Electrolyte of high-power lithium ion battery and lithium ion battery

By using electrolyte containing lithium dioxalate borate and fluorofluorophosphate homotriazine organic compounds in lithium-ion batteries, a SEI layer rich in F, P, and B was formed, and a high-power lithium-ion battery was solved at a maximum rate. Polarization and safety issues during charging and discharging improve cycle stability and high and low temperature performance.

CN118983518APending Publication Date: 2024-11-19WANXIANG 123 CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411063881.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing high-power lithium-ion batteries have increased polarization and safety risks during large-scale charging and discharging. The prior art maintains the stability of the SEI film by increasing the amount of film-forming additives, but leads to deterioration of cycle life.

Method used

Using an electrolyte containing lithium dioxalic acid borate and fluorofluorophosphate homotriazine organic compounds, the charge migration impedance is reduced, and cycle stability and high and low temperature are improved by forming an SEI layer rich in inorganic substances such as F, P, and B. performance.

Benefits of technology

While achieving high power performance, it ensures the long cycle life and high and low temperature performance of the battery, avoids the risk of electrode material corrosion and high-temperature thermal runaway from the battery, and reduces the acidity and DC internal resistance of the electrolyte.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention discloses an electrolyte of a high-power lithium ion battery and the lithium ion battery, the electrolyte of the high-power lithium ion battery comprises a lithium salt, an organic solvent and an additive, the lithium salt comprises lithium bis (oxalato) borate, and the additive comprises a fluoro-fluorophosphate s-triazine organic compound. According to the electrolyte of the high-power lithium ion battery and the lithium ion battery provided by the invention, when lithium bis (oxalato) borate is combined with the fluoro-fluorophosphate s-triazine organic compound for use, an SEI layer rich in inorganic matters such as F, P and B can be formed, and compared with organic SEI, the SEI is thinner and more compact, has an effect of rapidly conducting Li < + >, and can be applied to the lithium ion battery. The charge migration impedance is reduced, cracks are not easy to appear during circulation, the power performance of the battery is improved, and the cycle performance and high and low temperature performance of the battery are stabilized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium ion batteries, and in particular relates to an electrolyte of a high-power lithium ion battery and a lithium ion battery. Background Art

[0002] Lithium-ion batteries are widely used in new energy vehicles, electric bicycles, consumer electronics, energy storage and other fields due to their high energy, long life, high cost performance and low pollution. At the same time, as the country further improves vehicle fuel consumption and emission standards, energy conservation and emission reduction have become a common issue that all automobile companies need to face.

[0003] The 48V system of automobiles has the characteristics of low investment and significant energy saving and emission reduction. It can significantly increase the power of on-board power supply and meet the requirements of high-power on-board electrical appliances. It is a hot topic of research in the current automobile industry. The technical difficulty of 48V start-stop is to ensure high-rate charging and discharging, that is, high-power characteristics, while taking into account its long service life and excellent high and low temperature performance, which has high requirements for the design of the electrolyte. During high-rate charging and discharging, the construction of the battery SEI film is crucial. Under high-rate charging, the charge transfer impedance of the SEI film increases, which increases the electrode polarization during the charging process. At the same time, the heat generation of the battery cell increases significantly during high-rate charging and discharging. The hydrofluoric acid produced by the decomposition of lithium hexafluorophosphate, a lithium salt, will directly corrode the positive electrode material, and even corrode the copper foil, posing a safety hazard. In view of the increased polarization and safety issues that may occur during the above high-power charging and discharging, the current solution is mainly to optimize the electrolyte, increase the stability of the electrolyte, improve the stability and uniformity of the SEI, reduce the lithium precipitation problem that may occur during high-current charging and discharging, and reduce the thickness of the SEI film, thereby reducing the initial value and growth rate of DCIR, and achieving the requirements of long cycle life and good high and low temperature performance. The existing technical solution maintains the stability of the SEI film by increasing the amount of film-forming additives added and continuously decomposing the film during the cycle, but the continuous thickening of the SEI will cause an increase in DCIR, which in turn deteriorates the cycle life. Summary of the invention

[0004] The present invention provides an electrolyte for a high-power lithium-ion battery and a lithium-ion battery to solve the above-mentioned technical problems, and specifically adopts the following technical solutions:

[0005] An electrolyte for a high-power lithium-ion battery, comprising: a lithium salt, an organic solvent and an additive, wherein the lithium salt comprises lithium dioxalate borate, and the additive comprises a fluoro-substituted fluorophosphate-based triazine organic compound;

[0006] The fluorophosphoryl triazine organic compound has the structure shown below:

[0007]

[0008] Wherein, R1 is selected from one or more of hydrogen, halogen, substituted or unsubstituted alkane, alkene, alkyne, aromatic group, carbonate group, phosphate group, sulfonate group, sulfate group, fluorophosphate group, borate group, siloxy group, cyanoethoxy group and isocyanate group.

[0009] Further, R1 is selected from one or more of cyanoethoxy, phosphate, sulfate, sulfonyl, oxalate and siloxy groups.

[0010] Furthermore, the fluorophosphoryl-s-triazine organic compound is one of the following formulas:

[0011]

[0012] Furthermore, the amount of the fluorophosphoric acid-based triazine organic compound added is 0.01%-0.1% of the total mass of the electrolyte.

[0013] Furthermore, the amount of the fluorophosphoric acid-based triazine organic compound added is 0.01%-0.05% of the total mass of the electrolyte.

[0014] Further, the organic solvent comprises one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, methyl acetate, ethyl acetate, ethyl propionate, propyl propionate, fluorobenzene, fluoroethylene carbonate, fluoroethyl methyl carbonate, fluorodimethyl carbonate, and fluorodiethyl carbonate;

[0015] The lithium salt also includes one or more of lithium hexafluorophosphate, lithium bis(trifluorosulfonyl imide), lithium bis(oxalatoborate), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium difluorophosphate, lithium bis(trifluoromethanesulfonyl imide), lithium perchlorate, and lithium hexafluoroarsenate.

[0016] Furthermore, the amount of lithium bis(oxalatoborate) added is 0.03-4% of the total mass of the electrolyte.

[0017] Furthermore, the additives also include positive and negative electrode film-forming additives;

[0018] The positive and negative electrode film-forming additives include one or more of vinylene carbonate, fluoroethylene carbonate, methylene disulfonate, 1,3-propane sultone, vinyl sulfate, tris(trimethyl)silyl phosphate, lithium tetrafluorooxalate phosphate, lithium difluorooxalate borate, and lithium difluorophosphate.

[0019] Furthermore, the positive electrode film-forming additives are fluoroethylene carbonate, vinyl sulfate, lithium difluorophosphate, methylene disulfonate and tris(trimethyl)silyl phosphate, wherein the amount of fluoroethylene carbonate added accounts for 3%-10% of the total mass of the electrolyte, the amount of vinyl sulfate added accounts for 0.5-3% of the total mass of the electrolyte, the amount of lithium difluorophosphate added accounts for 0.3%-1.2% of the total mass of the electrolyte, the amount of methylene disulfonate added accounts for 0.2%-3% of the total mass of the electrolyte and the amount of tris(trimethyl)silyl phosphate added accounts for 0.3%-2% of the total mass of the electrolyte.

[0020] A high-power lithium-ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and the aforementioned electrolyte.

[0021] The present invention is also beneficial in that the electrolyte and lithium ion battery of the high-power lithium ion battery provided have good film-forming properties of lithium bis(oxalate borate), and the generated boron-containing SEI is dense and uniform, which can effectively protect the negative electrode interface and alleviate the occurrence of side reactions at the interface. At the same time, its good flame retardant properties can better alleviate the risk of high-temperature thermal runaway of the battery. The triazine group of the fluoro-substituted fluorophosphate-based triazine organic compound contains three N atoms with lone pairs of electrons, showing weak alkalinity, which can well neutralize the byproduct hydrofluoric acid of lithium hexafluorophosphate lithium salt, inhibit the increase in electrolyte acidity, and avoid corrosion of electrode materials. And the organic matter improves the flame retardant properties of the compound, the stability of SEI film formation, and the safety and cycle stability of the electrolyte through fluorine element substituents. Groups such as fluorophosphate groups can stably form films at the interface to achieve effects such as reduced impedance, improved circulation and low temperature performance. When lithium dioxalate borate is used in combination with fluorophosphoric acid-based triazine organic compounds, an SEI layer rich in inorganic substances such as F, P, and B can be formed. Compared with organic SEI, this SEI is thinner and denser, has the effect of fast Li+ conduction, reduces charge migration impedance and has higher stability during circulation, improves the power performance of the battery, and stabilizes the cycle performance and high and low temperature performance of the battery. Due to the synergistic effect of the functional groups of the fluorophosphoric acid-based triazine organic compound, it has a good effect of reducing impedance, improving high temperature cycle and storage performance, and improving cycle life, so its addition amount can be controlled at a lower level, generally at 100-300ppm. This lower addition amount will not affect the cycle stability of the lithium ion battery, and overcomes the shortcomings of cycle life degradation and significantly increased cost caused by the increase in byproducts that may be introduced by conventional additives. The present invention not only achieves high power performance, but also ensures good circulation, storage and high and low temperature performance. DETAILED DESCRIPTION

[0022] The embodiments of the present application are described in detail below, and examples of the embodiments are shown, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below by reference are exemplary and are intended to be used to explain the present application, and cannot be understood as limiting the present application.

[0023] The present application discloses an electrolyte for a high-power lithium-ion battery, comprising: a lithium salt, an organic solvent and an additive. The lithium salt comprises lithium dioxalate borate, and the additive comprises a fluorophosphoric acid-based triazine organic compound. The amount of the lithium dioxalate borate added accounts for 0.03-4% of the total mass of the electrolyte.

[0024] Specifically, the fluorophosphoryl-s-triazine organic compound has a structure shown in the following formula:

[0025]

[0026] Wherein, R1 is selected from one or more of hydrogen, halogen, substituted or unsubstituted alkane, alkene, alkyne, aromatic group, carbonate group, phosphate group, sulfonate group, sulfate group, fluorophosphate group, borate group, siloxy group, cyanoethoxy group and isocyanate group. Preferably, R1 is selected from one or more of cyanoethoxy group, phosphate group, sulfate group, sulfonyl ester group, oxalate group and siloxy group.

[0027] As a preferred embodiment, the fluorophosphoryl-s-triazine organic compound is one of the following formulas:

[0028] T1: T2: T3:

[0029] T3: T4: T5:

[0030] It is understandable that the triazine group in the fluorophosphoric acid triazine organic compound can react with the water in the electrolyte and the hydrofluoric acid, phosphorus pentafluoride and other acidic substances generated after storage. The reduction of acidic substances and water in the electrolyte effectively alleviates the decomposition and consumption of the electrolyte at the interface and enhances the storage performance of the lithium-ion battery. The fluorine substituent improves the flame retardant properties of this organic compound and the stability of SEI film formation, thereby improving the safety and cycle stability of the electrolyte. At the same time, the rate performance of the lithium-ion battery can also be improved by promoting the formation of a stable SEI through groups such as fluorophosphoric acid. Due to the synergistic effect of the various functional groups of this organic compound, it has a good effect of reducing impedance, improving high-temperature cycle and storage performance, and improving cycle life, so its addition amount can be controlled at a low level. The lower addition amount will not affect the cycle stability of the lithium-ion battery, and overcomes the shortcomings of increased DCIR and storage deterioration that may be introduced by conventional additives. The novel electrolyte additive of the present application improves its low-temperature and room-temperature power without sacrificing the cycle life of the lithium-ion battery, while optimizing the performance of high-temperature cycle and storage.

[0031] In the present application, the amount of fluorophosphoric acid-based triazine organic compounds added to T1-T6 accounts for 0.01%-0.1% of the total mass of the electrolyte. It is understandable that the amount of fluorophosphoric acid-based triazine organic compounds added directly affects the high-temperature storage, high-temperature cycle and DCIR of lithium-ion batteries. If the amount of fluorophosphoric acid-based triazine organic compounds added is higher, the performance improvement of high-temperature storage and cycle will be more obvious, but the DCIR reduction of the battery cell will be suppressed, and a small increase in DCIR will occur, which will slightly deteriorate the cycle life of the lithium-ion battery. This is because the new electrolyte will undergo redox decomposition at the positive and negative electrodes, forming a solid interface film at the interface between the positive and negative electrodes. The higher the amount of fluorophosphoric acid-based triazine organic compounds added, the thicker the solid interface film formed on the surface of the positive and negative electrodes, the DCIR of the battery cell will be slightly higher, and the DCIR of the lithium-ion battery cell will deteriorate. However, if the amount of fluorophosphoric acid-based triazine organic compound added is insufficient, its participation in film formation will be reduced, and the high-temperature storage and cycle performance of the battery cell will be reduced.

[0032] Considering that the amount of fluorophosphoric acid-based s-triazine organic compound added has an inverted U-shaped effect curve on the life of the battery cell and DCIR, in the present application, preferably, the amount of fluorophosphoric acid-based s-triazine organic compound added accounts for 0.01%-0.05% of the total mass of the electrolyte.

[0033] Furthermore, when the amount of the fluorinated fluorophosphate-based s-triazine organic compound added is less than 0.05%, it has almost no effect on the cycle life of the battery cell, and in order to take into account the high temperature storage, high temperature cycle and power performance of the lithium-ion battery, it is necessary to ensure that a sufficient amount of the fluorinated fluorophosphate-based s-triazine organic compound is added. Therefore, it is more preferred that the amount of the fluorinated fluorophosphate-based s-triazine organic compound added accounts for 0.03-0.05% of the total mass of the electrolyte.

[0034] In the embodiment of the present application, the organic solvent is mainly one or more of carbonate or carboxylate, specifically, the organic solvent comprises one or more of dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, ethylene carbonate, propylene carbonate, methyl acetate, ethyl acetate, ethyl propionate, propyl propionate, fluorobenzene, fluoroethylene carbonate, methyl ethyl carbonate, fluorodimethyl carbonate, and fluorodiethyl carbonate. Preferably, the organic solvent used in the present application comprises two or more of the above solvents, and the ratio between the solvents is not limited.

[0035] As a preferred embodiment, the lithium salt further comprises one or more of lithium hexafluorophosphate, lithium bis(trifluorosulfonyl)imide, lithium bis(oxalatoborate), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium difluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium perchlorate, and lithium hexafluoroarsenate. The present invention does not limit the content and proportion of lithium salts other than lithium bis(oxalatoborate).

[0036] The present application does not specifically limit the mass fraction of lithium salt and organic solvent in the electrolyte, and can be limited by referring to the mass fraction of lithium salt and solvent in the electrolyte commonly used in the field of lithium-ion batteries, or determined according to factors such as the positive electrode material, negative electrode material, separator, battery cell design, and development requirements of lithium-ion batteries. In a specific embodiment of the present application, the content of lithium salt is controlled between 8% and 17%.

[0037] As a preferred embodiment, the additive also includes positive and negative electrode film-forming additives. It is understandable that the new additive fluoro-fluorophosphate-based triazine organic compound mentioned in the present application can be used alone. It can also be used together with positive and negative electrode film-forming additives. Compared with the use of the new electrolyte additive alone, the electrolyte additive is used in combination with the positive and negative electrode film-forming additives, which improves the performance of the battery cell more significantly, reduces impedance, and improves the performance of high-temperature cycles and high-temperature storage. Adding positive and negative electrode film-forming additives to the electrolyte containing fluoro-fluorophosphate-based triazine compounds can further optimize the performance of lithium-ion batteries, especially improve the high-temperature cycle, storage and rate performance of lithium-ion batteries. This is mainly because the addition of positive and negative electrode film-forming additives can form CEI films and SEI films at the positive and negative electrodes before the decomposition of the new additives, which further enhances the stability of the interface film and further improves the cycle performance and life.

[0038] The positive and negative electrode film-forming additives involved in the present application are one or more of carbon-based additives, sulfur-based additives, phosphorus-based additives, boron-based additives, nitrogen-based additives, and silicon-based additives. Specifically, the positive and negative electrode film-forming additives include one or more of vinylene carbonate, fluoroethylene carbonate, methylene disulfonate, 1,3-propane sultone, vinyl sulfate, tris(trimethyl)silyl phosphate, lithium tetrafluorooxalate phosphate, lithium difluorooxalate borate, and lithium difluorophosphate.

[0039] The amount of film-forming additives added to the positive and negative electrodes will affect the cycle performance, storage performance and rate performance of the battery cell. Increasing the content of film-forming additives for the positive and negative electrodes can improve the cycle performance of the battery cell, but it will significantly increase the DC internal resistance of the battery cell and reduce the rate performance. In order to balance the effect of film-forming additives on electrical properties, it is necessary to optimize the amount of film-forming electrolyte additives added to the positive and negative electrodes. In an embodiment of the present application, the film-forming additives for the positive and negative electrodes are fluoroethylene carbonate, vinyl sulfate, lithium difluorophosphate, methylene disulfonate and tris(trimethyl)silyl phosphate. Among them, the added amount of fluoroethylene carbonate accounts for 3%-10% of the total mass of the electrolyte, the added amount of vinyl sulfate accounts for 0.5-3% of the total mass of the electrolyte, the added amount of lithium difluorophosphate accounts for 0.3%-1.2% of the total mass of the electrolyte, the added amount of methylene methanedisulfonate accounts for 0.2%-3% of the total mass of the electrolyte and the added amount of tris(trimethyl)silyl phosphate accounts for 0.3%-2% of the total mass of the electrolyte.

[0040] The present application also discloses a high-power lithium-ion battery, comprising: a positive electrode sheet, a negative electrode sheet, a separator and the aforementioned electrolyte.

[0041] The positive electrode active material of the lithium-ion battery of the present application includes one or more of all commonly used materials, such as lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium iron phosphate, lithium manganese iron phosphate, nickel-cobalt-manganese ternary material, nickel-cobalt-aluminum ternary material, lithium-rich manganese, etc.

[0042] The main preparation method of the positive electrode sheet is to select one or more of the above positive electrode active materials, lithium iron-rich lithium, conductive agent, and binder polyvinylidene fluoride (PVDF) according to the mass ratio of 93:2.5:2:2.5, disperse them in an appropriate amount of N-methylpyrrolidone, and then stir them thoroughly according to the homogenization process. The uniformly dispersed positive electrode slurry is evenly coated on aluminum foil, and the positive electrode sheet is obtained after baking, rolling, slitting, and punching.

[0043] The present invention does not strictly limit the type of negative electrode active materials. Currently commonly used negative electrode active materials can meet the requirements of the present invention. This patent selects one or more negative electrode materials. Negative electrode active materials include natural graphite, artificial graphite, hard carbon, soft carbon, silicon carbon, silicon dioxide, lithium titanate, etc.

[0044] The specific production process of the negative electrode sheet is as follows: select one or more negative electrode active materials, conductive agents, styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), put all raw materials into a planetary mixing tank at a mass ratio of 96:1:2:1, and make a uniformly dispersed negative electrode slurry according to the slurry making process. Then the negative electrode slurry is evenly coated on the copper foil, and after baking, rolling, slitting, and punching, the negative electrode sheet is obtained.

[0045] The present invention does not strictly limit the selection range of the diaphragm, and commonly used diaphragms meet the requirements of the present invention, for example: polypropylene diaphragm (PP), polyethylene diaphragm (PE), polyethylene / polypropylene double-layer composite film, polyimide electrospinning diaphragm (PI), polypropylene / polyethylene / polypropylene three-layer composite diaphragm (PP / PE / PP), ceramic diaphragm, PVDF coated diaphragm, etc.

[0046] After the positive and negative electrodes are punched, the positive electrode is placed in an oven at 110-140°C and the negative electrode is placed in an oven at 90-100°C for 20-30 hours. When the moisture content of the electrode sheet meets the requirements, the positive electrode sheet, the negative electrode sheet and the diaphragm are placed in a stacking machine to stack into a bare cell, and then the bare cell is packaged in a stamped aluminum-plastic film bag. After the packaged dry cell is dried at 80-95°C for 8-15 hours, the electrolyte of the present invention is injected into the dry cell, and the cell is placed, formed, placed at high temperature, evacuated and sealed, and divided into volumes to obtain a lithium-ion battery.

[0047] The specific embodiments of the present application are introduced below. The electrolytes in the embodiments and comparative examples in the present application are prepared by the following steps: controlling the moisture content in the glove box to be less than 10ppm, and controlling the moisture content of the solvent to be less than 10ppm. Use a pipette to accurately transfer ethylene carbonate and ethyl methyl carbonate in the glove box in a ratio of 3:7, then pour them into an aluminum bottle, stir them thoroughly and freeze them in a constant temperature box at 0°C for 1h. Then add lithium hexafluorophosphate to the mixed solvent at a concentration of 1.2mol / L, stirring while adding. Finally, add a certain amount of fluoroethylene carbonate, methylene disulfonate, vinyl sulfate, tris(trimethyl)silyl phosphate, lithium difluorophosphate, one or more of fluorofluorophosphate-based triazine organic compounds, and different contents of lithium dioxalate borate lithium salt.

[0048] The positive electrode active material of the lithium ion battery used in the examples and comparative examples of the present application is lithium iron phosphate, the negative electrode active material is artificial graphite, and the diaphragm is a polypropylene / polyethylene / polypropylene three-layer composite ceramic diaphragm.

[0049] Example 1

[0050] The positive and negative electrode film-forming additives used in this embodiment are 0.2% vinyl sulfate, 5% fluoroethylene carbonate, 1.5% tris(trimethyl)silyl phosphate, 0.6% methanedisulfonic acid methylene ester, and 0.8% lithium difluorophosphate. On this basis, T1 additive and lithium dioxalate borate are added. The amount of T1 added accounts for 0.05% of the mass fraction of the electrolyte, and the amount of lithium dioxalate borate added accounts for 1.8% of the mass fraction of the electrolyte.

[0051] Example 2

[0052] The positive and negative electrode film-forming additives used in this embodiment are 0.2% vinyl sulfate, 5% fluoroethylene carbonate, 1.5% tris(trimethyl)silyl phosphate, 0.6% methanedisulfonic acid methylene ester, and 0.8% lithium difluorophosphate. On this basis, T2 additive and lithium dioxalate borate are added. The amount of T2 added accounts for 0.05% of the mass fraction of the electrolyte, and the amount of lithium dioxalate borate added accounts for 1.8% of the mass fraction of the electrolyte.

[0053] Example 3

[0054] The positive and negative electrode film-forming additives used in this embodiment are 0.2% vinyl sulfate, 5% fluoroethylene carbonate, 1.5% tris(trimethyl)silyl phosphate, 0.6% methanedisulfonic acid methylene ester, and 0.8% lithium difluorophosphate. On this basis, T3 additive and lithium dioxalate borate are added. The amount of T3 added accounts for 0.05% of the mass fraction of the electrolyte, and the amount of lithium dioxalate borate added accounts for 1.8% of the mass fraction of the electrolyte.

[0055] Example 4

[0056] The positive and negative electrode film-forming additives used in this embodiment are 0.2% vinyl sulfate, 5% fluoroethylene carbonate, 1.5% tris(trimethyl)silyl phosphate, 0.6% methanedisulfonic acid methylene ester, and 0.8% lithium difluorophosphate. On this basis, T4 additive and lithium dioxalate borate are added. The amount of T4 added accounts for 0.05% of the mass fraction of the electrolyte, and the amount of lithium dioxalate borate added accounts for 1.8% of the mass fraction of the electrolyte.

[0057] Example 5

[0058] The positive and negative electrode film-forming additives used in this embodiment are 0.2% vinyl sulfate, 5% fluoroethylene carbonate, 1.5% tris(trimethyl)silyl phosphate, 0.6% methanedisulfonic acid methylene ester, and 0.8% lithium difluorophosphate. On this basis, T5 additive and lithium dioxalate borate are added. The amount of T5 added accounts for 0.05% of the mass fraction of the electrolyte, and the amount of lithium dioxalate borate added accounts for 1.8% of the mass fraction of the electrolyte.

[0059] Example 6

[0060] The positive and negative electrode film-forming additives used in this embodiment are 0.2% vinyl sulfate, 5% fluoroethylene carbonate, 1.5% tris(trimethyl)silyl phosphate, 0.6% methanedisulfonic acid methylene ester, and 0.8% lithium difluorophosphate. On this basis, T6 additive and lithium dioxalate borate are added. The amount of T2 added accounts for 0.05% of the mass fraction of the electrolyte, and the amount of lithium dioxalate borate added accounts for 1.8% of the mass fraction of the electrolyte.

[0061] Example 7

[0062] In this embodiment, no positive and negative electrode film-forming additives and lithium borate bis(oxalate) are used, and only T1 additive is added. The amount of T1 added accounts for 0.05% of the mass fraction of the electrolyte.

[0063] Example 8

[0064] In this embodiment, no positive and negative electrode film-forming additives and lithium borate bis(oxalate) are used, and only T2 additive is added. The amount of T2 added accounts for 0.05% of the mass fraction of the electrolyte.

[0065] Example 9

[0066] In this embodiment, no positive and negative electrode film-forming additives and lithium borate bis(oxalate) are used, and only T3 additive is added. The amount of T3 added accounts for 0.05% of the mass fraction of the electrolyte.

[0067] Example 10

[0068] In this embodiment, no positive and negative electrode film-forming additives and lithium borate bisoxalate are used, and only T4 additive is added. The amount of T4 added accounts for 0.05% of the mass fraction of the electrolyte.

[0069] Embodiment 11

[0070] In this embodiment, no positive and negative electrode film-forming additives and lithium borate bis(oxalate) are used, and only T5 additive is added. The amount of T5 added accounts for 0.05% of the mass fraction of the electrolyte.

[0071] Example 12

[0072] In this embodiment, no positive and negative electrode film-forming additives and lithium borate bis(oxalate) are used, and only T6 additive is added. The amount of T6 added accounts for 0.05% of the mass fraction of the electrolyte.

[0073] Comparative Example 1

[0074] This comparative example does not add lithium bis(oxalatoborate), any conventional positive and negative electrode film-forming additives, and fluorophosphoryl-s-triazine organic compounds;

[0075] Comparative Example 2

[0076] In this comparative example, only positive and negative electrode film-forming additives and lithium borate oxalate are added, which are 0.2% vinyl sulfate, 5% fluoroethylene carbonate, 1.5% tris(trimethyl)silyl phosphate, 0.6% methanedisulfonic acid methylene ester, 0.8% lithium difluorophosphate, and 1.8% lithium borate oxalate, respectively. No fluorophosphoric acid-based triazine organic compounds are added.

[0077] The electrolytes and lithium-ion batteries of the embodiments and comparative examples were tested and their performance differences were compared using the following methods:

[0078] (1) Lithium-ion battery rate performance

[0079] The embodiments and comparative examples in this patent test the rate performance of lithium-ion batteries according to the following steps. The detailed steps are: take a lithium-ion battery with a fixed capacity, place it at room temperature 25°C, and cycle it at 2C / 2C and 5C / 5C for 100 cycles, with a voltage range of 2.0 to 3.6V, and test the first coulomb efficiency, 2C capacity retention rate, and 5C capacity retention rate of the lithium-ion battery. See Table 1 for specific data.

[0080] Table 1 Lithium-ion battery rate performance test

[0081]

[0082] Table 1 shows the first coulombic efficiency of different cells and the capacity retention rate after 100 cycles of charge and discharge at 2C and 5C rates, respectively. From the rate performance data of lithium-ion batteries in Table 1, it can be seen that when the electrolyte used in the cell does not add commonly used positive and negative electrode film-forming additives, the capacity retention rate and first efficiency of the cell after 100 cycles at 2C and 5C are low. When lithium bis(oxalateborate), commonly used positive and negative electrode film-forming additives and new film-forming additives are added, the rate performance and first efficiency of the cell are significantly improved by forming a stable interface film at the positive and negative electrodes. When the new additive is used in combination with lithium bis(oxalateborate), it can not only form a stable interface film at the interface of the positive and negative electrodes, but also absorb moisture in the electrolyte to remove water and inhibit acid, further enhancing the stability of the positive and negative electrode interface film, reducing the gas production of the battery, thereby improving the first efficiency, reducing capacity loss under rate charge and discharge, and improving battery safety.

[0083] (2) Lithium-ion battery 45°C cycle test

[0084] The embodiments and comparative examples in this patent carry out a 45°C cycle test on lithium-ion batteries according to the following steps. The detailed steps are as follows: Take a lithium-ion battery that has been fixed in capacity and place it in a constant temperature box at 45°C. In order to fully reduce the temperature of the battery, control the shelf time of the battery to ensure that it is more than 1 hour. Then charge it with a constant current and constant voltage of 1C, with a cut-off voltage of 3.6V and a cut-off current of 0.05C. Then discharge it to 2.0V with a constant current of 1C. Perform charge and discharge cycles on the battery according to the above steps, and record the discharge capacity retention rate after 1000 and 2000 cycles. The discharge capacity retention rate of the battery after 400 and 800 cycles is calculated by dividing the discharge capacity of the battery after 400 and 800 cycles by the discharge capacity of the battery in the first cycle. See Table 2 for specific test data.

[0085] Table 2 Lithium-ion battery 45℃ cycle test

[0086]

[0087] (3) Lithium-ion battery storage test at 60°C

[0088] The steps of the high temperature storage performance test of the battery cell in the embodiments and comparative examples of this patent are as follows: discharge the fixed capacity battery cell to 2.0V at 1C constant current, set aside for 5 minutes, and then charge to 3.6V at 1C constant current and constant voltage, with a cut-off current of 0.05C. The battery was placed in a constant temperature box at 60°C and stored for 30 days, 60 days, 90 days, 120 days, and 150 days respectively. After the battery reaches the specified storage date, take out the battery cell, connect it to the battery test cabinet, discharge it to 2.0V at 1C constant current, and then charge it at 1C constant current and constant voltage. The 1C constant current discharge process is repeated 3 times. Finally, the discharge capacity recovery rate of the battery cell is obtained, and the relevant test results are shown in Table 3.

[0089] Table 3 Lithium-ion battery 60℃ storage test

[0090]

[0091]

[0092] Table 3 shows the capacity recovery rate of batteries filled with different electrolytes at different storage times. Compared with lithium-ion batteries without conventional electrolyte additives, the high-temperature storage performance of lithium-ion batteries is significantly improved after adding lithium bis(oxalatoborate), vinyl sulfate, fluoroethylene carbonate, tris(trimethyl)silyl phosphate, methanedisulfonic acid methylene ester, and lithium difluorophosphate to the battery. At the same time, on this basis, after the additional addition of T1-T6 electrolyte additives, the high-temperature storage capacity recovery rate of lithium-ion batteries is further improved, especially with the addition of T5 electrolyte additives. Comparing the high-temperature storage data of the embodiments and comparative examples, the T5 electrolyte additive has a higher degree of improvement in the high-temperature storage of the battery than T1, T2, T3, T4, and T6.

[0093] (4) DCIR test of lithium-ion battery at 25℃ and 50% SOC

[0094] The battery cells in the embodiments and comparative examples of this patent are tested for DCIR at 50% SOC at 25°C according to the following steps. First, the battery is constant-capacity and the discharge capacity is determined by 1C constant-current constant-voltage charging and 1C constant-current discharging. Then, the discharge time at 50% SOC is calculated based on the discharge capacity, and the capacity of the battery is adjusted to 50% SOC. After standing for one hour, the battery cell is charged and discharged for 20 seconds with a 3C pulse current. Based on the change in voltage, the DCIR of the battery is calculated. Relevant test results are shown in Table 4.

[0095] Table 4 DCIR test of lithium-ion battery at 25℃ and 50% SOC

[0096] Group DCIR / Ω Group DCIR / Ω Group DCIR / Ω Example 1 0.822 Example 6 0.851 Embodiment 11 0.951 Example 2 0.843 Example 7 0.922 Example 12 0.966 Example 3 0.833 Example 8 0.955 Comparative Example 1 0.866 Example 4 0.832 Example 9 0.932 Comparative Example 2 0.853 Example 5 0.812 Example 10 0.920

[0097] Table 4 lists the DCIR of the example and comparative example batteries. In comparative example 1, no film-forming additives or lithium dioxalate borate lithium salt were added, and the lithium-ion battery showed a higher DCIR, which indicates that the interface film formed at the interface where the positive and negative electrodes of the lithium-ion battery contact the electrolyte is thicker. The addition of conventional film-forming additives, lithium dioxalate borate lithium salt or a novel fluoro-substituted fluorophosphate-based triazine organic compound can reduce the DCIR of the lithium-ion battery by forming a stable, dense and thin interface film. When lithium dioxalate borate is used in combination with a novel fluoro-substituted fluorophosphate-based triazine organic compound, the DCIR of the lithium-ion battery is significantly reduced.

[0098] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the above embodiments do not limit the present invention in any form, and any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.

Claims

1. An electrolyte for a high-power lithium-ion battery, characterized in that: The invention comprises: a lithium salt, an organic solvent and an additive, wherein the lithium salt comprises lithium dioxalate borate, and the additive comprises a fluorophosphoryl-s-triazine organic compound; The fluorinated fluorophosphoryl-s-triazine organic compound has a structure shown in the following formula: Wherein, R1 is selected from one or more of hydrogen, halogen, substituted or unsubstituted alkane, alkene, alkyne, aromatic group, carbonate group, phosphate group, sulfonate group, sulfate group, fluorophosphate group, borate group, siloxy group, cyanoethoxy group and isocyanate group.

2. The electrolyte of the high-power lithium-ion battery according to claim 1, characterized in that: R1 is selected from one or more of cyanoethoxy, phosphate, sulfate, sulfonyl, oxalate and siloxy.

3. The electrolyte of the high-power lithium-ion battery according to claim 1, characterized in that: The fluorinated fluorophosphoryl-s-triazine organic compound is one of the following formulas:

4. The electrolyte of the high-power lithium-ion battery according to claim 1, characterized in that: The added amount of the fluorophosphoric acid-based triazine organic compound accounts for 0.01%-0.1% of the total mass of the electrolyte.

5. The electrolyte of the high-power lithium-ion battery according to claim 4, characterized in that: The added amount of the fluorophosphoric acid-based triazine organic compound accounts for 0.01%-00.05% of the total mass of the electrolyte.

6. The electrolyte of the high-power lithium-ion battery according to claim 1, characterized in that: The organic solvent comprises one or more of dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, methyl acetate, ethyl acetate, ethyl propionate, propyl propionate, fluorobenzene, fluoroethylene carbonate, fluoroethyl methyl carbonate, fluorodimethyl carbonate, and fluorodiethyl carbonate; The lithium salt further comprises one or more of lithium hexafluorophosphate, lithium bis(trifluorosulfonyl imide), lithium bis(oxalatoborate), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium difluorophosphate, lithium bis(trifluoromethanesulfonyl imide), lithium perchlorate, and lithium hexafluoroarsenate.

7. The electrolyte of the high-power lithium-ion battery according to claim 1, characterized in that: The amount of lithium bis(oxalatoborate) added is 0.03-4% of the total mass of the electrolyte.

8. The electrolyte of the high-power lithium-ion battery according to claim 1, characterized in that: The additives also include positive and negative electrode film-forming additives; The positive and negative electrode film-forming additives include one or more of vinylene carbonate, fluoroethylene carbonate, methylene disulfonate, 1,3-propane sultone, vinyl sulfate, tris(trimethyl)silyl phosphate, lithium tetrafluorooxalate phosphate, lithium difluorooxalate borate, and lithium difluorophosphate.

9. The electrolyte of the high-power lithium-ion battery according to claim 8, characterized in that: The positive electrode film-forming additives are fluoroethylene carbonate, vinyl sulfate, lithium difluorophosphate, methylene disulfonate and tris(trimethyl)silyl phosphate, wherein the amount of fluoroethylene carbonate added accounts for 3%-10% of the total mass of the electrolyte, the amount of vinyl sulfate added accounts for 0.5-3% of the total mass of the electrolyte, the amount of lithium difluorophosphate added accounts for 0.3%-1.2% of the total mass of the electrolyte, the amount of methylene disulfonate added accounts for 0.2%-3% of the total mass of the electrolyte, and the amount of tris(trimethyl)silyl phosphate added accounts for 0.3%-2% of the total mass of the electrolyte.

10. A high-power lithium-ion battery, characterized in that: The invention comprises: a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte as claimed in any one of claims 1 to 9.

Citation Information

Cited By

  • Non-aqueous electrolyte, lithium ion battery, battery module, battery pack and electric device

    CN119994195A