon germanium epitaxial stack on a substrate and a substrate processing apparatus. Background Art
[0002] Due to the continuous development of the semiconductor industry, three-dimensional transistors are considered to be the next generation devices. Among them, nanosheet field-effect transistors are considered promising because they can provide reduced leakage current and high drive current. Therefore, this may increase the attention on the manufacturing and processing of these devices.
[0003] In the three-dimensional transistor, the complementary field effect transistor (CFET) based on vertically stacked nanosheets is a transistor in which n-MOS and p-MOS devices are stacked on top of each other. This can be achieved by stacking silicon germanium epitaxial layers and silicon epitaxial layers, whereby the channel can be realized by performing a selective etching process to remove the silicon germanium layer.
[0004] One of the challenges that may be associated with the fabrication of CFETs is the ability to obtain a defect-free, fully strained SiGe-Si / Si epitaxial stack to avoid channel degradation.
[0005] Therefore, it may be desirable to provide methods that enable the formation of epitaxial layer stacks on substrates with improved layer properties. Summary of the invention
[0006] This summary is provided to introduce some concepts in a simplified form. These concepts are further described in detail in the detailed description of the exemplary embodiments of the present disclosure below. This summary is not intended to identify the key features or essential features of the claimed subject matter, nor is it intended to be used to limit the scope of the claimed subject matter.
[0007] It is an object of the present disclosure to enable the growth of epitaxial stacks on a substrate.
[0008] In a first aspect, the present disclosure relates to a method for forming an epitaxial stack. The method may include providing a substrate to a processing chamber. The method may also include performing a plurality of deposition cycles to form the epitaxial stack on the substrate. The epitaxial stack may include a plurality of first epitaxial pairs. Each first epitaxial pair may include a first epitaxial layer and a second epitaxial layer. The first epitaxial layer and the second epitaxial layer of each first epitaxial pair may include at least a first Group IV semiconductor material, and the second epitaxial layer of each first epitaxial pair may further include a second Group IV semiconductor material different from the first Group IV semiconductor material. Each of the plurality of deposition cycles may be performed at a pressure value less than 10 Torr.
[0009] The method according to the embodiment of the first aspect of the present disclosure may allow the formation of an epitaxial stack. It may advantageously allow the formation of a stack comprising Si 1-x Ge x and an epitaxial stack of Si epitaxial layers.
[0010] Another advantage of embodiments of the first aspect is that Si with reduced defects can be obtained. 1-x Ge x The epitaxial stack of Si and Si epitaxial layers. Such epitaxial stack can be advantageously suitable for manufacturing a gate-all-around field effect transistor (GAA-FET) device. In particular, such epitaxial stack can be advantageous for manufacturing a complementary field effect transistor (CFET) device.
[0011] An advantage of the embodiments of the first aspect is that Si can be formed at a relatively low process temperature (e.g., below 600° C.). 1- x Ge x Fully strained epitaxial stack of Si / Si epitaxial layers.
[0012] Another advantage of embodiments of the first aspect is that particle formation during formation of the epitaxial stack may be reduced.
[0013] It is also an advantage of embodiments of the first aspect that defect formation during formation of the epitaxial stack, such as misfit dislocation defects, may be reduced.
[0014] Another advantage of the embodiments of the first aspect is that Si can be achieved at lower process temperatures (e.g., below 600° C.) 1-x Ge x / Enhanced growth rate of Si epitaxial layer.
[0015] Another advantage of the embodiments of the first aspect is that due to Si 1-x Ge x The growth rate of the / Si epitaxial layer is increased at lower process temperatures, reducing the risk of process yield loss.
[0016] In a second aspect, the present disclosure relates to a substrate processing device. The substrate processing device may be suitable for forming an epitaxial stack. The substrate processing device may include a processing chamber constructed and arranged to hold a substrate. The device may include a silicon precursor storage module. The silicon precursor storage module may include a Si-containing precursor. The device may further include a germanium precursor storage module. The germanium precursor storage module may include a Ge-containing precursor. The device may also include a heater and a pressure controller, the heater may be configured to obtain a process temperature in the processing chamber, and the pressure controller may be configured to obtain a process pressure in the processing chamber. The device may further include a controller. The controller may be connected to the silicon precursor storage module and the germanium precursor storage module. The controller may be configured to execute instructions stored in a non-transitory computer-readable medium so that the substrate processing device forms an epitaxial stack in a substrate according to a method according to an embodiment of the first aspect of the present disclosure.
[0017] The substrate processing apparatus according to the embodiment of the second aspect of the present disclosure may allow the growth of an epitaxial stack on a substrate. It may particularly allow the growth of a fully strained Si substrate. 1-x Ge x / Si epitaxial stack.
[0018] An advantage of embodiments of the second aspect is that the risk of process yield loss at lower process temperatures (eg below 600° C.) may be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] It should be understood that the elements in the drawings are shown for simplicity and clarity and are not necessarily drawn to scale. For example, the sizes of some elements in the drawings may be exaggerated relative to other elements to help improve the understanding of the illustrated embodiments of the present disclosure.
[0020] Unless otherwise stated, the same reference numerals in the drawings will be used for the same elements. Reference numerals in the claims shall not be construed as limiting the scope.
[0021] Figure 1a is a flowchart of an exemplary method according to an embodiment of the first aspect of the present disclosure.
[0022] Figure 1b is a flow chart of an embodiment according to the first aspect of the present disclosure.
[0023] Figure 2a and Figure 2b is a schematic diagram of an epitaxial stack according to an embodiment of the first aspect of the present disclosure.
[0024] Figure 3a Si is deposited on a Si(100) surface at a chamber pressure of 40 Torr. 1-x Ge x Top view SEM image of the epitaxial layer obtained, where 20slm of N2 Flow rate as carrier gas, GeH 4 The flow rate is 800sccm, Si 2 H 6 The flow rates are (1) 30 sccm, (b) 40 sccm, (3) 80 sccm and (4) 120 sccm.
[0025] Figure 3b Si is deposited on a Si(100) surface at a process chamber pressure of 3 Torr. 1-x Ge x Top-down scanning electron microscope (SEM) image obtained after epitaxial layer growth, where 10slm N 2 Flow rate as carrier gas, SiH 4 The flow rate is 40sccm, GeH 4 The flow rates are (1) 200 sccm, (b) 400 sccm, (3) 800 sccm and (4) 160 sccm.
[0026] Figure 4a is a light scattering image of a disilane flow rate of 600 sccm.
[0027] Figure 4b is a light scattering image of a disilane flow rate of 100 sccm.
[0028] Figure 5 YesSi 1-x Ge x High-resolution X-ray diffraction (HR-XRD) pattern of Si / Si epitaxial stack, in which Si 1-x Ge x The epitaxial layers have different Ge atomic percentage concentrations, such as 20% and 40%.
[0029] Figure 6 is a schematic diagram of a substrate processing device according to an embodiment of the second aspect of the present disclosure. DETAILED DESCRIPTION
[0030] Although certain embodiments and examples are disclosed below, it will be appreciated by those skilled in the art that the present invention extends beyond the specifically disclosed embodiments and / or uses of the present invention and their obvious modifications and equivalents. Therefore, it is intended that the scope of the disclosed invention should not be limited by the specifically disclosed embodiments described below.
[0031] As used herein, the term "substrate" may refer to any one or more underlying materials, including any one or more underlying materials that may be modified or on which a device, circuit, or film may be formed. A "substrate" may be continuous or non-continuous; rigid or flexible; solid or porous; and combinations thereof. A substrate may be in any form, such as a powder, a plate, or a workpiece. A plate-like substrate may include wafers of various shapes and sizes. A substrate may be made of semiconductor materials, including, for example, silicon, silicon germanium, silicon oxide, gallium arsenide, gallium nitride, and silicon carbide.
[0032] For example, a substrate in powder form can be used in drug manufacturing. The porous substrate can include a polymer. Examples of workpieces can include medical devices (such as stents and syringes), jewelry, tool equipment, components for battery manufacturing (such as anodes, cathodes, or separators), or components of photovoltaic cells, etc.
[0033] The continuous substrate may extend beyond the boundaries of the processing chamber in which the deposition process occurs. In some processes, the continuous substrate may be moved through the process chamber so that the process continues until the end of the substrate is reached. The continuous substrate may be provided by a continuous substrate feeding system to allow the continuous substrate to be manufactured and output in any suitable form.
[0034] Non-limiting examples of continuous substrates may include sheets, nonwoven films, rolls, foils, meshes, flexible materials, bundles of continuous filaments or fibers (eg, ceramic fibers or polymer fibers). A continuous substrate may also include a carrier or sheet on which a non-continuous substrate is mounted.
[0035] The illustrations presented herein are not intended to be actual views of any particular material, structure, or device but are merely idealized representations used to describe embodiments of the present disclosure.
[0036] The specific embodiments shown and described are illustrations of the present invention and its best mode and are not intended to limit the scope of these aspects and embodiments in any way. In fact, for the sake of brevity, the traditional manufacturing, connection, preparation and other functional aspects of the system may not be described in detail. In addition, the connecting lines shown in the various figures are intended to represent exemplary functional relationships and / or physical connections between various elements. Many alternative or additional functional relationships or physical connections may exist in actual systems, and / or may not exist in some embodiments.
[0037] It should be understood that the configurations and / or methods described herein are exemplary in nature, and these specific embodiments or examples should not be considered restrictive, as many variations are possible. The specific routines or methods described herein may represent one or more of any number of processing strategies. Therefore, the various actions shown may be performed in the order shown, in other orders, or may be omitted in some cases.
[0038] The subject matter of the present disclosure includes all novel and nonobvious combinations and subcombinations of the various processes, systems and configurations, and other features, functions, acts and / or properties disclosed herein, and any and all equivalents thereof.
[0039] It should be noted that the term "comprising" used herein should not be interpreted as being limited to the means listed thereafter. It does not exclude other elements or steps. Therefore, it should be interpreted as specifying the presence of the features, steps or components mentioned. However, this does not prevent the presence or addition of one or more other steps, components or features or combinations thereof.
[0040] References to "embodiments" throughout the specification do not necessarily refer to the same embodiment, but may. In addition, in one or more embodiments, the particular features, structures, or characteristics may be combined in any suitable manner, which is apparent to those skilled in the art.
[0041] References to "some embodiments" throughout the specification mean that the specific structures, features, and steps described in conjunction with these embodiments are included in some embodiments of the present invention. Therefore, phrases such as "in some embodiments" appearing in different places throughout the specification do not necessarily refer to the same set of embodiments, but may refer to the same set of embodiments.
[0042] References throughout this specification to "one embodiment" or "an embodiment" mean that a particular feature, structure, or characteristic described in conjunction with the embodiment is included in at least one embodiment of the present disclosure. Therefore, the phrases "in one embodiment" or "in an embodiment" appearing in various places in this specification do not necessarily all refer to the same embodiment, but may refer to the same embodiment.
[0043] It should be noted that the term "essentially comprising" used in the claims means that in addition to those specifically mentioned components, other components may be present but are not required to be present, that is, those components that do not substantially affect the basic characteristics of the material, compound or composition involved.
[0044] The terms first, second, third, etc. in the specification and claims are used to distinguish similar elements. They are not necessarily used to describe a sequence in time, space, order, or any other manner. It should be understood that the terms so used are interchangeable where appropriate, and that the embodiments of the present disclosure described herein are capable of operating in other sequences than those described or shown herein.
[0045] The following terms are used only to aid in understanding the present disclosure.
[0046] As used herein, unless otherwise indicated, the term "purge gas" may refer to a gas provided to a processing chamber before and after a deposition pulse.
[0047] As used herein, unless otherwise specified, the term “misfit dislocation density” may refer to the number of misfit dislocations per unit area.
[0048] As used herein, unless otherwise specified, the term "epitaxial pair" may refer to a subset of epitaxial layers within an epitaxial stack, having two epitaxial layers that are different from each other.
[0049] As used herein, unless otherwise specified, the term "epitaxial stack" may refer to an entirety formed having at least nine pairs of epitaxial pairs.
[0050] As used herein, unless otherwise specified, the term "fully strained" may refer to an in-plane lattice parameter that matches the lattice parameter of an underlying layer or substrate.
[0051] As used herein, unless otherwise specified, the term "Si 1-x Ge x ” may refer to a silicon germanium epitaxial layer, where x may be in the range of 10 atomic % to 50 atomic %.
[0052] The present disclosure will now be described by a detailed description of a plurality of embodiments of the present disclosure. It is apparent that other embodiments of the present disclosure may be configured according to the knowledge of those skilled in the art without departing from the technical teachings of the present disclosure. The present disclosure is limited only by the terms of the claims included herein.
[0053] Figure 1a A flowchart of an exemplary method according to an embodiment of the first aspect of the present disclosure is shown. Figure 2a A schematic diagram showing an epitaxial stack according to an embodiment of the first aspect of the present invention is shown.
[0054] A method of forming an epitaxial stack 200 is described herein.
[0055] The method 100 may include providing 110 a substrate 210 to a process chamber. The process chamber may be included in a semiconductor processing device. The semiconductor processing device may be suitable for growing an epitaxial layer.
[0056] In some embodiments, the process chamber may be one of at least two process chambers included in a semiconductor processing apparatus.
[0057] In some embodiments, the process chamber may be a single process chamber contained in a semiconductor processing apparatus.
[0058] The method according to the embodiment of the first aspect may be run in a single chamber; however, the same method may be run simultaneously in more than one processing chamber of a semiconductor processing apparatus.
[0059] The method 100 may further include performing 120 more deposition cycles 130 to form an epitaxial stack 200 on the substrate.
[0060] The epitaxial stack 200 may include a plurality of first epitaxial pairs 201. Each first epitaxial pair 201 may include a first epitaxial layer 201a and a second epitaxial layer 201b. The first epitaxial layer 201a and the second epitaxial layer 201b of each first epitaxial pair 201 may include at least a first Group IV semiconductor material. The second epitaxial layer 201b of each first epitaxial pair 201 may further include a second Group IV semiconductor material different from the first Group IV semiconductor material. Each of the plurality of deposition cycles 130 may be performed at a pressure value less than 10 Torr.
[0061] In an embodiment, each of the plurality of deposition cycles 130 may be performed at a pressure value in a range from about 0.1 Torr to about 10 Torr.
[0062] In an embodiment, each of the plurality of deposition cycles 130 may be performed at a pressure value in a range from about 1 Torr to about 5 Torr.
[0063] The method according to an embodiment of the first aspect may allow the formation of an epitaxial stack 200 that may include different epitaxial layers 201a, 201b. Due to the reduced pressure in the processing chamber during the growth of the epitaxial stack 200, reduced particle formation and reduced defect formation can be achieved. This may be further advantageous for using such an epitaxial stack in the manufacture of a GAA-FET device, particularly when the channel is in the form of a thin sheet, such as a nanosheet FET or a CFET. This may be due to the presence of particles and / or defects in the epitaxial stack that may adversely affect device characteristics, such as leakage current, threshold voltage. The presence of particles may also have an impact on subsequent processing steps, such as deposition, lithography, and etching. When these particles and / or defects are formed, particularly when they are formed in the layers of the epitaxial stack 200, this may be critical, and the epitaxial stack will subsequently become the channel of such a device. Therefore, the formation of particles and / or defects in the epitaxial stack and the reduction of their presence may make the use of such an epitaxial stack 200 conducive to the manufacture of such a device.
[0064] In some embodiments, each of the plurality of deposition cycles 130 may be performed at a pressure value of about 3 Torr, with a pressure variation of + / - 1 Torr.
[0065] In an embodiment, each deposition cycle 130 of the plurality of deposition cycles may include a first deposition pulse 131 and a second deposition pulse 132 .
[0066] The first deposition pulse 131 may include providing a first Group IV semiconductor material precursor gas. In this manner, a first epitaxial layer 201a may be formed. The second deposition pulse 132 may include providing a first Group IV semiconductor material precursor gas, and may also include providing a second Group IV semiconductor material precursor gas. In this manner, a second epitaxial layer 201b may be formed. The second Group IV semiconductor material precursor gas may be different from the first Group IV semiconductor material precursor gas.
[0067] Thus, each deposition cycle 130 in the plurality of deposition cycles may form each first epitaxial pair 201 of the epitaxial stack 200. Thus, multiple repetitions of each deposition cycle 103 may result in the formation of the epitaxial stack 200. In other words, the epitaxial stack 200 may look like an epitaxial stack having alternating layers of first epitaxial layers 201a and second epitaxial layers 201b. The number of times each deposition cycle may be repeated may depend on the final thickness of the epitaxial stack 200 to be obtained.
[0068] In an embodiment, the formation order of the first epitaxial layer 201a and the second epitaxial layer 201b may be different depending on the substrate. Therefore, in some embodiments, although the first epitaxial layer 201a may be formed on the substrate, in some embodiments, the second epitaxial layer 201b may be formed on the substrate.
[0069] In some embodiments, the first epitaxial layer 201 a may be formed directly on the substrate, and in some embodiments, the second epitaxial layer 201 b may be formed directly on the substrate, as schematically shown in FIG. 2 .
[0070] In some embodiments, during each deposition cycle 130, the first Group IV semiconductor material precursor gas may be provided to the process chamber in a continuous flow, and the second Group IV semiconductor material precursor gas may be provided to the process chamber intermittently.
[0071] In other words, providing the first Group IV semiconductor material precursor gas in a continuous flow means providing the first Group IV semiconductor material precursor gas during the first deposition pulse 131 and during the second deposition pulse 132. Therefore, in other words, the intermittent supply of the second Group IV semiconductor material precursor gas may mean providing it only during the second deposition pulse 132.
[0072] This may provide an advantage of reducing the number of purge pulses when switching between the formation of the first epitaxial layer 201 a and the second epitaxial layer 201 b .
[0073] In an embodiment, the first Group IV semiconductor material precursor gas that may be included in the first deposition pulse 131 for forming the first epitaxial layer 201a may substantially include the second Si-containing precursor gas, and the second Group IV semiconductor material precursor gas that may be further included in the second deposition pulse 132 may substantially include the Ge-containing precursor gas in addition to the first Group IV semiconductor material precursor gas for forming the second epitaxial layer 201b. In this way, the first epitaxial layer 201a including Si and the second epitaxial layer 201b may be formed. 1-x Ge x The first epitaxial pair of the second epitaxial layer 201b.
[0074] The first epitaxial layer 201a includes Si and the epitaxial layer 201a includes Si. 1-x Ge x The formation of such an epitaxial stack 200 of the second epitaxial layer 201b of the epitaxial pair may be advantageous in the manufacture of a GAA-FET device, especially when the channel is in the form of a thin sheet, such as a nanosheet FET or a CFET. 1-x Ge x After the epitaxial layer, the Si epitaxial layer can form the channel of the p-MOS device and n-MOS device of the FET.
[0075] In an embodiment, the second Si-containing precursor gas may be silane and the Ge-containing precursor gas may be germane. This may advantageously allow for an increased growth rate of the epitaxial layer at process temperatures below 600°C.
[0076] In some embodiments, the second Si-containing precursor gas may be a higher-order silane. Thus, in some embodiments, the second Si-containing precursor gas may be, for example, disilane or trisilane.
[0077] In some embodiments, the second Si-containing precursor gas may be disilane, and the Ge-containing precursor gas may be monogermane.
[0078] Back to Figure 3a and Figure 3b , showing Si grown on a Si(100) substrate 1-x Ge x Comparison of the surface of the epitaxial layer as a function of different process parameters, where the process temperature is set to 490°C, where x represents the Ge concentration between 15 atomic % and 40 atomic %.
[0079] from Figure 3a It was observed that when the process pressure was set to 40 Torr, Si 1-x Ge x The surface is subject to particle formation. When GeH 4 When the flow rate is fixed at 800sccm, Si 2 H6 The increase in flow rate between 30 sccm and 120 sccm (from image 1 to image 4 to the left) appears to reduce particle formation, but does not reduce the size of the epitaxial Si 1-x Ge x The particles are completely removed from the layer. In images 3 and 4, Si 1- x Ge x The Ge concentrations in the layers are 34.6 atomic % and 29 atomic %, respectively.
[0080] exist Figure 3b It was observed that when the process pressure was set to 3 Torr, Si 1-x Ge x There are no particles on the surface of the epitaxial layer. SiH 4 The flow rate was set to 40 sccm, and the GeH 4 The flow rate varies from 200 sccm to 1600 sccm (from image 1 to image 4 to the left). From image 1 to image 4, Si 1-x Ge x The Ge concentration in the layer is 15.3 atomic %, 21.7 atomic %, 32.1 atomic % and 40 atomic %.
[0081] Without wishing to be bound by theory, it can be stated that when the pressure is maintained in the range of 20 torr to 40 torr, the formation of particles may occur due to gas phase reactions occurring typically in the temperature range of 450° C. to 600° C. to obtain a multilayer Si layer alternating with Si epitaxial layers. 1-x Ge x Epitaxial Si 1-x Ge x As the pressure decreases, the opportunity for this gas phase reaction to occur may decrease, thereby advantageously reducing particle formation.
[0082] Another advantage of the embodiments of the first aspect is that Si can be formed at a relatively low process temperature (e.g., below 600° C.). 1-x Ge x A fully strained epitaxial stack of Si / Si epitaxial layers. Having a fully strained epitaxial stack may provide the advantage of reducing the risk of dislocations. This may advantageously reduce dislocation density.
[0083] In an embodiment, the second Si-containing precursor gas can be provided to the process chamber at a flow rate in the range of 30 sccm to 600 sccm, and the Ge-containing precursor gas can be provided to the process chamber at a flow rate in the range of 100 sccm to 1600 sccm. The flow rate ranges of the second Si-containing precursor gas disclosed herein are applicable during both the first deposition pulse 131 and the second deposition pulse 132.
[0084] In an embodiment, the flow rate of the second Si-containing precursor gas can be at least 30 sccm to at most 100 sccm, or at least 100 sccm to at most 150 sccm, or at least 150 sccm to at most 200 sccm, or at least 200 sccm to at most 250 sccm, or at least 250 sccm to at most 300 sccm, or at least 300 sccm to at most 350 sccm, or at least 350 sccm to at most 400 sccm, or at least 400 sccm to at most 450 sccm, or at least 450 sccm to at most 500 sccm, or at least 500 sccm to at most 550 sccm, or at least 550 sccm to at most 600 sccm.
[0085] In an embodiment, the flow rate of the Ge-containing precursor gas may be at least 100 sccm to at most 200 sccm, or at least 200 sccm to at most 300 sccm, or at least 300 sccm to at most 400 sccm, or at least 400 sccm to at most 500 sccm, or at least 500 sccm to at most 600 sccm, or at least 600 sccm to at most 700 sccm, or at least 700 sccm to at most 800 sccm, or at least 800 sccm. sccm to at most 900 sccm or at least 900 sccm to at most 1000 sccm or at least 1000 sccm to at most 1100 sccm or at least 1100 sccm to at most 1200 sccm or at least 1200 sccm to at most 1300 sccm or at least 1300 sccm to at most 1400 sccm or at least 1400 sccm to at most 1500 sccm or at least 1500 sccm to at most 1600 sccm.
[0086] It should be noted that the flow rate of the Ge-containing precursor gas may vary depending on the type of Ge-containing precursor. In some embodiments, the Ge-containing precursor may be a higher order germane, such as digermane, and the flow rate may be in the range of 5 sccm to 10 sccm.
[0087] In embodiments, the second Si-containing precursor gas may be provided at a flow rate in the range of 30 sccm to 100 sccm during the first deposition pulse 131 and in the range of 50 sccm to 100 sccm during the second deposition pulse 132. In these embodiments, the second Si-containing precursor gas may be disilane.
[0088] In some embodiments, the flow rate of the second Si-containing precursor gas may be at least 30 sccm to at most 40 sccm or at least 40 sccm to at most 50 sccm or at least 50 sccm to at most 60 sccm or at least 60 sccm to at most 70 sccm or at least 70 sccm to at most 80 sccm or at least 80 sccm to at most 90 sccm or at least 90 sccm to at most 100 sccm.
[0089] In embodiments, adjusting the disilane flow rate may provide the advantage of further reducing particle formation.
[0090] Back to Figure 4a and Figure 4b , showing a comparison of light scattering images of the Si surface of the epitaxial stack.
[0091] From the comparison of the images, it is observed that when the disilane flow rate used to form the epitaxial layer is reduced from 600 sccm to 100 sccm, the presence of particles on the surface has decreased. Therefore, adjusting the flow rate of the second Si-containing precursor gas can advantageously allow control of particle formation on the surface of the formed epitaxial layer.
[0092] However, in some embodiments, a purge pulse may be provided to the process chamber between the formation of the respective epitaxial layers, i.e., between the formation of the first epitaxial layer 201a and the second epitaxial layer 201b and between the second epitaxial layer and the first epitaxial layer of the epitaxial stack 200. Therefore, in these embodiments, the intermittent supply of the second Group IV semiconductor material precursor gas is not performed.
[0093] Therefore, in some embodiments, each deposition cycle 130 may further include a purge pulse. The purge pulse may include providing a first Si-containing precursor gas and providing a hydrogen halide gas.
[0094] In an embodiment, the provision of the purge pulse 133 may be performed for a predetermined duration before and after each deposition pulse 131, 132. Thus, the first Si-containing precursor gas and the hydrogen halide gas may be provided before the first deposition pulse 131, after the first deposition pulse 131, and after the second deposition pulse 132 of each deposition cycle 130. This may result in the purge pulse 133 being performed between the formation of each individual epitaxial layer included in the epitaxial stack 200, such as Figure 1b As shown schematically in FIG.
[0095] In an embodiment, the provision of the first Si-containing precursor gas and the provision of the hydrogen halide gas may be completed during an overlapping period. In other words, the first Si-containing precursor gas flow and the hydrogen halide precursor gas flow may overlap each other during a predetermined period in the purge pulse. Therefore, in an embodiment, there may be a period during which the first Si-containing precursor gas and the hydrogen halide precursor gas are simultaneously provided to the process chamber.
[0096] In some embodiments, the first Si-containing precursor gas may be provided substantially simultaneously with the provision of the hydrogen halide gas. In other words, the first Si-containing precursor gas may co-flow with the hydrogen halide gas to the process chamber. In other words, the first Si-containing precursor gas may be provided to the process chamber together with the hydrogen halide gas, such that the provision of the first Si-containing precursor gas and the provision of the hydrogen halide gas to the process chamber begin and end substantially simultaneously.
[0097] As disclosed herein, co-flowing the first Si-containing precursor gas with the hydrogen halide gas can provide the advantage of obtaining a sharper interface between different epitaxial layers, i.e., between the first epitaxial layer 201a and the second epitaxial layer 201b of the epitaxial stack 200. Co-flowing can particularly provide the advantage of reducing or substantially eliminating the misfit dislocation density that can be observed when growing the epitaxial stack 200, particularly the epitaxial stack 200 disclosed herein.
[0098] In an embodiment, the first Si-containing precursor gas and the hydrogen halide gas may include chlorine. The presence of chlorine may allow for sharper interfaces between epitaxial layers during formation of the epitaxial layers in the epitaxial stack.
[0099] In an embodiment, the first Si-containing precursor gas may be chlorosilane.
[0100] In some embodiments, the chlorosilane may be dichlorosilane (DCS).
[0101] In some embodiments, the purge pulse may thus include providing DCS and hydrogen chloride gas (HCl).
[0102] In some embodiments, dichlorosilane may be included in the provision of the purge gas during an overlapping period with the hydrogen chloride.
[0103] In some embodiments, the purge gas may include dichlorosilane co-flowing with hydrogen chloride.
[0104] In an embodiment, the ratio of the flow rate of the first Si-containing precursor gas to the flow rate of the hydrogen halide gas may be about 1:1.
[0105] It is noted that the flow ratio between the two precursors can be varied as long as a passivation effect rather than deposition is observed on the surface.
[0106] In an embodiment, the flow rate of the first Si-containing precursor gas and the flow rate of the hydrogen halide gas may be about 300 sccm.
[0107] In an embodiment, the predetermined duration of providing the purge gas to the process chamber may be approximately 5 seconds.
[0108] Now back to Figure 2b , Figure 2b A schematic diagram of an epitaxial stack according to an embodiment of the first aspect of the present disclosure is shown.
[0109] In an embodiment, the epitaxial stack 300 may further include a second epitaxial pair 301. The second epitaxial pair 301 may be different from the first epitaxial pair 201. The epitaxial stack 300 may be formed on the substrate 210 with at least one second epitaxial pair 301 between two adjacent first epitaxial pairs 201. This may provide the advantage of achieving selective etching between different layers of different epitaxial pairs of the epitaxial stack.
[0110] In an embodiment, the second epitaxial pair 301 may include a first epitaxial layer 201a and a third epitaxial layer 301b. The third epitaxial layer may include at least a first Group IV semiconductor material. The third epitaxial layer 301b may further include a second Group IV semiconductor material. The plurality of first epitaxial pairs 201 may have a first concentration of the second Group IV semiconductor material, and the third epitaxial layer 301b may have a second concentration of the second Group IV semiconductor material. The second concentration may be different from the first concentration.
[0111] The concentration difference of the second Group IV semiconductor material included in the second epitaxial layer 201 b and the third epitaxial layer 301 b may provide an advantage of being able to selectively remove one of the second epitaxial layer 201 b or the third epitaxial layer 301 b from the other.
[0112] In an embodiment, the epitaxial stack 300 may be formed in such a manner that each second epitaxial layer 201 b and each third epitaxial layer 301 b are separated from each other by the first epitaxial layer 201 a. Figure 2b As shown schematically in FIG.
[0113] In an embodiment, the second epitaxial layer 201b and the third epitaxial layer 301b may be respectively referred to as sacrificial layers of the first epitaxial pair 201 and the second epitaxial pair 301. In other words, at least one of the second epitaxial layer 201b and the third epitaxial layer 301b may be removed from the epitaxial stack 200, 300 in one of the processing steps after the epitaxial stack is formed.
[0114] In an embodiment, the second concentration may be higher than the first concentration. This may allow selective removal of the third epitaxial layer relative to the second epitaxial layer.
[0115] In an embodiment, the first concentration of the second Group IV semiconductor material can be in a range of about 10 atomic % to 25 atomic %. The second concentration of the second Group IV semiconductor material can be in a range of about 30 atomic % to about 45 atomic %. It should be noted that the values of the first concentration and the second concentration can vary within a given concentration range. This can allow for adjustment of the etch selectivity when removing the third epitaxial layer relative to the second epitaxial layer.
[0116] Therefore, in an embodiment, the first epitaxial layer 201a of the first epitaxial pair 201 may be a Si epitaxial layer, and the second epitaxial layer 201b of the first epitaxial pair 201 may be a Si epitaxial layer having a first concentration. 1-x Ge x The first epitaxial layer 201a of the second epitaxial pair 301 may be a Si epitaxial layer, and the third epitaxial layer 301b of the second epitaxial pair 301 may be a Si epitaxial layer having a second concentration. 1- x Ge x Epitaxial layer.
[0117] Figure 5 shows Si with different Ge concentrations 1-x Ge x Epitaxial Si 1-x Ge x High-resolution X-ray diffraction (HR-XRD) patterns of the epitaxial stack 200. 1-x Ge x The epitaxial layers have different Ge concentrations of 20 atomic % or 40 atomic %. Figure 5 The peak shape and peak intensity show that the epitaxial stack is not completely relaxed.
[0118] In an embodiment, the thickness of each epitaxial layer 201a, 201b, 301b may be the same or may be different from each other. The thickness of each epitaxial layer may be customized according to the final use of the epitaxial stack 200, 300. The total thickness of the epitaxial stack 200, 300 may be a function of at least one of the total number of epitaxial pairs 201, 301 and the thickness of each epitaxial layer 201a, 201b, 301b.
[0119] In an embodiment, each of the plurality of deposition cycles 130 may be performed at a temperature in the range of 450°C to 600°C. This may provide the advantage of being able to grow an epitaxial stack at a lower process temperature, as disclosed herein. Thus, it may allow an epitaxial stack having a reduced risk of strain relaxation to be obtained. When the epitaxial stack is used to manufacture a semiconductor device, as disclosed herein, the reduced risk of strain relaxation may provide the advantage of obtaining improved device characteristics, such as leakage current and threshold voltage. Furthermore, this may advantageously allow keeping up with advanced CMOS (complementary metal oxide semiconductor) processing, as epitaxial growth at lower process temperatures may become critical.
[0120] In an embodiment, each of the plurality of deposition cycles 130 may be performed within a temperature range of at least 450°C to at most 475°C, or at least 475°C to at most 500°C, or at least 500°C to at most 525°C, or at least 525°C to at most 550°C, or at least 550°C to at most 575°C, or at least 575°C to at most 600°C.
[0121] In an embodiment, the precursor disclosed herein may be provided in the presence of a carrier gas. In other words, the first deposition pulse 131, the second deposition pulse 132, and the purge pulse 133 may further include providing a carrier gas. In an embodiment, the carrier gas may include H 2 or N 2 and rare gases such as Ar, Ne, He, Xe, and Kr.
[0122] In some embodiments, the carrier gas may consist primarily of N 2 , Ar, He or a combination thereof.
[0123] In some embodiments, the carrier gas may consist primarily of H 2 , Ar, He or a combination thereof.
[0124] A method of forming the epitaxial stack 200, 300 is also described herein.
[0125] The method may include providing a substrate to a processing chamber. The processing chamber may be included in a semiconductor processing device. The semiconductor processing device may be suitable for growing an epitaxial layer.
[0126] In some embodiments, the process chamber may be one of at least two process chambers included in a semiconductor processing apparatus.
[0127] In some embodiments, the process chamber may be a single process chamber contained in a semiconductor processing apparatus.
[0128] The method according to the embodiment of the first aspect may be run in a single chamber; however, the same method may be run simultaneously in more than one processing chamber of a semiconductor processing apparatus.
[0129] The method may further include performing a plurality of deposition cycles to form an epitaxial stack on the substrate.
[0130] The epitaxial stack may include a plurality of first epitaxial pairs. Each first epitaxial pair may include a first epitaxial layer and a second epitaxial layer. The first epitaxial layer and the second epitaxial layer of each first epitaxial pair may include at least a first Group IV semiconductor material. The second epitaxial layer of each first epitaxial pair may also include a second Group IV semiconductor material different from the first semiconductor Group IV semiconductor material. Each deposition cycle of the plurality of deposition cycles may include a first deposition pulse and a second deposition pulse, wherein each deposition cycle may also include a purge pulse before and after each deposition pulse, and the purge pulse may include providing a first Si-containing precursor gas and providing a hydrogen halide gas.
[0131] The first deposition pulse, the second deposition pulse, and the purge pulse may be performed as disclosed herein according to the embodiments of the first aspect of the present disclosure.
[0132] The method is advantageous in reducing the misfit dislocation density in an epitaxial film formed on a substrate. In addition, the method can advantageously allow for the creation of sharp interfaces between epitaxial layers of an epitaxial stack.
[0133] In an embodiment, the processing temperature may be in the range of 450°C to 600°C.
[0134] Here it is further described as Figure 6 A substrate processing device is schematically shown in FIG.
[0135] The substrate processing apparatus 1000 may be suitable for forming an epitaxial stack.
[0136] The substrate processing apparatus 1000 may include a processing chamber 1010, which may be constructed and arranged to hold a substrate. The apparatus 1000 may also include a silicon precursor storage module 1040 and a germanium precursor storage module 1050. The silicon precursor storage module may include a Si-containing precursor, and the germanium precursor storage module may include a Ge-containing precursor. In an embodiment, the number of silicon precursor storage modules 1040 or the number of germanium precursor storage modules 1050 may be increased according to the number of different Si-containing or Ge-containing precursors used in the formation of the epitaxial stack.
[0137] The apparatus 1000 may further include a heater 1020 , which may be configured to obtain a process temperature in the processing chamber 1010 .
[0138] In some embodiments, the process temperature in the processing chamber 1010 may be measured by a pyrometer. The pyrometer may be suspended in the processing chamber 1010 above the substrate.
[0139] In some embodiments, the process temperature may be measured using a thermocouple. The thermocouple may be located below a support (e.g., a susceptor) that supports the substrate in the process chamber 1010 during the process. It should be noted that the substrate temperature measured by a pyrometer suspended above the substrate in the process chamber 1010 and the substrate temperature measured using a thermocouple may be different from each other, especially at low process temperatures, such as below 600° C., especially below 500° C.
[0140] It may also include a pressure controller 1030 , which may be configured to obtain a process pressure in the processing chamber 1010 .
[0141] The apparatus may further include a controller 1060. The controller 1060 may be operably connected to the silicon precursor storage module 1040 and the germanium precursor storage module 1050. According to an embodiment of the first aspect of the present disclosure, the controller may be configured to execute instructions stored in a non-transitory computer-readable medium to enable the substrate processing apparatus 1000 to form an epitaxial stack on a substrate.
[0142] The substrate processing apparatus 1000 can provide advantages for growing epitaxial stacks on substrates. In particular, fully strained Si on substrates can be obtained. 1-x Ge x / Si epitaxial stack growth, where x represents the Ge concentration between 10 atomic % and 50 atomic %.
[0143] Substrate processing apparatus 1000 can advantageously allow growth of epitaxial stacks while reducing the risk of process yield loss. This can be achieved with apparatus 1000, particularly at lower process temperatures, such as below 600° C. Thus, apparatus 1000 can help reduce manufacturing costs for advanced CMOS manufacturing.
[0144] The embodiments of the present disclosure do not limit the scope of the present invention, because these embodiments are defined by the claims attached hereto and their legal equivalents. Any equivalent embodiments are within the scope of the present invention. In addition to the content disclosed herein, modifications different from each other of the present disclosure will be apparent to those skilled in the art. Such modifications and embodiments derived therefrom are also intended to fall within the scope of the claims attached hereto.
Claims
1. A method for forming an epitaxial stack, the method comprising: include: - providing a substrate to a process chamber, - performing a plurality of deposition cycles to form an epitaxial stack on the substrate, the epitaxial stack comprising a plurality of first epitaxial pairs, wherein each first epitaxial pair comprises a first epitaxial layer and a second epitaxial layer, wherein the first epitaxial layer and the second epitaxial layer of each first epitaxial pair comprise at least a first Group IV semiconductor material, and the second epitaxial layer of each first epitaxial pair further comprises a second Group IV semiconductor material different from the first Group IV semiconductor material, Each of the plurality of deposition cycles is performed at a pressure value less than 10 Torr.
2. The method according to claim 1, in, Each of the plurality of deposition cycles is performed at a pressure value in a range from about 1 Torr to about 5 Torr.
3. The method according to claim 1 or 2, in, Each deposition cycle of the plurality of deposition cycles comprises: - a first deposition pulse comprising providing a first Group IV semiconductor material precursor gas to form a first epitaxial layer; and - a second deposition pulse comprising providing the first Group IV semiconductor material precursor gas and further comprising providing a second Group IV semiconductor material precursor gas, thereby forming a second epitaxial layer, wherein the second Group IV semiconductor material precursor gas is different from the first Group IV semiconductor material precursor gas.
4. The method according to any one of claims 1 to 3, in, Each deposition cycle also includes a purge pulse including providing a first Si-containing precursor gas and providing a hydrogen halide gas.
5. The method according to claim 4, in, Purge pulses are performed for a predetermined duration before and after each deposition.
6. The method according to claim 4, in, The providing of the first Si-containing precursor gas and the providing of the hydrogen halide gas are completed during an overlapping period.
7. The method according to any one of claims 4 to 6, in, The first Si-containing precursor gas and the hydrogen halide gas contain chlorine.
8. The method according to any one of claims 4 to 7, in, The first Si-containing precursor gas is chlorosilane.
9. The method according to any one of claims 4 to 8, in, The first Si-containing precursor gas is dichlorosilane, and the hydrogen halide gas is hydrogen chloride.
10. The method according to any one of claims 4 to 9, in, The ratio of the flow rate of the first Si-containing precursor gas to the flow rate of the hydrogen halide gas is about 1:
1.
11. The method according to any one of claims 4 to 10, in, The flow rates of the first Si-containing precursor gas and the hydrogen halide gas are about 300 sccm.
12. The method according to any one of claims 5 to 11, in, The predetermined duration is approximately 5 seconds.
13. The method according to claim 3, in, During each deposition cycle, the first Group IV semiconductor material precursor gas is provided as a continuous flow, and wherein the second Group IV semiconductor material precursor gas is provided intermittently.
14. The method according to any one of claims 1 to 13, in, The first Group IV semiconductor material precursor gas substantially includes a second Si-containing precursor gas, and the second Group IV semiconductor material precursor gas substantially includes a Ge-containing precursor gas.
15. The method according to claim 14, in, The second Si-containing precursor gas is silane, and the Ge-containing precursor gas is germane.
16. The method according to claim 14 or 15, in, The second Si-containing precursor gas is disilane, and the Ge-containing precursor gas is monogermane.
17. The method according to claim 16, in, The second Si-containing precursor gas is provided at a flow rate in a range of 30 sccm to 600 sccm, and the Ge-containing precursor gas is provided at a flow rate in a range of 100 sccm to 1600 sccm.
18. The method according to claim 17, in, The second Si-containing precursor gas is provided at a flow rate in the range of 30 sccm to 100 sccm during the first deposition pulse and at a flow rate in the range of 50 sccm to 100 sccm during the second deposition pulse.
19. The method according to claim 1, in, The epitaxial stack further includes a second epitaxial pair that is different from the first epitaxial pair, and wherein the epitaxial stack is formed on the substrate with at least one second epitaxial pair located between two adjacent first epitaxial pairs.
20. The method according to claim 19, in, The second epitaxial pairs include a first epitaxial layer and a third epitaxial layer, the third epitaxial layer includes at least the first Group IV semiconductor material and also includes a second Group IV semiconductor material, wherein the plurality of first epitaxial pairs have a first concentration of the second Group IV semiconductor material, and the third epitaxial pairs have a second concentration of the second Group IV semiconductor material, the second concentration being different from the first concentration.