Preparation method for improving performance of solar cell and cell
By screening out solar cells with high series resistance and refiring at lower than normal temperature, the series resistance problem caused by uneven sintering is solved, and a good Ag-Si alloy layer is formed, which improves the conversion efficiency and output characteristics of solar cells. .
Patent Information
- Application Number
- CN202411085289.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During the sintering process of solar cells, the Ag-Si alloy layer is unevenly sintered due to disturbance of the gas atmosphere in the sintering furnace, resulting in an increase in the series resistance of the battery cell and low conversion efficiency.
The cells with large series resistances were screened out and refired at lower than the normal sintering temperature to form a smooth and evenly distributed Ag-Si alloy layer, reducing the series resistance and increasing ohmic contact.
Through low-temperature refiring, the insufficient sintering area is compensated, micro defects and oxygen precipitation are reduced, and the conversion efficiency and output characteristics of solar cells are improved.
Smart Images

Figure CN118983374A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of photovoltaic technology, and in particular to a preparation method and a battery for improving the performance of a solar cell. Background Art
[0002] The sintering process of silver paste can increase the doping concentration of the tunneling oxide layer of ultra-thin silicon oxide. Since silver is a +1 valent element and silicon is a tetravalent element, the bonding of the two provides many holes, thereby generating a hole barrier on the back surface, causing the band structure near the back surface of the cell to change. When electrons diffuse to the back surface, the hole barrier generated on the back surface makes it difficult for electrons to pass through, thereby reducing the recombination of electrons and holes during the diffusion process, increasing the diffusion length of carriers, and improving the life of minority carriers. At the same time, the sintering process can cause the silver paste printed on the back surface to react with crystalline silicon to generate an Ag-Si alloy layer. Due to the structural difference between silver atoms and silicon atoms, the two will form a lattice mismatch after combining, thereby generating a certain amount of stress, which can effectively improve the effect of removing impurities from the back surface.
[0003] However, the formation of the Ag-Si alloy layer is related to many factors such as the gas atmosphere during the sintering process and the size of the velvet surface. Once the gas atmosphere changes during the sintering process, the quality of the formed Ag-Si alloy layer will be affected.
[0004] Among solar cells after screen sintering, some of the defects of the cells are caused by uneven sintering of the Ag-Si alloy layer due to changes in the gas atmosphere in the sintering furnace during the sintering process. For example, due to uneven gas distribution or too low gas concentration in some areas, the sintering degree of the back field is insufficient locally or in a large area, and a good quality Ag-Si alloy layer is not formed. These sintering defects will increase the series resistance of the cell, resulting in low conversion efficiency of the cell.
[0005] In view of this, this application is hereby filed. Summary of the invention
[0006] The problem with the prior art is that during the sintering process, the disturbance of the gas atmosphere in the sintering furnace causes sintering defects of the cell, such as insufficient sintering of a local or large area of the back field during the sintering process. These sintering defects will increase the series resistance of the cell, resulting in low conversion efficiency of the cell. In order to solve the above problem, the present invention provides a preparation method and a cell for improving the performance of solar cells. By screening out cells with large series resistance and re-firing them at a temperature lower than the normal sintering temperature, a smooth and evenly distributed Ag-Si alloy layer can be obtained on the back field surface to compensate for the insufficient sintering of a local or large area of the back field during the normal sintering process, thereby reducing the series resistance of the cell, enabling it to form a better ohmic contact, and improving the conversion efficiency of crystalline silicon solar cells.
[0007] The present invention is achieved through the following technical solutions:
[0008] In a first aspect, the present invention provides a method for improving the performance of a solar cell, comprising the following steps:
[0009] (1) Screening out solar cells with a series resistance greater than 1 mΩ from among the solar cells sintered by the wire mesh;
[0010] (2) Re-firing the solar cell with a series resistance greater than 1 mΩ.
[0011] The present invention can obtain a smooth and evenly distributed Ag-Si alloy layer on the back surface of the solar cell by screening out solar cells with relatively large series resistance and re-firing them at a temperature lower than the normal sintering temperature, so as to make up for the insufficient sintering of a part or a large area of the back surface during the normal sintering process, reduce the series resistance of the solar cell, enable it to form a better ohmic contact, and improve the conversion efficiency of the crystalline silicon solar cell.
[0012] In a specific embodiment, the sintering temperature of the re-firing is 5-10°C lower than the sintering temperature of the wire mesh in step (1).
[0013] In a specific embodiment, the sintering temperature of the re-firing in step (2) is the temperature of the lower temperature zone ten, which is 10°C lower than the temperature of the lower temperature zone ten of the wire mesh sintering in step (1).
[0014] In a specific embodiment, in a specific embodiment, the sintering conditions in the lower temperature zone of the re-firing in step (2) are set from temperature zone one to temperature zone ten as: 290°C, 455°C, 545°C, 575°C, 630°C, 635°C, 655°C, 675°C, 715°C, 745°C, and the actual peak temperature at the back of the re-firing sintering furnace is 685-690°C.
[0015] During the normal sintering process, the sintering temperature needs to reach the melting point of silver or higher, and the sintering temperature of silver is generally around 700°C, or above 720°C. After reaching a certain temperature, further increasing the sintering temperature will affect the smoothness of the Ag-Si alloy layer. Therefore, since the screened battery cells have undergone a sintering process, if the sintering temperature is the same as or higher than the normal sintering temperature during the re-firing process, it will affect the smoothness of the Ag-Si alloy layer, and the smoothness of the Ag-Si alloy layer in the sintered area will also be affected.
[0016] Therefore, the present invention selects a re-firing temperature that is 10°C lower than the normal sintering temperature. Due to the low-temperature re-firing, the recombination rate of the battery back surface can be reduced again in the area with insufficient sintering degree, and the long-wave spectrum response and battery output characteristics can be improved, thereby ensuring the smoothness of the Ag-Si alloy layer formed by re-firing, and then the screened battery cells form a good Ag-Si alloy layer; in addition, a lot of oxygen and micro-defects will form precipitation on the surface of the battery cell during the sintering process, but they will also be effectively absorbed by the re-formed Ag-Si alloy layer. Due to the reduction of these micro-defects and precipitation, more silicon atoms can be melted into the silver electrode material, so that the upper and lower electrodes form a good ohmic contact, reducing the series resistance and improving the conversion efficiency.
[0017] In a specific embodiment, the screen sintering in step (1) is the sintering of the back field silver paste of the solar cell, which is used to form an Ag-Si alloy layer with the Si wafer substrate.
[0018] In a specific embodiment, the sintering conditions in the upper temperature zone of the wire mesh sintering in step (1) are 450°C, 525°C, 570°C, 610°C, 640°C, 680°C, 695°C, 710°C, 745°C, and 815°C from temperature zone one to temperature zone ten, respectively.
[0019] In a specific embodiment, the sintering conditions in the lower temperature zone of the wire mesh sintering in step (1) are 290°C, 455°C, 545°C, 575°C, 630°C, 635°C, 655°C, 675°C, 715°C, and 755°C from temperature zone one to temperature zone ten, respectively.
[0020] In a specific embodiment, the drying zones for sintering the wire mesh in step (1) are 390°C, 345°C, 335°C, 325°C, 305°C, and 290°C from rapid heating to temperature zone five, respectively.
[0021] In a specific embodiment, the belt speed of the drying zone is 17 m / min.
[0022] In a second aspect, the present invention provides a high-performance solar cell manufactured by the preparation method.
[0023] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0024] 1. A preparation method and a battery for improving the performance of a solar cell provided in an embodiment of the present invention can obtain a smooth and evenly distributed Ag-Si alloy layer on the back surface of the solar cell by screening out solar cells with large series resistance and re-firing them at a temperature lower than the normal sintering temperature, so as to make up for the insufficient sintering of a part or a large area of the back surface during the normal sintering process, reduce the series resistance of the solar cell, enable it to form an ohmic contact better, and improve the conversion efficiency of the crystalline silicon solar cell;
[0025] 2. A preparation method and a battery for improving the performance of a solar cell provided by an embodiment of the present invention, wherein the re-firing temperature is selected to be 10°C lower than the normal sintering temperature. Due to the re-firing at a low temperature, the recombination velocity of the back surface of the battery can be reduced again in the area with insufficient sintering degree, thereby improving the long-wave spectrum response and battery output characteristics, thereby ensuring the smoothness of the Ag-Si alloy layer formed by re-firing, and further enabling the screened battery cells to form a good Ag-Si alloy layer;
[0026] 3. According to a preparation method and a battery for improving the performance of solar cells provided by an embodiment of the present invention, a lot of oxygen and micro defects will form precipitation on the surface of the battery cell during the sintering process, which will also be effectively absorbed by the newly formed Ag-Si alloy layer. Due to the reduction of these micro defects and precipitation, more silicon atoms can be melted into the silver electrode material, so that the upper and lower electrodes form a good ohmic contact, reducing the series resistance and improving the conversion efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 The present invention provides a solar cell manufacturing process. DETAILED DESCRIPTION
[0029] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.
[0030] In the following description, a large number of specific details are set forth in order to provide a thorough understanding of the present invention. However, it is apparent to one of ordinary skill in the art that these specific details need not be employed to practice the present invention. In other embodiments, in order to avoid obscuring the present invention, well-known materials or methods are not specifically described.
[0031] Throughout the specification, references to "one embodiment," "an embodiment," "an example," or "an example" mean that a particular feature, structure, or characteristic described in conjunction with the embodiment or example is included in at least one embodiment of the present invention. Therefore, the phrases "one embodiment," "an embodiment," "an example," or "an example" appearing in various places throughout the specification do not necessarily all refer to the same embodiment or example. In addition, particular features, structures, or characteristics may be combined in one or more embodiments or examples in any suitable combination and / or subcombination. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0032] At present, the formation of the Ag-Si alloy layer is related to many factors such as the gas atmosphere and the size of the velvet surface during the sintering process. Once the gas atmosphere changes during the sintering process, the quality of the formed Ag-Si alloy layer will be affected. In the solar cells after screen sintering, the defects of some cells are caused by the uneven sintering of the Ag-Si alloy layer due to the change of the gas atmosphere in the sintering furnace during the sintering process. For example, due to uneven gas distribution or too low gas concentration in some areas, the sintering degree of the back field is insufficient locally or over a large area, and a good quality Ag-Si alloy layer is not formed. These sintering defects will increase the series resistance of the cell, resulting in low conversion efficiency of the cell.
[0033] In order to solve the above problems, the present invention provides the following technical solutions:
[0034] First, as Figure 1 As shown, the present invention provides a preparation method for improving the performance of solar cells, comprising the following steps:
[0035] (1) Screening out solar cells with a series resistance greater than 1 mΩ from among the solar cells sintered by the wire mesh;
[0036] (2) Re-firing the solar cell with a series resistance greater than 1 mΩ.
[0037] The present invention can obtain a smooth and evenly distributed Ag-Si alloy layer on the back surface of the solar cell by screening out solar cells with relatively large series resistance and re-firing them at a temperature lower than the normal sintering temperature, so as to make up for the insufficient sintering of a part or a large area of the back surface during the normal sintering process, reduce the series resistance of the solar cell, enable it to form a better ohmic contact, and improve the conversion efficiency of the crystalline silicon solar cell.
[0038] In a specific embodiment, the sintering temperature of the re-firing is 5-10° C. lower than the sintering temperature of the wire mesh in step (1).
[0039] In a specific embodiment, the sintering temperature of the re-firing in step (2) is the temperature of the lower temperature zone ten, which is 10°C lower than the temperature of the lower temperature zone ten of the wire mesh sintering in step (1).
[0040] In a specific embodiment, in a specific embodiment, the sintering conditions in the lower temperature zone of the re-firing in step (2) are set from temperature zone one to temperature zone ten as: 290°C, 455°C, 545°C, 575°C, 630°C, 635°C, 655°C, 675°C, 715°C, 745°C, and the actual peak temperature at the back of the re-firing sintering furnace is 685-690°C.
[0041] During the normal sintering process, the sintering temperature needs to reach the melting point of silver or higher, and the sintering temperature of silver is generally around 700°C, or above 720°C. After reaching a certain temperature, further increasing the sintering temperature will affect the smoothness of the Ag-Si alloy layer. Therefore, since the screened battery cells have undergone a sintering process, if the sintering temperature is the same as or higher than the normal sintering temperature during the re-firing process, it will affect the smoothness of the Ag-Si alloy layer, and the smoothness of the Ag-Si alloy layer in the sintered area will also be affected.
[0042] Therefore, the present invention selects a re-firing temperature that is 10°C lower than the normal sintering temperature. Due to the low-temperature re-firing, the recombination rate of the battery back surface can be reduced again in the area with insufficient sintering degree, and the long-wave spectrum response and battery output characteristics can be improved, thereby ensuring the smoothness of the Ag-Si alloy layer formed by re-firing, and then the screened battery cells form a good Ag-Si alloy layer; in addition, a lot of oxygen and micro-defects will form precipitation on the surface of the battery cell during the sintering process, but they will also be effectively absorbed by the re-formed Ag-Si alloy layer. Due to the reduction of these micro-defects and precipitation, more silicon atoms can be melted into the silver electrode material, so that the upper and lower electrodes form a good ohmic contact, reducing the series resistance and improving the conversion efficiency.
[0043] In a specific embodiment, the screen sintering in step (1) is the sintering of the back field silver paste of the solar cell, which is used to form an Ag-Si alloy layer with the Si wafer substrate.
[0044] In a specific embodiment, the sintering conditions in the upper temperature zone of the wire mesh sintering in step (1) are 450°C, 525°C, 570°C, 610°C, 640°C, 680°C, 695°C, 710°C, 745°C, and 815°C from temperature zone one to temperature zone ten, respectively.
[0045] In a specific embodiment, the sintering conditions in the lower temperature zone of the wire mesh sintering in step (1) are 290°C, 455°C, 545°C, 575°C, 630°C, 635°C, 655°C, 675°C, 715°C, and 755°C from temperature zone one to temperature zone ten, respectively.
[0046] In a specific embodiment, the drying zones for sintering the wire mesh in step (1) are 390°C, 345°C, 335°C, 325°C, 305°C, and 290°C from rapid heating to temperature zone five, respectively.
[0047] In a specific embodiment, the belt speed of the drying zone is 17 m / min.
[0048] In a second aspect, the present invention provides a high-performance solar cell manufactured by the preparation method.
[0049] Example 1
[0050] An embodiment of the present invention provides a method for preparing a solar cell, comprising the following steps:
[0051] (1) After the screen sintering, the solar cells with a series resistance of more than 1 mΩ are selected; the sintering conditions of the upper temperature zone of the screen sintering are 450°C, 525°C, 570°C, 610°C, 640°C, 680°C, 695°C, 710°C, 745°C, and 815°C from temperature zone 1 to temperature zone 10; the sintering conditions of the lower temperature zone of the screen sintering are 290°C, 455°C, 545°C, 575°C, 630°C, 635°C, 655°C, 675°C, 715°C, and 755°C from temperature zone 1 to temperature zone 10; during the screen sintering, the peak actual temperature of the back of the sintering furnace is 700°C;
[0052] (2) For the solar cell with a series resistance of >1 mΩ, the sintering conditions in the upper temperature zone from temperature zone one to temperature zone ten are 450°C, 525°C, 570°C, 610°C, 640°C, 680°C, 695°C, 710°C, 745°C, and 815°C, respectively; the sintering conditions in the lower temperature zone from temperature zone one to temperature zone ten are 290°C, 455°C, 545°C, 575°C, 630°C, 635°C, 655°C, 675°C, 715°C, and 745°C, respectively, which is 10°C lower than the wire mesh sintering process temperature, that is, the re-firing is performed at a peak actual temperature of 690°C at the back of the sintering furnace.
[0053] The re-sintered cells were tested, and the test electrical performance results are shown in Table 1 below.
[0054] Table 1
[0055]
[0056]
[0057] As can be seen from Table 1, the re-firing temperature is 10°C lower than the normal sintering temperature, and the short-circuit current, open-circuit voltage and filling FF of the battery cell are all improved.
[0058] Comparative Example 1
[0059] This comparative example provides a method for preparing a solar cell, comprising the following steps:
[0060] (1) After the screen sintering, the solar cells with a series resistance of more than 1 mΩ are selected; the sintering conditions of the upper temperature zone of the screen sintering are 450°C, 525°C, 570°C, 610°C, 640°C, 680°C, 695°C, 710°C, 745°C, and 815°C from temperature zone 1 to temperature zone 10; the sintering conditions of the lower temperature zone of the screen sintering are 290°C, 455°C, 545°C, 575°C, 630°C, 635°C, 655°C, 675°C, 715°C, and 755°C from temperature zone 1 to temperature zone 10; when the screen is sintered, the peak actual temperature of the back of the sintering furnace is 700°C;
[0061] (2) The solar cell with a series resistance of >1 mΩ is re-fired, and the sintering conditions in the upper temperature zone are 450°C, 525°C, 570°C, 610°C, 640°C, 680°C, 695°C, 710°C, 745°C, and 815°C from temperature zone one to temperature zone ten, respectively; the sintering conditions in the lower temperature zone are 290°C, 455°C, 545°C, 575°C, 630°C, 635°C, 655°C, 675°C, 715°C, and 735°C from temperature zone one to temperature zone ten, respectively, which is 20°C lower than the wire mesh sintering process temperature, that is, the peak actual temperature at the back of the sintering furnace is 680°C for re-firing.
[0062] The re-sintered cells were tested, and the test electrical performance results are shown in Table 2 below.
[0063] Table 2
[0064]
[0065] It can be seen from Table 2 that the re-firing temperature is 20°C lower than the normal sintering temperature, and the electrical performance of the battery cell has a negative gain.
[0066] Comparative Example 2
[0067] This comparative example provides a method for preparing a solar cell, comprising the following steps:
[0068] (1) After the screen sintering, the solar cells with a series resistance of more than 1 mΩ are selected; the sintering conditions of the upper temperature zone of the screen sintering are 450°C, 525°C, 570°C, 610°C, 640°C, 680°C, 695°C, 710°C, 745°C, and 815°C from temperature zone 1 to temperature zone 10; the sintering conditions of the lower temperature zone of the screen sintering are 290°C, 455°C, 545°C, 575°C, 630°C, 635°C, 655°C, 675°C, 715°C, and 755°C from temperature zone 1 to temperature zone 10; when the screen is sintered, the peak actual temperature of the back of the sintering furnace is 700°C;
[0069] (2) The solar cell with a series resistance of more than 1 mΩ is re-fired, and the sintering conditions in the upper temperature zone from temperature zone one to temperature zone ten are 450°C, 525°C, 570°C, 610°C, 640°C, 680°C, 695°C, 710°C, 745°C, and 815°C, respectively; the sintering conditions in the lower temperature zone from temperature zone one to temperature zone ten are 290°C, 455°C, 545°C, 575°C, 630°C, 635°C, 655°C, 675°C, 715°C, and 765°C, respectively, which is 10°C higher than the wire mesh sintering process, i.e., the peak actual temperature at the back of the sintering furnace is 710°C for re-firing.
[0070] The re-sintered cells were tested, and the test electrical performance results are shown in Table 3 below.
[0071] Table 3
[0072]
[0073] It can be seen from Table 3 that when the re-firing temperature is increased by 10°C compared with the normal sintering temperature, the electrical performance of the cell has a negative gain.
[0074] The present invention can obtain a smooth and evenly distributed Ag-Si alloy layer on the back surface of the solar cell by screening out solar cells with relatively large series resistance and re-firing them at a temperature lower than the normal sintering temperature, so as to make up for the insufficient sintering of a part or a large area of the back surface during the normal sintering process, reduce the series resistance of the solar cell, enable it to form a better ohmic contact, and improve the conversion efficiency of the crystalline silicon solar cell.
[0075] The present invention selects a re-firing temperature that is 10°C lower than the normal sintering temperature. Due to the low-temperature re-firing, the recombination speed of the battery back surface can be reduced again in the area with insufficient sintering degree, and the long-wave spectrum response and battery output characteristics can be improved, thereby ensuring the smoothness of the Ag-Si alloy layer formed by re-firing, and then the screened battery cells form a good Ag-Si alloy layer; in addition, a lot of oxygen and micro-defects will form precipitation on the surface of the battery cell during the sintering process, but they will also be effectively absorbed by the re-formed Ag-Si alloy layer. Due to the reduction of these micro-defects and precipitation, more silicon atoms can be melted into the silver electrode material, so that the upper and lower electrodes form a good ohmic contact, reducing the series resistance and improving the conversion efficiency.
[0076] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A method for improving the performance of a solar cell, characterized in that: The steps include: (1) Screening out solar cells with a series resistance greater than 1 mΩ from among the solar cells sintered by the wire mesh; (2) Re-firing the solar cell with a series resistance greater than 1 mΩ.
2. A method for improving the performance of a solar cell according to claim 1, characterized in that: The sintering temperature of the re-firing is 5-10°C lower than the sintering temperature of the wire mesh in step (1).
3. A method for improving the performance of a solar cell according to claim 1, characterized in that: The sintering temperature of the re-firing in step (2) is the temperature of the lower temperature zone temperature zone ten, which is 10° C. lower than the temperature of the lower temperature zone temperature zone ten of the wire mesh sintering in step (1).
4. A method for improving the performance of a solar cell according to claim 1, characterized in that: The sintering conditions in the lower temperature zone of the re-firing in step (2) are set from temperature zone one to temperature zone ten as: 290°C, 455°C, 545°C, 575°C, 630°C, 635°C, 655°C, 675°C, 715°C, and 745°C, respectively, and the actual peak temperature at the back of the re-firing sintering furnace is 685-690°C.
5. The method for improving the performance of a solar cell according to claim 1, characterized in that: The screen sintering in step (1) is the sintering of the back field silver paste of the solar cell, which is used to form an Ag-Si alloy layer with the Si wafer substrate.
6. A method for improving the performance of a solar cell according to claim 1, characterized in that: The sintering conditions in the lower temperature zone of the wire mesh sintering in step (1) are 290°C, 455°C, 545°C, 575°C, 630°C, 635°C, 655°C, 675°C, 715°C, and 755°C from temperature zone one to temperature zone ten, respectively.
7. A method for improving the performance of a solar cell according to claim 1, characterized in that: The sintering conditions in the upper temperature zone of the wire mesh sintering in step (1) are set to 450°C, 525°C, 570°C, 610°C, 640°C, 680°C, 695°C, 710°C, 745°C, and 815°C from temperature zone 1 to temperature zone 10, respectively.
8. The method for improving the performance of a solar cell according to claim 1, characterized in that: The drying zones for sintering the screen in step (1) are 390° C., 345° C., 335° C., 325° C., 305° C., and 290° C. from rapid heating to temperature zone five.
9. A method for improving the performance of a solar cell according to claim 7, characterized in that: The belt speed of the drying zone is 17 m / min.
10. A high-performance solar cell, characterized in that: The invention is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for sintering solar battery cell
CN102222732A
Processing method of low efficient solar cell
CN102468363A
Solar silicon wafer sintering furnace
CN202083220U