High-compressive-strength aerogel gasket for power battery cell and preparation method of high-compressive-strength aerogel gasket
By using modified ultrafine mullite fiber felt and silicon methylated silica aerogel in the power battery cell, the problem of insufficient compressive resistance is solved, and gas with high compressive strength and low thermal conductivity is achieved Gel gaskets improve the safety of electric vehicle batteries.
Patent Information
- Application Number
- CN202411084910.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-12-01
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
AI Technical Summary
In the existing power battery cell fireproof and thermal insulation aerogel gaskets, the ultra-fine mullite fiber felt is insufficient to maintain the structural integrity under 1MPa preload force, resulting in an increase in thermal conductivity and unable to effectively prevent thermal runaway. spread.
Ultrafine mullite fiber felt as fiber matrix, silica aerogel was prepared by sol-gel method, and silicon methylation modification and normal pressure drying were carried out, combining polyethyl silicate and methyl triethoxylate. Base silane and alkaline silica sol are used as silicon source precursors to improve the hydrophobicity and compressive resistance of the gel framework.
The produced aerogel gasket has high compressive strength and low apparent thermal conductivity, which can improve safety in electric vehicle batteries and avoid thermal runaway spread.
Smart Images

Figure CN118983584A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of functional composite materials, and in particular to a high compressive strength aerogel gasket for a power battery cell and a preparation method thereof. Background Art
[0002] GB 18384-2020 "Safety Requirements for Electric Vehicles", GB 38032-2020 "Safety Requirements for Electric Buses" and GB38031-2020 "Safety Requirements for Power Batteries for Electric Vehicles" are three mandatory national standards that require that when thermal runaway occurs in the battery system of an electric vehicle, at least 5 minutes of escape time must be guaranteed for the driver and passengers. In order to solve the battery safety problem of electric vehicles, aerogel fireproof and heat-insulating gaskets need to be arranged between the power battery cells. Through the fireproof and heat-insulating effects of the aerogel fireproof and heat-insulating gaskets, when a single cell in the power battery module experiences thermal runaway, it can be ensured that thermal runaway will not spread to other adjacent cells within 5 minutes.
[0003] The core material of the traditional power battery cell fireproof and heat-insulating aerogel gasket is mainly made of glass fiber surface felt, pre-oxidized polyacrylonitrile needle felt or aluminum silicate ceramic fiber needle felt as the fiber matrix, and silica aerogel is in-situ compounded into the fiber pores. The core material is encapsulated with PET film or PI film, or a high molecular polymer flame-retardant coating is used on the surface of the core material, and a silicone rubber frame is compounded on the edge of the encapsulated core material to obtain a power battery cell fireproof and heat-insulating aerogel gasket. The fireproof and heat-insulating aerogel gasket between cells with a certain degree of flexibility not only plays a role in fireproofing and heat insulation when the battery is thermally runaway, but also plays a buffering and damping role during the normal operation of electric vehicles, absorbing the volume changes of the cells during battery charging and discharging and the random vibration energy generated when the electric vehicle is driving on the road.
[0004] In the prior art fireproof and heat-insulating aerogel gaskets for power battery cells, the heat insulation performance and high temperature resistance of the fiber matrix used for composite aerogel need to be improved. Tsinghua University published a flexible mullite fiber aerogel material and its preparation method in Chinese patent CN110846741B. If the ultrafine mullite fiber felt produced by this method is used as the fiber matrix of the composite aerogel, it is different from the traditional 3-10 micron diameter aluminum silicate ceramic fiber felt. The fiber diameter of the ultrafine mullite fiber felt is 300-1000nm, so the apparent thermal conductivity of the fiber matrix is lower and the temperature resistance is higher.
[0005] However, the ultrafine mullite fiber felt produced by this method has good compressibility but insufficient pressure resistance. When assembling the battery module, a pre-tightening force of 1MPa needs to be applied to keep the battery cell in a compressed state. Therefore, the fireproof and heat-insulating gaskets between the battery cells must have sufficiently high compressive strength. The thickness compression rate of the gasket with too low compressive strength exceeds 50% under a pressure of 1MPa, and its actual thermal conductivity increases sharply, which cannot achieve the main function of preventing the spread of thermal runaway. Therefore, the ultrafine mullite fiber felt produced by this method cannot be directly used in the fireproof and heat-insulating aerogel gaskets of power battery cells. Summary of the invention
[0006] The present invention aims to overcome the above-mentioned problems existing in the fireproof and heat-insulating aerogel gaskets for power battery cells in the prior art, and provides a high compressive strength aerogel gasket for power battery cells and a preparation method thereof. Ultrafine mullite fiber felt is used as a fiber matrix, and a normal pressure drying method is adopted to composite silica aerogel. By selecting the type of silicon source precursor and performing silicon methylation modification on the gel, the gasket can have high compressive strength and low apparent thermal conductivity.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions: A high compressive strength aerogel gasket for a power battery cell comprises an aerogel composite core material and a packaging film; the aerogel composite core material comprises a matrix and a silica aerogel loaded in the pores of the matrix; the matrix is an ultrafine mullite fiber felt; the silica aerogel is obtained by solvent replacement and silicon methylation modification of an alcohol gel prepared by a sol-gel method and then drying at normal pressure, and the content of SiO2 gel particles in the silica aerogel is 5 to 12 wt%.
[0008] The present invention adopts ultrafine mullite fiber felt as the fiber matrix composite silica aerogel. Compared with the ceramic fiber felt used in the battery core insulation aerogel gasket in the prior art, the ultrafine mullite fiber felt has better thermal insulation performance and temperature resistance, and is more conducive to improving the safety of electric vehicle batteries.
[0009] Preferably, the sol in the sol-gel method is prepared by adding ammonia and NH4F aqueous solution to the hydrolyzate after the silicon source precursor is mixed with ethanol and hydrochloric acid; the silicon source precursor is obtained by mixing three silicon sources: polyethyl silicate, methyltriethoxysilane and alkaline silica sol.
[0010] In order to solve the problem of insufficient compression resistance of ultrafine mullite fiber felt, the present invention adopts a mixed silicon source of three silicon sources, namely polyethyl silicate, methyltriethoxysilane, and alkaline silica sol, as a precursor, and ethanol as a solvent, and obtains a silica alcohol gel by an acid-base two-step catalytic method, and then the alcohol gel is subjected to solvent replacement and silicon methylation modification, and then a silica aerogel is obtained by drying at normal pressure. The present invention adopts a mixed silicon source of three silicon sources, namely polyethyl silicate, methyltriethoxysilane, and alkaline silica sol, as a precursor, and adds methyltriethoxysilane to the precursor, so that Si-CH3 can be evenly distributed on the surface of the gel skeleton, thereby improving the hydrophobicity of the gel skeleton, and the gel skeleton structure is less likely to collapse and be destroyed during the normal pressure drying process; then polyethyl silicate and alkaline silica sol are added at the same time for co-hydrolysis, which is beneficial to increase the silica content in the gel, so that the aerogel gasket obtains a better compression resistance effect. In order to further improve the skeleton stability of the gel during the normal pressure drying process, the present invention performs solvent replacement on the ethanol in the alcohol gel and further performs silicon methylation modification on the gel; after the solvent replacement and silicon methylation modification, the present invention can be dried at normal pressure, avoiding the consumption and emission of a large amount of CO2 during the supercritical drying process, thereby reducing process energy consumption and cost. The gasket prepared by the present invention has high compressive strength and low apparent thermal conductivity, and is used in power battery cells to improve the safety of electric vehicle batteries.
[0011] Preferably, the mass ratio of polyethyl silicate, methyltriethoxysilane and alkaline silica sol is 2-4:1-3:1; the polyethyl silicate is Si-40, and the mass fraction of alkaline silica sol is 35-45%. Compared with Si-28 and Si-32, Si-40 is used as the silicon source, and the raw material consumption is more economical under the same SiO2 aerogel output, which can reduce the cost; and Si-40 as the silicon source can produce less ethanol byproducts than Si-28 and Si-32 as the silicon source, which is more conducive to purification.
[0012] Preferably, the concentration of hydrochloric acid is 0.5-2 mol / L, and the mass ratio of the silicon source precursor, ethanol and hydrochloric acid is 6:10-40:0.4-0.6.
[0013] Preferably, the average fiber diameter of the ultrafine mullite fiber felt is 300-1000 nm, and the volume density is 10-30 mg / cm 3 .
[0014] The present invention also provides a method for preparing the above-mentioned high compressive strength aerogel gasket for power battery cells, comprising the following steps: (1) mixing three silicon sources, namely polyethyl silicate, methyltriethoxysilane and alkaline silica sol, to obtain a silicon source precursor; (2) mixing a silicon source precursor, ethanol and hydrochloric acid, and stirring to obtain a hydrolyzate; (3) adding ammonia water and NH4F aqueous solution to the hydrolyzate, stirring and reacting to obtain a sol; (4) Under vacuum conditions, immersing a substrate in the sol, allowing the substrate to stand for gelation to form an alcohol gel on the substrate surface, thereby obtaining an alcohol gel composite core material; and continuing to stand for gelation; wherein the substrate is an ultrafine mullite fiber felt; (5) taking out the alcohol gel composite core material and placing it in a modification liquid for solvent replacement and silicon methylation modification; (6) drying the modified alcohol gel composite core material at normal pressure and baking to obtain an aerogel composite core material; (7) Encapsulating the aerogel composite core material with a packaging film to obtain the high compressive strength aerogel gasket.
[0015] Preferably, in step (1), the mass ratio of polyethyl silicate, methyltriethoxysilane and alkaline silica sol is 2-4:1-3:1; the polyethyl silicate is Si-40, and the mass fraction of alkaline silica sol is 35-45%.
[0016] Preferably, in step (2), the concentration of hydrochloric acid is 0.5-2 mol / L, the mass ratio of silicon source precursor, ethanol and hydrochloric acid is 6:10-40:0.4-0.6; and the stirring reaction time is 8-24 h.
[0017] Preferably, in step (3), the concentrations of aqueous ammonia and aqueous NH4F solution are both 0.5-2 mol / L, the mass ratio of the hydrolyzate, aqueous ammonia and aqueous NH4F solution is 41-42:1:0.1-0.3; and the stirring reaction time is 2-5 min.
[0018] Preferably, the average fiber diameter of the ultrafine mullite fiber felt in step (4) is 300-1000 nm, and the volume density is 10-30 mg / cm 3 .
[0019] Preferably, the gel time in step (4) is 8 to 10 minutes; the gel aging time is 24 to 48 hours, and the aging temperature is 25 to 50°C.
[0020] Preferably, in step (5), the components of the modified liquid include heptane, ethanol, dimethyldiethoxysilane and trimethylchlorosilane in a mass ratio of 35-45:15-25:15-25:15-25. Dimethyldiethoxysilane plays an aging role, further strengthening the gel skeleton, thereby improving the compressive strength of the aerogel after drying; trimethylchlorosilane can react with the hydroxyl groups on the surface of the wet gel to modify the gel surface by silyl methylation to obtain a hydrophobic surface, so that the structure of the wet gel will not collapse during the normal pressure drying process, which can ensure the structural integrity and high specific surface area of the aerogel, thereby ensuring that the aerogel gasket has a low thermal conductivity.
[0021] Preferably, the solvent replacement and silylation modification process in step (5) is carried out at least three times, each time for 12 to 24 hours.
[0022] Preferably, the normal pressure drying time in step (6) is 6 to 8 hours; the drying method is: firstly heating from room temperature to 110 to 130°C for 25 to 35 minutes, and keeping warm for 25 to 35 minutes; then heating to 145 to 155°C for 8 to 12 minutes, and keeping warm for 25 to 35 minutes.
[0023] Preferably, the packaging film described in step (7) is a PET film or a PI film; and the packaging method is hot pressing packaging.
[0024] Therefore, the present invention has the following beneficial effects: (1) Ultrafine mullite fiber felt is used as the fiber matrix composite silica aerogel. Compared with the ceramic fiber felt in the prior art, the ultrafine mullite fiber felt has better thermal insulation and temperature resistance, which is more conducive to improving the safety of electric vehicle batteries; (2) Using a mixture of three silicon sources, polyethyl silicate, methyltriethoxysilane, and alkaline silica sol, as a precursor is beneficial to improving the compressive resistance of the aerogel gasket; (3) Solvent replacement and silyl methylation modification of the alcohol gel allow the gel to be dried at normal pressure, avoiding the consumption and emission of large amounts of CO2 during the supercritical drying process, thereby reducing process energy consumption and costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 is a SEM image of the aerogel composite core material prepared in Example 1 of the present invention; Figure 2 is a SEM image of the silica aerogel on the surface of the aerogel composite core material prepared in Example 1 of the present invention; Figure 3 It is the compression deformation curve of the aerogel gasket in the embodiment of the present invention and the comparative example. DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with specific implementation methods.
[0027] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments, unless otherwise specified, are conventional methods in the art.
[0028] Overall embodiment: A method for preparing the above-mentioned high compressive strength aerogel gasket for power battery cells comprises the following steps: (1) mixing three silicon sources, namely polyethyl silicate, methyltriethoxysilane and alkaline silica sol, to obtain a silicon source precursor; (2) mixing a silicon source precursor, ethanol and hydrochloric acid, and stirring to obtain a hydrolyzate; (3) adding ammonia water and NH4F aqueous solution to the hydrolyzate, stirring and reacting to obtain a sol; (4) Under vacuum conditions, immersing a substrate in the sol, allowing the substrate to stand for gelation to form an alcohol gel on the substrate surface, thereby obtaining an alcohol gel composite core material; and continuing to stand for gelation; wherein the substrate is an ultrafine mullite fiber felt; (5) taking out the alcohol gel composite core material and placing it in a modification liquid for solvent replacement and silicon methylation modification; (6) drying the modified alcohol gel composite core material at normal pressure and baking to obtain an aerogel composite core material; (7) Encapsulating the aerogel composite core material with a packaging film to obtain the high compressive strength aerogel gasket.
[0029] As a specific implementation, in step (1), the mass ratio of polyethyl silicate, methyltriethoxysilane and alkaline silica sol is 2-4:1-3:1; the polyethyl silicate is Si-40, and the mass fraction of alkaline silica sol is 35-45%.
[0030] As a specific implementation manner, the concentration of hydrochloric acid in step (2) is 0.5-2 mol / L, the mass ratio of silicon source precursor, ethanol and hydrochloric acid is 6:10-40:0.4-0.6; and the stirring reaction time is 8-24 hours.
[0031] As a specific implementation, in step (3), the concentrations of ammonia water and NH4F aqueous solution are both 0.5-2 mol / L, the mass ratio of the hydrolyzate, ammonia water and NH4F aqueous solution is 41-42:1:0.1-0.3; and the stirring reaction time is 2-5 min.
[0032] As a specific embodiment, the average fiber diameter of the ultrafine mullite fiber felt described in step (4) is 300-1000 nm, and the volume density is 10-30 mg / cm 3 .
[0033] As a specific implementation manner, in step (4), the gel time is 8 to 10 minutes; the gel aging time is 24 to 48 hours, and the aging temperature is 25 to 50°C.
[0034] As a specific implementation, in step (5), the components of the modifying liquid include heptane, ethanol, dimethyldiethoxysilane and trimethylchlorosilane in a mass ratio of 35-45:15-25:15-25:15-25.
[0035] As a specific implementation, the solvent replacement and silylation modification process in step (5) is carried out at least 3 times, each time for 12 to 24 hours.
[0036] As a specific implementation method, the normal pressure drying time in step (6) is 6 to 8 hours; the drying method is: first, heating from room temperature to 110 to 130° C. for 25 to 35 minutes, and keeping warm for 25 to 35 minutes; then heating to 145 to 155° C. for 8 to 12 minutes, and keeping warm for 25 to 35 minutes.
[0037] As a specific implementation, the packaging film described in step (7) is a PET film or a PI film; and the packaging method is hot pressing packaging.
[0038] Embodiment 1: A method for preparing a high compressive strength aerogel gasket for a power battery cell comprises the following steps: (1) mixing three silicon sources, polyethyl silicate Si-40, methyltriethoxysilane, and 40 wt % alkaline silica sol (Aladdin) in a mass ratio of 3:2:1 to obtain a silicon source precursor; (2) mixing a silicon source precursor, ethanol and 1 mol / L hydrochloric acid in a mass ratio of 6:35:0.5, stirring and reacting for 12 hours to obtain a hydrolyzate; (3) adding 1 mol / L ammonia water and 1 mol / L NH4F aqueous solution to the hydrolyzate, wherein the mass ratio of the hydrolyzate, ammonia water and NH4F aqueous solution is 41.5:1:0.2, and stirring the mixture for 2 min to obtain a sol; (4) Prepared according to the method in Example 1 of patent CN110846741B, a volume density of 22 mg / cm 3 , the room temperature thermal conductivity is 0.032 W·m -1 ·K -1 , ultrafine mullite fiber felt with an average fiber diameter of 0.6 μm; (5) placing the ultrafine mullite fiber felt in a vacuum tank, turning on the vacuum pump, pumping to a gauge pressure of -0.05 MPa, closing the vacuum pump and the vacuum pump inlet valve, sucking the sol obtained in step (3) into the vacuum tank, so that the sol liquid surface completely immerses the upper surface of the ultrafine mullite fiber felt, and allowing the ultrafine mullite fiber felt to stand for 10 minutes to form an alcohol gel on the surface of the ultrafine mullite fiber felt to obtain an alcohol gel composite core material; heating the alcohol gel to 50° C. and keeping it at this temperature for 24 hours to age the gel; (6) The alcohol gel composite core material is taken out from the vacuum tank, and the floating glue on the surface of the core material is removed with a plastic scraper, and then the core material is placed in a container containing a modification liquid, and heated to 50°C for solvent replacement and silicon methylation modification, and the core materials are isolated by a guide net; the above solvent replacement and silicon methylation modification process is repeated 3 times, each time for 24 hours; the components of the modification liquid include heptane, ethanol, dimethyldiethoxysilane and trimethylchlorosilane in a mass ratio of 40:20:20:20; (7) placing the modified alcohol gel composite core material in a fume hood and spreading it out, opening the fume hood, and ventilating it at room temperature for 8 hours to obtain a substantially dry aerogel core material; (8) The substantially dried aerogel core material is dried in an oven by the following drying procedure: first, the temperature is raised from room temperature to 120° C. in 30 minutes and kept at this temperature for 30 minutes; then, the temperature is raised to 150° C. in 10 minutes and kept at this temperature for 30 minutes. After being taken out, an aerogel composite core material is obtained. In the aerogel prepared in this embodiment, the content of SiO2 gel particles is 5 wt %. The aerogel composite core material is subjected to SEM tests of different proportions. The results are as follows: Figure 1 and Figure 2 As shown in; (9) cutting the aerogel composite core material with a packaging film, and performing hot-press packaging on a hot-pressing molding machine using a PET film to obtain the high compressive strength aerogel gasket; (10) Add a silicone rubber frame to the high compressive strength aerogel gasket.
[0039] Embodiment 2: A method for preparing a high compressive strength aerogel gasket for a power battery cell comprises the following steps: (1) mixing three silicon sources, polyethyl silicate Si-40, methyltriethoxysilane, and 40 wt % alkaline silica sol (Aladdin) in a mass ratio of 3:2:1 to obtain a silicon source precursor; (2) mixing a silicon source precursor, ethanol and 1 mol / L hydrochloric acid in a mass ratio of 6:20.5:0.5, stirring and reacting for 12 hours to obtain a hydrolyzate; (3) adding 1 mol / L ammonia water and 1 mol / L NH4F aqueous solution to the hydrolyzate, wherein the mass ratio of the hydrolyzate, ammonia water and NH4F aqueous solution is 41.5:1:0.2, and stirring the mixture for 2 min to obtain a sol; (4) Prepared according to the method in Example 1 of patent CN110846741B, a volume density of 22 mg / cm 3 , the room temperature thermal conductivity is 0.032 W·m -1 ·K -1 , ultrafine mullite fiber felt with an average fiber diameter of 0.6 μm; (5) placing the ultrafine mullite fiber felt in a vacuum tank, turning on the vacuum pump, pumping to a gauge pressure of -0.05 MPa, closing the vacuum pump and the vacuum pump inlet valve, sucking the sol obtained in step (3) into the vacuum tank, so that the sol liquid surface completely immerses the upper surface of the ultrafine mullite fiber felt, and allowing the ultrafine mullite fiber felt to stand for 10 minutes to form an alcohol gel on the surface of the ultrafine mullite fiber felt to obtain an alcohol gel composite core material; heating the alcohol gel to 50° C. and keeping it at this temperature for 24 hours to age the gel; (6) The alcohol gel composite core material is taken out from the vacuum tank, and the floating glue on the surface of the core material is removed with a plastic scraper, and then the core material is placed in a container containing a modification liquid, and heated to 50°C for solvent replacement and silicon methylation modification, and the core materials are isolated by a guide net; the above solvent replacement and silicon methylation modification process is repeated 3 times, each time for 24 hours; the components of the modification liquid include heptane, ethanol, dimethyldiethoxysilane and trimethylchlorosilane in a mass ratio of 40:20:20:20; (7) placing the modified alcohol gel composite core material in a fume hood and spreading it out, opening the fume hood, and ventilating it at room temperature for 8 hours to obtain a substantially dry aerogel core material; (8) The substantially dried aerogel core material is dried in an oven by the following drying procedure: first, the temperature is raised from room temperature to 120° C. in 30 minutes and kept at this temperature for 30 minutes; then, the temperature is raised to 150° C. in 10 minutes and kept at this temperature for 30 minutes. After being taken out, an aerogel composite core material is obtained. In the aerogel prepared in this embodiment, the content of SiO2 gel particles is 8 wt%; (9) cutting the aerogel composite core material with a packaging film, and performing hot-press packaging on a hot-pressing molding machine using a PET film to obtain the high compressive strength aerogel gasket; (10) Add a silicone rubber frame to the high compressive strength aerogel gasket.
[0040] Embodiment 3: A method for preparing a high compressive strength aerogel gasket for a power battery cell comprises the following steps: (1) mixing three silicon sources, polyethyl silicate Si-40, methyltriethoxysilane, and 40 wt % alkaline silica sol (Aladdin) in a mass ratio of 3:2:1 to obtain a silicon source precursor; (2) mixing a silicon source precursor, ethanol and 1 mol / L hydrochloric acid in a mass ratio of 6:11.1:0.5, stirring and reacting for 12 hours to obtain a hydrolyzate; (3) adding 1 mol / L ammonia water and 1 mol / L NH4F aqueous solution to the hydrolyzate, wherein the mass ratio of the hydrolyzate, ammonia water and NH4F aqueous solution is 41.5:1:0.2, and stirring the mixture for 2 min to obtain a sol; (4) Prepared according to the method in Example 1 of patent CN110846741B, a volume density of 22 mg / cm 3, the room temperature thermal conductivity is 0.032 W·m -1 ·K -1 , ultrafine mullite fiber felt with an average fiber diameter of 0.6 μm; (5) placing the ultrafine mullite fiber felt in a vacuum tank, turning on the vacuum pump, pumping to a gauge pressure of -0.05 MPa, closing the vacuum pump and the vacuum pump inlet valve, sucking the sol obtained in step (3) into the vacuum tank, so that the sol liquid surface completely immerses the upper surface of the ultrafine mullite fiber felt, and allowing the ultrafine mullite fiber felt to stand for 10 minutes to form an alcohol gel on the surface of the ultrafine mullite fiber felt to obtain an alcohol gel composite core material; heating the alcohol gel to 50° C. and keeping it at this temperature for 24 hours to age the gel; (6) The alcohol gel composite core material is taken out from the vacuum tank, and the floating glue on the surface of the core material is removed with a plastic scraper, and then the core material is placed in a container containing a modification liquid, and heated to 50°C for solvent replacement and silicon methylation modification, and the core materials are isolated by a guide net; the above solvent replacement and silicon methylation modification process is repeated 3 times, each time for 24 hours; the components of the modification liquid include heptane, ethanol, dimethyldiethoxysilane and trimethylchlorosilane in a mass ratio of 40:20:20:20; (7) placing the modified alcohol gel composite core material in a fume hood and spreading it out, opening the fume hood, and ventilating it at room temperature for 8 hours to obtain a substantially dry aerogel core material; (8) The substantially dried aerogel core material is dried in an oven by the following drying procedure: first, the temperature is raised from room temperature to 120° C. in 30 minutes and kept at this temperature for 30 minutes; then, the temperature is raised to 150° C. in 10 minutes and kept at this temperature for 30 minutes. After taking out, an aerogel composite core material is obtained. In the aerogel prepared in this embodiment, the content of SiO2 gel particles is 12 wt%; (9) cutting the aerogel composite core material with a packaging film, and performing hot-press packaging on a hot-pressing molding machine using a PET film to obtain the high compressive strength aerogel gasket; (10) Add a silicone rubber frame to the high compressive strength aerogel gasket.
[0041] Comparative Example 1: In Comparative Example 1, the surface of the ultrafine mullite fiber felt is not composited with silica aerogel.
[0042] Comparative Example 2: A method for preparing a high compressive strength aerogel gasket for a power battery cell comprises the following steps: (1) polyethyl silicate Si-40, ethanol and 1 mol / L hydrochloric acid were mixed in a mass ratio of 6:35:0.5, and stirred for reaction for 12 hours to obtain a hydrolyzate; (2) adding 1 mol / L ammonia water and 1 mol / L NH4F aqueous solution to the hydrolyzate, wherein the mass ratio of the hydrolyzate, ammonia water and NH4F aqueous solution is 41.5:1:0.2, and stirring for 2 min to obtain a sol; (3) Prepared according to the method in Example 1 of patent CN110846741B, a volume density of 22 mg / cm 3 , the room temperature thermal conductivity is 0.032 W·m -1 ·K -1 , ultrafine mullite fiber felt with an average fiber diameter of 0.6 μm; (4) placing the ultrafine mullite fiber felt in a vacuum tank, turning on the vacuum pump, pumping to a gauge pressure of -0.05 MPa, closing the vacuum pump and the vacuum pump inlet valve, sucking the sol obtained in step (2) into the vacuum tank, so that the sol liquid surface completely immerses the upper surface of the ultrafine mullite fiber felt, and allowing the ultrafine mullite fiber felt to stand for 10 minutes to form an alcohol gel on the surface of the ultrafine mullite fiber felt to obtain an alcohol gel composite core material; heating the alcohol gel to 50° C. and keeping it at this temperature for 24 hours to age the gel; (5) taking the alcohol gel composite core material out of the vacuum tank, using a plastic scraper to remove the floating glue on the surface of the core material, and then placing the core material in a container containing a modification liquid, heating it to 50°C for solvent replacement and silicon methylation modification, and isolating the core materials with a guide net; the above solvent replacement and silicon methylation modification process is repeated 3 times, each time for 24 hours; the components of the modification liquid include heptane, ethanol, dimethyldiethoxysilane and trimethylchlorosilane in a mass ratio of 40:20:20:20; (6) placing the modified alcohol gel composite core material in a fume hood and spreading it out, opening the fume hood, and ventilating it at room temperature for 8 hours to obtain a substantially dry aerogel core material; (7) The substantially dried aerogel core material is dried in an oven by the following drying procedure: first, the temperature is raised from room temperature to 120° C. in 30 minutes and kept at this temperature for 30 minutes; then, the temperature is raised to 150° C. in 10 minutes and kept at this temperature for 30 minutes. After being taken out, an aerogel composite core material is obtained. In the aerogel prepared in this embodiment, the content of SiO2 gel particles is 5 wt %. The aerogel composite core material is subjected to SEM tests of different proportions. The results are as follows: Figure 1 and Figure 2 As shown in; (8) cutting the aerogel composite core material with a packaging film, and performing hot-press packaging on a hot-pressing molding machine using a PET film to obtain the high compressive strength aerogel gasket; (9) Add a silicone rubber frame to the high compressive strength aerogel gasket.
[0043] Comparative Example 3: A method for preparing a high compressive strength aerogel gasket for a power battery cell comprises the following steps: (1) Methyltriethoxysilane, ethanol and 1 mol / L hydrochloric acid were mixed in a mass ratio of 6:35:0.5, and stirred for reaction for 12 hours to obtain a hydrolyzate; (2) adding 1 mol / L ammonia water and 1 mol / L NH4F aqueous solution to the hydrolyzate, wherein the mass ratio of the hydrolyzate, ammonia water and NH4F aqueous solution is 41.5:1:0.2, and stirring for 2 min to obtain a sol; (3) Prepared according to the method in Example 1 of patent CN110846741B, a volume density of 22 mg / cm 3 , the room temperature thermal conductivity is 0.032 W·m -1 ·K -1 , ultrafine mullite fiber felt with an average fiber diameter of 0.6 μm; (4) placing the ultrafine mullite fiber felt in a vacuum tank, turning on the vacuum pump, pumping to a gauge pressure of -0.05 MPa, closing the vacuum pump and the vacuum pump inlet valve, sucking the sol obtained in step (2) into the vacuum tank, so that the sol liquid surface completely immerses the upper surface of the ultrafine mullite fiber felt, and allowing the ultrafine mullite fiber felt to stand for 10 minutes to form an alcohol gel on the surface of the ultrafine mullite fiber felt to obtain an alcohol gel composite core material; heating the alcohol gel to 50° C. and keeping it at this temperature for 24 hours to age the gel; (5) taking the alcohol gel composite core material out of the vacuum tank, using a plastic scraper to remove the floating glue on the surface of the core material, and then placing the core material in a container containing a modification liquid, heating it to 50°C for solvent replacement and silicon methylation modification, and isolating the core materials with a guide net; the above solvent replacement and silicon methylation modification process is repeated 3 times, each time for 24 hours; the components of the modification liquid include heptane, ethanol, dimethyldiethoxysilane and trimethylchlorosilane in a mass ratio of 40:20:20:20; (6) placing the modified alcohol gel composite core material in a fume hood and spreading it out, opening the fume hood, and ventilating it at room temperature for 8 hours to obtain a substantially dry aerogel core material; (7) The substantially dried aerogel core material is dried in an oven by the following drying procedure: first, the temperature is raised from room temperature to 120° C. in 30 minutes and kept at this temperature for 30 minutes; then, the temperature is raised to 150° C. in 10 minutes and kept at this temperature for 30 minutes. After being taken out, an aerogel composite core material is obtained. In the aerogel prepared in this embodiment, the content of SiO2 gel particles is 5 wt %. The aerogel composite core material is subjected to SEM tests of different proportions. The results are as follows: Figure 1 and Figure 2 As shown in; (8) cutting the aerogel composite core material with a packaging film, and performing hot-press packaging on a hot-pressing molding machine using a PET film to obtain the high compressive strength aerogel gasket; (9) Add a silicone rubber frame to the high compressive strength aerogel gasket.
[0044] Comparative Example 4: A method for preparing a high compressive strength aerogel gasket for a power battery cell comprises the following steps: (1) 40 wt % alkaline silica sol (Aladdin), ethanol and 1 mol / L hydrochloric acid were mixed in a mass ratio of 6:35:0.5, and stirred for 12 h to obtain a hydrolyzate; (2) adding 1 mol / L ammonia water and 1 mol / L NH4F aqueous solution to the hydrolyzate, wherein the mass ratio of the hydrolyzate, ammonia water and NH4F aqueous solution is 41.5:1:0.2, and stirring for 2 min to obtain a sol; (3) Prepared according to the method in Example 1 of patent CN110846741B, a volume density of 22 mg / cm 3 , the room temperature thermal conductivity is 0.032 W·m -1 ·K -1 , ultrafine mullite fiber felt with an average fiber diameter of 0.6 μm; (4) placing the ultrafine mullite fiber felt in a vacuum tank, turning on the vacuum pump, pumping to a gauge pressure of -0.05 MPa, closing the vacuum pump and the vacuum pump inlet valve, sucking the sol obtained in step (2) into the vacuum tank, so that the sol liquid surface completely immerses the upper surface of the ultrafine mullite fiber felt, and allowing the ultrafine mullite fiber felt to stand for 10 minutes to form an alcohol gel on the surface of the ultrafine mullite fiber felt to obtain an alcohol gel composite core material; heating the alcohol gel to 50° C. and keeping it at this temperature for 24 hours to age the gel; (5) taking the alcohol gel composite core material out of the vacuum tank, using a plastic scraper to remove the floating glue on the surface of the core material, and then placing the core material in a container containing a modification liquid, heating it to 50°C for solvent replacement and silicon methylation modification, and isolating the core materials with a guide net; the above solvent replacement and silicon methylation modification process is repeated 3 times, each time for 24 hours; the components of the modification liquid include heptane, ethanol, dimethyldiethoxysilane and trimethylchlorosilane in a mass ratio of 40:20:20:20; (6) placing the modified alcohol gel composite core material in a fume hood and spreading it out, opening the fume hood, and ventilating it at room temperature for 8 hours to obtain a substantially dry aerogel core material; (7) The substantially dried aerogel core material is dried in an oven by the following drying procedure: first, the temperature is raised from room temperature to 120° C. in 30 minutes and kept at this temperature for 30 minutes; then, the temperature is raised to 150° C. in 10 minutes and kept at this temperature for 30 minutes. After being taken out, an aerogel composite core material is obtained. In the aerogel prepared in this embodiment, the content of SiO2 gel particles is 5 wt %. The aerogel composite core material is subjected to SEM tests of different proportions. The results are as follows: Figure 1 and Figure 2 As shown in; (8) cutting the aerogel composite core material with a packaging film, and performing hot-press packaging on a hot-pressing molding machine using a PET film to obtain the high compressive strength aerogel gasket; (9) Add a silicone rubber frame to the high compressive strength aerogel gasket.
[0045] Comparative Example 5: A method for preparing a high compressive strength aerogel gasket for a power battery cell comprises the following steps: (1) mixing two silicon sources, polyethyl silicate Si-40 and methyltriethoxysilane, in a mass ratio of 3:2 to obtain a silicon source precursor; (2) mixing a silicon source precursor, ethanol and 1 mol / L hydrochloric acid in a mass ratio of 6:35:0.5, stirring and reacting for 12 hours to obtain a hydrolyzate; (3) adding 1 mol / L ammonia water and 1 mol / L NH4F aqueous solution to the hydrolyzate, wherein the mass ratio of the hydrolyzate, ammonia water and NH4F aqueous solution is 41.5:1:0.2, and stirring the mixture for 2 min to obtain a sol; (4) Prepared according to the method in Example 1 of patent CN110846741B, a volume density of 22 mg / cm 3 , the room temperature thermal conductivity is 0.032 W·m -1 ·K -1 , ultrafine mullite fiber felt with an average fiber diameter of 0.6 μm; (5) placing the ultrafine mullite fiber felt in a vacuum tank, turning on the vacuum pump, pumping to a gauge pressure of -0.05 MPa, closing the vacuum pump and the vacuum pump inlet valve, sucking the sol obtained in step (3) into the vacuum tank, so that the sol liquid surface completely immerses the upper surface of the ultrafine mullite fiber felt, and allowing the ultrafine mullite fiber felt to stand for 10 minutes to form an alcohol gel on the surface of the ultrafine mullite fiber felt to obtain an alcohol gel composite core material; heating the alcohol gel to 50° C. and keeping it at this temperature for 24 hours to age the gel; (6) The alcohol gel composite core material is taken out from the vacuum tank, and the floating glue on the surface of the core material is removed with a plastic scraper, and then the core material is placed in a container containing a modification liquid, and heated to 50°C for solvent replacement and silicon methylation modification, and the core materials are isolated by a guide net; the above solvent replacement and silicon methylation modification process is repeated 3 times, each time for 24 hours; the components of the modification liquid include heptane, ethanol, dimethyldiethoxysilane and trimethylchlorosilane in a mass ratio of 40:20:20:20; (7) placing the modified alcohol gel composite core material in a fume hood and spreading it out, opening the fume hood, and ventilating it at room temperature for 8 hours to obtain a substantially dry aerogel core material; (8) The substantially dried aerogel core material is dried in an oven by the following drying procedure: first, the temperature is raised from room temperature to 120° C. in 30 minutes and kept at this temperature for 30 minutes; then, the temperature is raised to 150° C. in 10 minutes and kept at this temperature for 30 minutes. After being taken out, an aerogel composite core material is obtained. In the aerogel prepared in this embodiment, the content of SiO2 gel particles is 5 wt %. The aerogel composite core material is subjected to SEM tests of different proportions. The results are as follows: Figure 1 and Figure 2 As shown in; (9) cutting the aerogel composite core material with a packaging film, and performing hot-press packaging on a hot-pressing molding machine using a PET film to obtain the high compressive strength aerogel gasket; (10) Add a silicone rubber frame to the high compressive strength aerogel gasket.
[0046] The difference between Comparative Example 5 and Example 1 is that polyethyl silicate Si-40 and methyltriethoxysilane in a mass ratio of 3:2 are used as silicon source precursors, and the rest are the same as in Example 1.
[0047] The apparent thermal conductivity and the compression deformation under different pressure loads of the aerogel gaskets prepared in the above examples and comparative examples were tested. The results are shown in Tables 1 and Figure 3 as shown in .
[0048] Table 1: Aerogel gasket performance test results.
[0049] from Figure 3 As can be seen from Table 1, the aerogel cushions prepared by the method of the present invention in Examples 1 to 3 have low apparent thermal conductivity and good thermal insulation performance; they also have high compressive strength and small compression deformation under pressure load, meeting the requirements for use of power battery cells.
[0050] However, the ultrafine mullite fiber felt without silica aerogel loading in Comparative Example 1 has low compressive strength and large compression deformation under pressure load, which cannot meet the use requirements of the battery cell.
[0051] In Comparative Examples 2 to 4, a single silicon source was used to prepare silica aerogel, and in Comparative Example 5, no alkaline silica sol was added to the silicon source. The compressive strength of the aerogel gasket obtained was lower than that in Example 1, and the compression rate under a pressure of 1 MPa exceeded 50%, which could not meet the safety requirements of electric vehicle batteries.
Claims
1. A high compressive strength aerogel gasket for a power battery cell, characterized in that: It comprises an aerogel composite core material and a packaging film; the aerogel composite core material comprises a matrix and a silica aerogel loaded in the pores of the matrix; the matrix is an ultrafine mullite fiber felt; the silica aerogel is obtained by solvent replacement and silicon methylation modification of an alcohol gel prepared by a sol-gel method and then drying at normal pressure, and the content of SiO2 gel particles in the silica aerogel is 5-12wt%.
2. The high compressive strength aerogel gasket for power battery cells according to claim 1, characterized in that: The sol in the sol-gel method is prepared by adding ammonia and NH4F aqueous solution to the hydrolyzate after the silicon source precursor is mixed with ethanol and hydrochloric acid; the silicon source precursor is obtained by mixing three silicon sources: polyethyl silicate, methyltriethoxysilane, and alkaline silica sol.
3. The high compressive strength aerogel gasket for power battery cells according to claim 2, characterized in that: The mass ratio of polyethyl silicate, methyltriethoxysilane and alkaline silica sol is 2-4:1-3:1; the polyethyl silicate is Si-40, and the mass fraction of alkaline silica sol is 35-45%.
4. The high compressive strength aerogel gasket for power battery cells according to claim 2 or 3, characterized in that: The concentration of hydrochloric acid is 0.5~2 mol / L, and the mass ratio of the silicon source precursor, ethanol and hydrochloric acid is 6:10~40:0.4~0.
6.
5. The high compressive strength aerogel gasket for power battery cells according to claim 1, characterized in that: The average fiber diameter of the ultrafine mullite fiber felt is 300-1000 nm, and the volume density is 10-30 mg / cm 3 .
6. A method for preparing a high compressive strength aerogel gasket for a power battery cell as claimed in any one of claims 1 to 5, characterized in that: The steps include: (1) Mixing three silicon sources, namely, polyethyl silicate, methyltriethoxysilane, and alkaline silica sol, to obtain a silicon source precursor; (2) mixing a silicon source precursor, ethanol and hydrochloric acid, and stirring to react to obtain a hydrolyzate; (3) adding ammonia water and NH4F aqueous solution to the hydrolyzate, stirring and reacting to obtain a sol; (4) Under vacuum conditions, immersing a substrate in the sol, allowing the substrate to stand for gelation to form an alcohol gel on the surface of the substrate, thereby obtaining an alcohol gel composite core material; and continuing to stand for gelation; wherein the substrate is an ultrafine mullite fiber felt; (5) taking out the alcohol gel composite core material and placing it in a modification liquid for solvent replacement and silicon methylation modification; (6) drying the modified alcohol gel composite core material at normal pressure and baking to obtain an aerogel composite core material; (7) Encapsulating the aerogel composite core material with a packaging film.
7. The preparation method according to claim 6, characterized in that: In step (3), the concentrations of aqueous ammonia and aqueous NH4F solution are both 0.5-2 mol / L, and the mass ratio of hydrolyzate, aqueous ammonia and aqueous NH4F solution is 41-42:1:0.1-0.3; the stirring reaction time is 2-5 min.
8. The preparation method according to claim 6, characterized in that: In step (4), the standing gel time is 8 to 10 minutes; the gel aging time is 24 to 48 hours, and the aging temperature is 25 to 50°C.
9. The preparation method according to claim 6, characterized in that: In step (5), the components of the modification liquid include heptane, ethanol, dimethyldiethoxysilane and trimethylchlorosilane in a mass ratio of 35-45:15-25:15-25:15-25; the solvent replacement and silylation modification process is carried out at least 3 times, each time for 12-24 hours.
10. The preparation method according to claim 6, characterized in that: The normal pressure drying time in step (6) is 6 to 8 hours. The drying method is: first, heating from room temperature to 110 to 130°C for 25 to 35 minutes, and keeping warm for 25 to 35 minutes; then heating to 145 to 155°C for 8 to 12 minutes, and keeping warm for 25 to 35 minutes.
Citation Information
Cited By
Silicon dioxide aerogel heat insulation pad, and preparation method therefor and use thereof
WO2026157615A1