Preparation method of three-dimensional carbon fiber battery with composite Bi-coated NC core-shell structure

The preparation of Bi@NC core-shell structure through electrospinning method solves the long-term cycleability problem of sodium metal negative electrodes under high capacity and high density, achieves efficient sodium ion diffusion and cycling stability, and reduces electrolyte consumption. Enhanced the mechanical strength and ionic conductivity of the material.

CN118983423AActive Publication Date: 2024-11-19ZHENGZHOU UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411212231.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-19
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

The long-term cycleability of sodium metal anode at high capacity and high density is still a significant challenge, and the uncontrollable growth of sodium dendrites leads to battery short circuits and safety hazards, hindering its practical application.

Method used

The three-dimensional sodium metal host negative electrode of Bi@NC core-shell structure was prepared by electrostatic spinning method. By controlling the spinning solution ratio and annealing temperature, the porous Bi@NC core-shell structure was obtained, reducing the direct contact between sodium and electrolyte, and forming a stable SEI films enhance mechanical strength and ionic conductivity.

Benefits of technology

A simple, controllable and economical preparation process is realized, the structural integrity of the active negative electrode material is maintained, the consumption of electrolyte is reduced, the mechanical strength and ionic conductivity of the material are enhanced, and the Coulomb efficiency and cyclic stability of sodium metal batteries are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983423A_ABST
    Figure CN118983423A_ABST
Patent Text Reader

Abstract

The three-dimensional carbon fiber continuous film with the composite Bi-coated NC core-shell structure is prepared by adopting an electrostatic spinning method, and the method comprises the following steps: firstly, preparing an electrostatic spinning precursor solution, then carrying out high-temperature calcination to obtain a Bi-coated NC flexible fiber film, and controlling the specific form of the Bi-coated NC core-shell structure fiber by changing the annealing temperature and time. The method is simple in process, low in cost and high in practicability, fiber films with different core-shell structures and morphologies can be obtained only by changing the annealing temperature, the annealing time and the use amount of the Bi precursor, and the fiber films show excellent performance when applied to a sodium metal negative electrode host and have good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy electrochemistry, and in particular to a method for preparing a three-dimensional carbon fiber battery with a composite Bi@NC core-shell structure. Background Art

[0002] Under the urgent demand for sustainable energy storage technology, sodium metal has an ultra-high theoretical specific capacity (1166 mA h g -1 ), low electrochemical potential (-2.714 V vs. standard hydrogen electrode) and abundant and cheap sodium-based resources have become a research hotspot in the energy field. However, due to the high electrochemical activity and infinite volume change of sodium metal, the uncontrollable excessive side reactions between sodium and electrolyte and the uncontrollable growth of sodium dendrites lead to rapid capacity decay and low Coulomb efficiency. At the same time, sodium dendrites may pierce the diaphragm and cause battery short circuit, and even bring major safety hazards, which seriously hinder the practical application of sodium metal anode. Optimizing electrolytes and electrolyte additives, designing three-dimensional sodium metal hosts, constructing low nucleation barrier engineering and interface engineering, and improving current collectors and diaphragms are commonly used improvement strategies by researchers. Among them, the core-shell structure based on amorphous carbon shells designed by combining the two improvement strategies of low nucleation barrier engineering and nano-interface is favored by researchers. The coulombic efficiency and cycling stability of Na-metal batteries can be improved by incorporating a variety of heterogeneous seeds such as N-doped carbon, Au nanoparticles, SnS2 nanosheets, CoSe2, Sb nanoparticles, Sn atoms, and Zn atoms into hollow amorphous carbon shells. Despite these advances, the long-term cyclability of Na-metal anodes at high capacity and density remains a significant challenge. The development of three-dimensional core-shell structured Na hosts, combining structural integrity with efficient charge transport, has shown potential to address this issue. However, the fabrication complexity of these hosts still hinders their widespread adoption. Fortunately, electrospinning has emerged as an economically attractive and controllable fabrication method. Bismuth (Bi) has a high affinity and enhances the diffusion kinetics of Na-ions, which helps promote efficient and dendrite-free cycling in Na-metal anodes. The cost-effectiveness of Bi is also a considerable advantage, promoting the prospect of large-scale deployment. Although the application of electrospun Bi-embedded fibers is mainly limited to Na-ion batteries, three-dimensional Bi core-carbon shell structures are now emerging as promising hosts for Na-metal anodes. Furthermore, the sodium deposition space provided by the core-shell structure is conducive to elucidating the underlying mechanism promoting the diffusion of sodium ions inside the sodium-bismuth alloy, which will provide valuable insights for ultimately improving the cyclability and performance of the sodium metal anode.

[0003] Electrospinning technology has the advantages of simple operation, controllable preparation, economy and environmental protection, and is widely used in sodium metal batteries. First, the diameter of the fiber is controlled by controlling the ratio of the precursor solution to find a size that is conducive to sodium deposition. Secondly, it can be spun out in a short time according to the prepared precursor solution, without the need to use a large amount of chemical reagents. Finally, the annealed material is flexible, resistant to folding and deformation, and can be used directly as a negative electrode material to avoid adding electrochemically inactive materials. During the high-temperature carbonization process, abundant nanopores of 10 to 50 nm were obtained by removing polymethyl methacrylate (PMMA) to obtain a Bi@NC core-shell structure. Summary of the invention

[0004] The present invention proposes a Bi@NC core-shell structured three-dimensional sodium metal host negative electrode prepared by an electrospinning method, which has a simple manufacturing process, strong controllability, is environmentally friendly and economical, and the porous structure can maintain the structural integrity of the active negative electrode material.

[0005] The technical solution of the present invention is: a method for preparing a Bi@NC core-shell structured nanometal battery negative electrode material, the steps are as follows: first prepare a spinning solution, then use an electrospinning method to obtain a three-dimensional carbon fiber continuous film, then place it in a vacuum drying oven for drying, and finally anneal it at different temperatures, assemble the battery, and obtain a three-dimensional carbon fiber battery with a composite Bi@NC core-shell structure.

[0006] The preparation steps of the spinning solution are as follows: adding polyacrylonitrile and polymethyl methacrylate to NN dimethylamide, heating and stirring for 2-5 hours in a water bath at 60°C-80°C, then adding BiCl3, and continuing to stir and react for 8-10 hours to obtain a spinning solution, wherein the mass ratio of polyacrylonitrile, polymethyl methacrylate and BiCl3 is 3-5:2-3:1.

[0007] The preparation steps of the three-dimensional carbon fiber continuous film obtained by the electrospinning method are as follows: pour the spinning solution into a syringe, connect the needle, then apply 12kV high voltage, control the rotation speed of the collecting device and the injection speed, and finally spin the silk on aluminum foil. The electrospinning method is: the syringe is 10ml, the inner diameter of the needle is 0.25mm, the rotation speed of the collecting device is 350r / min, the working voltage is 12KV, and the injection speed is 4ml / h.

[0008] The vacuum drying conditions are: in a vacuum drying oven at 60°C-80°C for 5-7 hours.

[0009] The annealing conditions of the electrospinning material are as follows: annealing with N2 / H2 mixed gas, the starting temperature is 20°C, the heating rate is 2°C / min, the temperature is increased to 350°C at a heating rate of 2°C / min, kept warm for 3h, increased to 720°C and kept warm for 4h, and cooled to the starting temperature of 20°C at a heating rate of 1°C / min.

[0010] The electrospinning material annealing conditions are as follows: annealing is performed using a N2 / H2 mixed gas, with a starting temperature of 25°C and a heating rate of 2°C / min. The temperature is raised to 350°C at a heating rate of 2°C / min, kept at that temperature for 3 hours, raised to 650°C and kept at that temperature for 8 hours, and then cooled to the starting temperature of 25°C at a heating rate of 1°C / min.

[0011] The annealing conditions of the electrospinning material can also be: annealing with N2 / H2 mixed gas, the starting temperature is 30°C, the heating rate is 2°C / min, rising to 350°C at a heating rate of 2°C / min, keeping warm for 3h, rising to 700°C and keeping warm for 5h, and cooling to the starting temperature of 30°C at a heating rate of 1°C / min.

[0012] Different annealing temperatures have different morphologies. When the temperature is high, Bi is easily volatilized, leaving a porous structure.

[0013] The steps of assembling the battery are as follows: first place the positive electrode sheet, then place the nanosheet, place the Bi@NC material, add electrolyte (35 ml), place 2 layers of PP separator, and then add electrolyte (35 ml), the electrolyte is NaPF6, place the Bi@NC material, place the sodium sheet, place the nickel mesh, the shrapnel, and finally add the negative electrode shell.

[0014] The present invention uses electrostatic spinning technology to prepare a Bi@NC core-shell structure three-dimensional sodium metal host as a nanometal negative electrode. The method first prepares a spinning solution, and then uses an electrostatic spinning method to prepare a nanometal three-dimensional structure host, which is placed in a vacuum drying oven for drying. Annealing is performed with a N2 / H2 mixed gas. At an annealing temperature of 720°C, a porous structure will appear, increasing the specific surface area, and these pores can accommodate the expansion of Bi particles. The core-shell structure can avoid direct contact between sodium and the electrolyte, reduce the consumption of the electrolyte, and form a stable SEI film on the carbon shell, which has strong ionic conductivity and strong mechanical strength.

[0015] The beneficial effects of the present invention are: (1) The electrospinning technology is simple, efficient, environmentally friendly and economical, and the diameter of the fiber can be directly controlled by changing the parameters; (2) At an annealing temperature of 720°C, PMMA will volatilize and a porous structure will appear, increasing the specific surface area. These pores can accommodate the expansion of Bi particles. Using this structure, other metals can be placed in it to maintain the structural integrity of the active negative electrode material; (3) The core-shell structure can prevent the electrolyte from directly contacting sodium, reduce the consumption of electrolyte, and enhance the mechanical strength of the material and the electrical conductivity of ions. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 Transmission electron microscopy (a, b, c) of Bi@NC fibers prepared at different annealing temperatures in Example 1 and scanning electron microscopy (d, e, f) of Bi@NC spinning materials; Figure 2 XRD spectrum of the Bi@NC core-shell structure three-dimensional sodium metal host negative electrode material prepared in Example 1; Figure 3 The Raman spectrum of the Bi@NC core-shell structure three-dimensional sodium metal host negative electrode material prepared in Example 1; Figure 4 The Bi@NC core-shell structure three-dimensional sodium metal host negative electrode material in Example 1 is 3 mA cm -2 , 3 mAh cm -2 Coulomb efficiency diagram below; Figure 5 The Bi@NC core-shell structure three-dimensional sodium metal host negative electrode material in Example 1 is 30 mA cm -2 , 3 mAhcm -2 The long cycle diagram below. DETAILED DESCRIPTION

[0017] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] Example 1 A method for preparing a Bi@NC core-shell structured nanometal battery negative electrode material, the steps are as follows: (1) Prepare the spinning solution. First, pour 15 ml of NN dimethylformamide (DMF), then slowly add 1.6 g of polyacrylonitrile (PAN) and 0.6 g of polymethyl methacrylate (PMMA) into DMF, heat in a 70 °C water bath and stir for 2 h to obtain a yellow viscous solution, then slowly add 0.42 g of BiCl3 and stir for another 8 h to obtain a uniform white solution; (2) Using electrospinning technology to obtain a three-dimensional carbon fiber continuous film, the steps are as follows: pouring the spinning solution into a syringe, connecting a needle, then applying high voltage, controlling the speed of the collecting device and the injection speed, and finally spinning the silk on aluminum foil. The spinning conditions are: the syringe is 10 ml, the inner diameter of the needle is 0.25 mm, the speed of the collecting device is 350 r / min, the working voltage is 12 KV, and the injection speed is 4 ml / h; (3) The spun samples were placed in a vacuum drying oven at 60 °C for 5 h, and finally annealed at different temperatures; annealing conditions: annealing with N2 / H2 mixed gas, starting temperature at 20 °C, heating rate at 2 °C / min, heating to 350 °C at 2 °C / min, keeping the temperature for 3 h, heating to 720 °C and keeping the temperature for 4 h, and cooling to the starting temperature of 20 °C at 1 °C / min; (4) Assemble the battery. The steps are as follows: first place the positive electrode sheet, then place the nanosheet, place the Bi@NC material, add electrolyte (35 ml), place 2 layers of PP separator, then add electrolyte NaPF6 (35 ml), place the Bi@NC material, place the nanosheet, place the nickel mesh, shrapnel, and finally add the negative electrode shell.

[0019] Example 2 A method for preparing a Bi@NC core-shell structured nanometal battery negative electrode material, the steps are as follows: (1) Prepare the spinning solution. First, pour 30 ml of NN dimethylformamide (DMF), then slowly add 5 g of polyacrylonitrile (PAN) and 3 g of polymethyl methacrylate (PMMA) into DMF, heat in a 60 °C water bath and stir for 3 h to obtain a yellow viscous solution, then slowly add 1 g of BiCl3 and stir for another 8 h to obtain a uniform white solution; (2) Using electrospinning technology to obtain a three-dimensional carbon fiber continuous film, the steps are as follows: pouring the spinning solution into a syringe, connecting a needle, then applying high voltage, controlling the speed of the collecting device and the injection speed, and finally spinning the silk on aluminum foil. The spinning conditions are: the syringe is 10 ml, the inner diameter of the needle is 0.25 mm, the speed of the collecting device is 350 r / min, the working voltage is 12 KV, and the injection speed is 4 ml / h; (3) The spun samples were placed in a vacuum drying oven at 80 °C for 7 h, and finally annealed at different temperatures; annealing conditions: annealing with N2 / H2 mixed gas, starting temperature at 20 °C, heating rate at 2 °C / min, heating to 350 °C at 2 °C / min, keeping the temperature for 3 h, heating to 720 °C and keeping the temperature for 4 h, and cooling to the starting temperature of 20 °C at 1 °C / min; (4) Assemble the battery. The steps are as follows: first place the positive electrode sheet, then place the nanosheet, place the Bi@NC material, add electrolyte (35 ml), place 2 layers of PP separator, then add electrolyte NaPF6 (35 ml), place the Bi@NC material, place the nanosheet, place the nickel mesh, shrapnel, and finally add the negative electrode shell.

[0020] Example 3 A method for preparing a Bi@NC core-shell structured nanometal battery negative electrode material, the steps are as follows: (1) Prepare the spinning solution. First, pour 30 ml of NN dimethylformamide (DMF), then slowly add 3 g of polyacrylonitrile (PAN) and 2 g of polymethyl methacrylate (PMMA) into DMF, heat in a water bath at 80 °C and stir for 3 h to obtain a yellow viscous solution, then slowly add 1 g of BiCl3 and stir for another 8 h to obtain a uniform white solution; (2) Using electrospinning technology to obtain a three-dimensional carbon fiber continuous film, the steps are as follows: pouring the spinning solution into a syringe, connecting a needle, then applying high voltage, controlling the speed of the collecting device and the injection speed, and finally spinning the silk on aluminum foil. The spinning conditions are: the syringe is 10 ml, the inner diameter of the needle is 0.25 mm, the speed of the collecting device is 350 r / min, the working voltage is 12 KV, and the injection speed is 4 ml / h; (3) The spun samples were placed in a vacuum drying oven at 60 °C for 3 h, and finally annealed at different temperatures; annealing conditions: annealing with N2 / H2 mixed gas, starting temperature at 20 °C, heating rate at 2 °C / min, heating to 350 °C at 2 °C / min, keeping the temperature for 3 h, heating to 720 °C and keeping the temperature for 4 h, and cooling to the starting temperature of 20 °C at 1 °C / min; (4) Assemble the battery. The steps are as follows: first place the positive electrode sheet, then place the nanosheet, place the Bi@NC material, add electrolyte (35 ml), place 2 layers of PP separator, then add electrolyte NaPF6 (35 ml), place the Bi@NC material, place the nanosheet, place the nickel mesh, shrapnel, and finally add the negative electrode shell.

[0021] Example 4 A method for preparing a Bi@NC core-shell structured nanometal battery negative electrode material, the steps are as follows: (1) Prepare the spinning solution. First, pour 15 ml of NN dimethylformamide (DMF), then slowly add 1.6 g of polyacrylonitrile (PAN) and 0.6 g of polymethyl methacrylate (PMMA) into DMF, heat in a 70 °C water bath and stir for 2 h to obtain a yellow viscous solution, then slowly add 0.42 g of BiCl3 and stir for another 8 h to obtain a uniform white solution; (2) Using electrospinning technology to obtain a three-dimensional carbon fiber continuous film, the steps are as follows: pouring the spinning solution into a syringe, connecting a needle, then applying high voltage, controlling the speed of the collecting device and the injection speed, and finally spinning the silk on aluminum foil. The spinning conditions are: the syringe is 10 ml, the inner diameter of the needle is 0.25 mm, the speed of the collecting device is 350 r / min, the working voltage is 12 KV, and the injection speed is 4 ml / h; (3) The spun samples were placed in a vacuum drying oven at 60 °C for 5 h, and finally annealed at different temperatures; annealing conditions: annealing with N2 / H2 mixed gas, starting temperature at 25 °C, heating rate at 2 °C / min, heating to 350 °C at 2 °C / min, keeping the temperature for 3 h, heating to 650 °C and keeping the temperature for 8 h, and cooling to the starting temperature of 25 °C at 1 °C / min; (4) Assemble the battery. The steps are as follows: first place the positive electrode sheet, then place the nanosheet, place the Bi@NC material, add electrolyte (35 ml), place 2 layers of PP separator, then add electrolyte NaPF6 (35 ml), place the Bi@NC material, place the nanosheet, place the nickel mesh, shrapnel, and finally add the negative electrode shell.

[0022] Example 5 A method for preparing a Bi@NC core-shell structured nanometal battery negative electrode material, the steps are as follows: (1) Prepare the spinning solution. First, pour 15 ml of NN dimethylformamide (DMF), then slowly add 1.6 g of polyacrylonitrile (PAN) and 0.6 g of polymethyl methacrylate (PMMA) into DMF, heat in a 70 °C water bath and stir for 2 h to obtain a yellow viscous solution, then slowly add 0.42 g of BiCl3 and stir for another 8 h to obtain a uniform white solution; (2) Using electrospinning technology to obtain a three-dimensional carbon fiber continuous film, the steps are as follows: pouring the spinning solution into a syringe, connecting a needle, then applying high voltage, controlling the speed of the collecting device and the injection speed, and finally spinning the silk on aluminum foil. The spinning conditions are: the syringe is 10 ml, the inner diameter of the needle is 0.25 mm, the speed of the collecting device is 350 r / min, the working voltage is 12 KV, and the injection speed is 4 ml / h; (3) placing the spun sample in a vacuum drying oven at 60°C for 5 hours, and finally annealing it at different temperatures; Annealing conditions: the annealing conditions of the electrospinning material can also be: annealing with a N2 / H2 mixed gas, with a starting temperature of 30°C and a heating rate of 2°C / min, heating to 350°C at a heating rate of 2°C / min, keeping the temperature for 3 hours, heating to 700°C and keeping the temperature for 5 hours, and cooling to the starting temperature of 30°C at a heating rate of 1°C / min; (4) Assemble the battery. The steps are as follows: first place the positive electrode sheet, then place the nanosheet, place the Bi@NC material, add electrolyte (35 ml), place 2 layers of PP separator, then add electrolyte NaPF6 (35 ml), place the Bi@NC material, place the nanosheet, place the nickel mesh, shrapnel, and finally add the negative electrode shell.

Claims

1. A method for preparing a three-dimensional carbon fiber battery with a composite Bi@NC core-shell structure, characterized in that: The steps are as follows: first prepare the spinning solution, then use the electrospinning method to obtain a three-dimensional carbon fiber continuous film, then dry it in a vacuum drying oven, and finally anneal it at different temperatures, assemble the battery, and obtain a three-dimensional carbon fiber battery with a composite Bi@NC core-shell structure.

2. The method for preparing a three-dimensional carbon fiber battery with a composite Bi@NC core-shell structure according to claim 1, characterized in that: The preparation steps of the spinning solution are as follows: add polyacrylonitrile and polymethyl methacrylate to NN dimethylamide, heat and stir for 2-5 hours in a water bath at 60°C-80°C, then add BiCl3, continue stirring and reacting for 8-10 hours to obtain a spinning solution, wherein the mass ratio of polyacrylonitrile, polymethyl methacrylate and BiCl3 is 3-5:2-3:

1.

3. The method for preparing a three-dimensional carbon fiber battery with a composite Bi@NC core-shell structure according to claim 1, characterized in that: The steps for preparing the three-dimensional carbon fiber continuous film by using the electrospinning method are as follows: pour the spinning solution into a syringe, connect the needle, then apply 12kV high voltage, control the rotation speed of the collection device and the injection speed, and finally spin the silk on aluminum foil.

4. The method for preparing a three-dimensional carbon fiber battery with a composite Bi@NC core-shell structure according to claim 1, characterized in that: The vacuum drying conditions are: in a vacuum drying oven at 60°C-80°C for 5-7 hours.

5. The method for preparing a three-dimensional carbon fiber battery with a composite Bi@NC core-shell structure according to claim 1, characterized in that: The annealing conditions of the electrospinning material are as follows: annealing with N2 / H2 mixed gas, the starting temperature is 20°C, the heating rate is 2°C / min, the temperature is increased to 350°C at a heating rate of 2°C / min, kept warm for 3h, increased to 720°C and kept warm for 4h, and cooled to the starting temperature of 20°C at a heating rate of 1°C / min.

6. The method for preparing a three-dimensional carbon fiber battery with a composite Bi@NC core-shell structure according to claim 1, characterized in that: The annealing conditions of the electrospinning material are as follows: annealing with N2 / H2 mixed gas, the starting temperature is 25°C, the heating rate is 2°C / min, heating to 350°C at a heating rate of 2°C / min, keeping warm for 3h, heating to 650°C and keeping warm for 8h, and cooling to the starting temperature of 25°C at a heating rate of 1°C / min.

7. The method for preparing a three-dimensional carbon fiber battery with a composite Bi@NC core-shell structure according to claim 1, characterized in that: The annealing conditions of the electrospinning material are as follows: annealing with N2 / H2 mixed gas, the starting temperature is 30°C, the heating rate is 2°C / min, the temperature is increased to 350°C at a heating rate of 2°C / min, kept warm for 3h, increased to 700°C and kept warm for 5h, and cooled to the starting temperature of 30°C at a heating rate of 1°C / min.

8. The method for preparing a three-dimensional carbon fiber battery with a composite Bi@NC core-shell structure according to claim 1, characterized in that: The steps of assembling the battery are as follows: first place the positive electrode sheet, then place the nanosheet, place the Bi@NC material, add electrolyte, place 2 layers of PP separator, then add electrolyte, place the Bi@NC material, place the sodium sheet, place the nickel mesh, the shrapnel, and finally add the negative electrode shell.

9. The method for preparing a three-dimensional carbon fiber battery with a composite Bi@NC core-shell structure according to claim 8, characterized in that: The electrolyte is NaPF6.

Citation Information

Patent Citations

  • Bismuth-based nano material as well as preparation method and application thereof

    CN113161530A

  • Porous bismuth carbon fiber negative electrode material for potassium ion battery and preparation method of porous bismuth carbon fiber negative electrode material

    CN115522284A

  • Preparation method of M-Sb alloy packaged carbon nanofiber negative electrode material and application of M-Sb alloy packaged carbon nanofiber negative electrode material in potassium / lithium ion battery

    CN115732655A

  • Negative electrode material for lithium metal battery, preparation method of negative electrode material and lithium metal battery

    CN115842121A

  • Core-shell typed cobalt / carbon composite nanofiber and method of manufacturing the same

    KR1020100123072A