Thin film type circulator chip and preparation method thereof

By setting a compatible layer on the ferrite substrate of the thin-film ring chip, the adhesion between the metal layer and the substrate is improved, and the problem of the metal layer being easily fall off under heating or external force is solved, thereby achieving a more stable film layer structure and electrical performance.

CN118983630APending Publication Date: 2024-11-19GUANGZHOU AURORA TECHNOLOGIES CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411059959.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Under the action of heating or external force, the metal film layer is prone to bubble, peeling and falling off, resulting in insufficient adhesion.

Method used

The compatible layer is provided on the surface of the ferrite substrate, including a FeCoNi alloy layer, a FeCo alloy layer, a FeNi alloy layer or a CoNi alloy layer. The compatible layer, a base layer and a metal seed layer are deposited by physical vapor deposition method to improve the metal layer and the substrate adhesion.

Benefits of technology

The adhesion between the metal film layer and the ferrite matrix is ​​significantly improved, and the bubble, peeling and falling off of the metal layer under the action of heating treatment or external forces is avoided, ensuring the stability and electrical performance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983630A_ABST
    Figure CN118983630A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of thin film type circulator chips, and particularly relates to a thin film type circulator chip and a preparation method thereof. The thin film type circulator chip provided by the invention comprises a ferrite substrate, and a compatible layer, a base layer, a metal seed layer and a metal layer which are sequentially arranged on the surface of the ferrite substrate of the circulator chip, the compatible layer comprises one or more of a FeCoNi alloy layer, a FeCo alloy layer, a FeNi alloy layer and a CoNi alloy layer. The compatible layer is arranged on the surface of the ferrite substrate, the components of the compatible layer and the ferrite substrate are similar by reasonably selecting the material of the compatible layer, and the adhesive force of the compatible layer and the ferrite substrate is improved, so that the adhesive force of the metal layer and the ferrite substrate is finally improved. Therefore, after the thin film type circulator chip provided by the invention is subjected to heating treatment or external force action, the metal layer does not have the problems of blistering, peeling and falling off.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thin film circulator chips, and in particular relates to a thin film circulator chip and a preparation method thereof. Background Art

[0002] There are two types of processing technology for electronic components: thick film technology and thin film technology. The thick film technology processes the circuit by screen printing the electrode slurry. At present, the smallest processable line is generally 50μm, and the edge is uneven (the burr on the electrode edge is generally between 12.5 and 25μm). The circuit integration is low, the precision is poor, and the frequency of use is low. The thin film technology uses physical vapor deposition to prepare a metal film on the surface of the substrate, and combines photolithography and etching technology to process the circuit. The line precision is high, the smallest processable line is 10μm, the line edge is smooth (the burr on the electrode edge is generally less than 0.1μm), the circuit integration is high, and the frequency of use is high. However, the products produced by the thin film process are prone to weak film layer strength, which is specifically manifested in blistering of the metal film layer when heated at a certain temperature (such as Figure 1 As shown), or the metal film layer peels off under the action of a certain external force (as shown Figure 2 shown).

[0003] Circulator chips are widely used electronic components made of ferrite substrates. Their notable features are that they have three ports and can transmit electrical signals in one direction, such as Figure 6 The schematic diagram of signal transmission of the circulator chip shown in the figure shows that the signals from 1 to 2, from 2 to 3 and from 3 to 1 are conductive, and conversely, the signals from 2 to 1, from 1 to 3 and from 3 to 2 are isolated. Since the signal transmission forms a closed loop, the component is called a circulator chip (it is not called a circulator because of its ring or quasi-ring shape).

[0004] Thin-film circulator chips, which are prepared by physical vapor deposition of metal films through processes such as photolithography and etching, are an important branch of the circulator chip technology field.

[0005] The film structure of the thin film circulator chip prepared by the conventional processing technology is as follows: Figure 3As shown, metal materials such as Ti, TiW or NiCr are generally used as the base layer for physical vapor deposition of metal thin films on the surface of ferrite substrates, that is, Ti, TiW or NiCr are deposited on the surface of ferrite substrates. Then, a Ni layer, a Cu layer or a Ni+Cu layer is deposited on the surface of the base layer, and then an Au layer or an Ag layer is deposited. For conventional ceramic materials, such as BaTiO3, SrTiO3 and MgTiO3, ceramic substrates with titanate as the main component, Ti, TiW or NiCr is used as the base layer. Ti, TiW or NiCr has good compatibility with the substrate, and the stress between the base layer of the metal film and the substrate is small. When the metal film is deposited on the surface of the substrate, good adhesion can be obtained. However, since ferrite materials are mainly composed of elements such as Fe, Co, and Ni, Ti, TiW, or NiCr is selected as the base material for physical vapor deposition. The compatibility between Ti, TiW, or NiCr and the substrate is poor, and the stress between the base layer of the metal film and the substrate is large, so the adhesion between the metal film layer and the ferrite substrate is poor.

[0006] When the thin film circulator chip is assembled in the circuit, it must be heated. For example, when soldering with gold-tin eutectic solder, the thin film circulator chip needs to be soldered at 300-320℃ for 60-90s. After soldering, the metal film of the thin film circulator chip has poor adhesion to the ferrite substrate, which is prone to similar Figure 1 and Figure 2 The problem of blistering and falling off of the metal film layer in the Summary of the invention

[0007] The object of the present invention is to provide a thin film circulator chip and a preparation method thereof. The thin film circulator chip provided by the present invention significantly improves the adhesion between the metal film layer and the ferrite matrix. The metal film layer of the thin film circulator chip is stable, and after heat treatment or external force, the metal layer does not have problems of blistering, peeling and falling off.

[0008] In order to achieve the above object, the present invention provides the following technical solutions:

[0009] The present invention provides a thin film circulator chip, comprising a ferrite substrate, a compatibility layer, a primer layer, a metal seed layer and a metal layer arranged in sequence on the surface of the ferrite substrate; the compatibility layer comprises one or more layers of a FeCoNi alloy layer, a FeCo alloy layer, a FeNi alloy layer and a CoNi alloy layer.

[0010] Preferably, the compatibility layer has a thickness of 0.01 to 1.0 μm.

[0011] Preferably, the primer layer includes one or more layers of a Ti layer, a TiW layer and a NiCr layer; and the thickness of the primer layer is 0.01 to 0.5 μm.

[0012] Preferably, the metal seed layer includes an Au layer or an Ag layer; and the thickness of the metal seed layer is 0.01-0.5 μm.

[0013] Preferably, the metal layer includes an Au layer or an Ag layer.

[0014] Preferably, the thin film circulator chip further comprises a transition layer disposed between the primer layer and the metal seed layer, wherein the transition layer comprises a Ni layer and / or a Cu layer; and the thickness of the transition layer is 0.5 to 5.0 μm.

[0015] The present invention provides a method for preparing the thin film circulator chip described in the above technical solution, comprising the following steps:

[0016] Using a physical vapor deposition method, a compatible layer film, a base film and a metal seed layer film are sequentially deposited on the surface of a ferrite substrate to obtain a first semi-finished product;

[0017] After coating a photoresist on the surface of the metal seed layer film of the first semi-finished product, photolithography is performed to form a pattern of a circulator chip on the surface of the first semi-finished product to obtain a patterned first semi-finished product;

[0018] Electroplating is performed on the pattern surface of the patterned first semi-finished product to obtain a metal layer film, thereby obtaining a second semi-finished product;

[0019] After removing the photoresist from the second semi-finished product, etching and cutting are performed in sequence to obtain the thin film circulator chip.

[0020] Preferably, the compatibility layer film is deposited by magnetron sputtering, and the target material used in the magnetron sputtering is an alloy target, and the alloy target includes one or more of a FeCoNi alloy target, a FeCo alloy target, a FeNi alloy target and a CoNi alloy target.

[0021] Preferably, the conditions of the magnetron sputtering include: a sputtering temperature of 100 to 400° C., and a sputtering vacuum of 0.1 to 10 Pa.

[0022] Preferably, the thickness of the metal layer film is 2.0-10 μm.

[0023] The present invention provides a thin film circulator chip, comprising a ferrite substrate, a compatibility layer, a primer layer, a metal seed layer and a metal layer sequentially arranged on the surface of the ferrite substrate; the compatibility layer comprises one or more layers of a FeCoNi alloy layer, a FeCo alloy layer, a FeNi alloy layer and a CoNi alloy layer. The present invention arranges a compatibility layer on the surface of the ferrite substrate, and by reasonably selecting the material of the compatibility layer, the composition of the compatibility layer and the ferrite substrate is similar, thereby improving the adhesion between the compatibility layer and the ferrite substrate, thereby ultimately improving the adhesion between the metal layer and the ferrite substrate. Therefore, the thin film circulator chip provided by the present invention has no blistering, peeling and shedding problems on the metal layer after heat treatment or external force.

[0024] Furthermore, in the present invention, the thickness of the compatibility layer is 0.01 to 1.0 μm. The thickness of the compatibility layer cannot be too small or too large. When the thickness of the compatibility layer is less than 0.01 μm, the compatibility layer will be discontinuous and will not have the effect of improving adhesion; when the thickness of the compatibility layer is greater than 1.0 μm, the electrical performance of the device will be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a physical picture of the metal film blistering after heating at 350℃ in the thin film process;

[0026] Figure 2 This is a physical picture of the metal film peeling off and being torn off during the bonding process in the thin film process;

[0027] Figure 3 Schematic diagram of the film structure of a thin film circulator chip prepared by conventional technology;

[0028] Figure 4 A schematic diagram of the film structure of a thin film circulator chip prepared according to an embodiment of the present invention;

[0029] Figure 5 A test image of a thin film circulator chip prepared according to an embodiment of the present invention;

[0030] Figure 6 This is a schematic diagram of signal transmission of the circulator chip;

[0031] Figure 7 This is a test photo of the thin film circulator chip prepared in Example 2;

[0032] Figure 8 This is a test photo of the thin film circulator chip prepared in Example 3;

[0033] Fig. 9 This is a test photo of the thin film circulator chip prepared in Example 4;

[0034] Fig.10This is a test photo of the thin film circulator chip prepared in Comparative Example 1;

[0035] Fig.11 This is a test photo of the thin film circulator chip prepared in Comparative Example 2;

[0036] Among them: 1 is a ferrite substrate, 2 is a base film, 3 is a transition layer film, 4 is a metal seed layer film, and 5 is a compatible layer film. DETAILED DESCRIPTION

[0037] The present invention provides a thin film circulator chip, comprising a ferrite substrate, a compatibility layer, a primer layer, a metal seed layer and a metal layer arranged in sequence on the surface of the ferrite substrate; the compatibility layer comprises one or more layers of a FeCoNi alloy layer, a FeCo alloy layer, a FeNi alloy layer and a CoNi alloy layer.

[0038] In the present invention, unless otherwise specified, all preparation raw materials / components are commercially available products well known to those skilled in the art.

[0039] Figure 4 The schematic diagram of the film layer structure of the thin film circulator chip provided by the present invention is shown below in combination with Figure 4 , the thin film circulator chip provided by the present invention is described in detail.

[0040] The thin film circulator chip provided by the present invention comprises a ferrite substrate, wherein the main components of the ferrite substrate are preferably Fe, Co and Ni.

[0041] The thin film circulator chip provided by the present invention comprises a compatibility layer arranged on the surface of the ferrite substrate. In the present invention, the compatibility layer comprises one or more layers of a FeCoNi alloy layer, a FeCo alloy layer, a FeNi alloy layer and a CoNi alloy layer, and more preferably a FeCoNi alloy layer. In a specific embodiment of the present invention, the FeCoNi alloy layer is specifically Fe 25 Co 25 Ni 50 , that is, the mass percentage of Fe element in the FeCoNi alloy layer is 25%, the mass percentage of Co element is 25%, and the mass percentage of Ni element is 50%.

[0042] In the present invention, the thickness of the compatibility layer is preferably 0.01 to 1.0 μm, more preferably 0.05 to 0.5 μm, and further preferably 0.1 to 0.25 μm. The thickness of the compatibility layer cannot be too small or too large. When the thickness of the compatibility layer is less than 0.01 μm, the compatibility layer will be discontinuous and will not have the effect of improving adhesion; when the thickness of the compatibility layer is greater than 1.0 μm, the electrical performance of the device will be reduced.

[0043] The thin film circulator chip provided by the present invention comprises a primer layer arranged on the surface of the compatible layer. In the present invention, the primer layer preferably comprises one or more layers of a Ti layer, a TiW layer and a NiCr layer, more preferably a Ti layer, a TiW layer or a NiCr layer. The thickness of the primer layer is preferably 0.01 to 0.5 μm, more preferably 0.05 to 0.4 μm, and further preferably 0.1 to 0.25 μm.

[0044] In the present invention, the thin film circulator chip preferably further comprises a transition layer disposed between the primer layer and the metal seed layer. In the present invention, the transition layer preferably comprises a Ni layer and / or a Cu layer. The thickness of the transition layer is preferably 0.5 to 5 μm, more preferably 1.0 to 4.0 μm, and further preferably 1.5 to 3.0 μm.

[0045] The thin film circulator chip provided by the present invention comprises a metal seed layer disposed on the surface of the base layer. The metal seed layer preferably comprises an Au layer or an Ag layer. The thickness of the metal seed layer is preferably 0.01 to 0.5 μm, more preferably 0.05 to 0.4 μm, and further preferably 0.1 to 0.25 μm.

[0046] The thin film circulator chip provided by the present invention comprises a metal layer arranged on the surface of the metal seed layer. The metal layer preferably comprises an Au layer or an Ag layer. The material types of the metal layer and the metal seed layer are preferably the same. When the metal seed layer is an Au layer, the metal layer is an Au layer. When the metal seed layer is an Ag layer, the metal layer is an Ag layer. The thickness of the metal layer is preferably 2.0 to 10 μm.

[0047] The present invention provides a method for preparing the thin film annular device described in the above technical solution, comprising the following steps:

[0048] Using a physical vapor deposition method, a compatible layer film, a base film and a metal seed layer film are sequentially deposited on the surface of a ferrite substrate to obtain a first semi-finished product;

[0049] After coating a photoresist on the surface of the metal seed layer film of the first semi-finished product, photolithography is performed to form a pattern of a circulator chip on the surface of the first semi-finished product to obtain a patterned first semi-finished product;

[0050] Electroplating is performed on the pattern surface of the patterned first semi-finished product to obtain a metal layer film, thereby obtaining a second semi-finished product;

[0051] After removing the photoresist from the second semi-finished product, etching and cutting are performed in sequence to obtain the thin film circulator chip.

[0052] The present invention adopts a physical vapor deposition method to sequentially deposit a compatible layer film, a primer layer film and a metal seed layer film on the surface of a ferrite substrate to obtain a first semi-finished product. In the present invention, before depositing the compatible layer film, the primer layer film and the metal seed layer film by the physical vapor deposition method, the present invention preferably performs a pretreatment on the ferrite substrate, and the pretreatment preferably includes: washing, drying and heat treating the ferrite substrate in sequence. The washing is preferably performed by an ultrasonic method or a megasonic method. The reagent used for the washing is preferably ethanol or acetone, and the ethanol is specifically preferably anhydrous ethanol, and the acetone is specifically preferably analytical pure acetone. The washing time is preferably 15 to 30 minutes. The drying is preferably performed by gas drying, and the gas used for the drying is preferably filtered compressed air or nitrogen. The temperature of the heat treatment is preferably 120 to 140°C, the time of the heat treatment is preferably 60 to 90 minutes, and the implementation method of the heat treatment is specifically preferably baking.

[0053] The present invention uses a physical vapor deposition method to deposit a compatibility layer film on the surface of a ferrite substrate. In the present invention, the deposition method of the compatibility layer film is preferably magnetron sputtering, and the target material used in the magnetron sputtering is preferably an alloy target, and the alloy target preferably includes one or more of a FeCoNi alloy target, a FeCo alloy target, a FeNi alloy target, and a CoNi alloy target, and is more preferably a FeCoNi alloy target. The FeCoNi alloy target is specifically Fe 25 Co 25 Ni 50 The alloy target, that is, the mass percentage of Fe element in the FeCoNi alloy target is 25%, the mass percentage of Co element is 25%, and the mass percentage of Ni element is 50%. The conditions of the magnetron sputtering preferably include: the sputtering temperature is preferably 100-400°C, and the sputtering vacuum is preferably 0.1-10Pa. The specific implementation method of the magnetron sputtering deposition of the compatible layer film is preferably: placing the pre-treated ferrite substrate into the cavity of the magnetron sputtering machine, and then heating it at 300-600°C for 120-180 minutes in the cavity to deposit the compatible layer film by magnetron sputtering. The deposition thickness of the compatible layer film is preferably 0.01-1.0μm.

[0054] After obtaining the compatible layer film, the present invention uses a physical vapor deposition method to deposit a base film on the surface of the compatible layer film. The deposition thickness of the base film is preferably 0.01 to 0.5 μm. In the present invention, the deposition method of the base film is preferably magnetron sputtering. The present invention has no special requirements for the specific implementation of the magnetron sputtering deposition of the base film.

[0055] After obtaining the base film, the present invention preferably further comprises depositing a transition layer film on the surface of the base film film by a physical vapor deposition method. In the present invention, the deposition thickness of the transition layer film is preferably 0.5 to 5.0 μm. In the present invention, the deposition method of the transition layer film is preferably magnetron sputtering. The present invention has no special requirements for the specific implementation method of magnetron sputtering to deposit the transition layer film.

[0056] After obtaining the base film or the transition layer film, the present invention uses a physical vapor deposition method to deposit a metal seed layer film on the surface of the base film or the transition layer film. In the present invention, the deposition thickness of the metal seed layer film is preferably 0.1 to 0.5 μm. In the present invention, the deposition method of the metal seed layer film is preferably magnetron sputtering. The present invention has no special requirements for the specific implementation of the magnetron sputtering deposition of the metal seed layer film.

[0057] After obtaining the first semi-finished product, the present invention performs photolithography after coating the surface of the metal seed layer film of the first semi-finished product with photoresist, and forms a pattern of the circulator chip on the surface of the first semi-finished product to obtain a patterned first semi-finished product. In the present invention, the photoresist is retained in a partial area of ​​the pattern of the circulator chip, and the surface of the metal seed layer film is exposed in a partial area.

[0058] After obtaining the patterned first semi-finished product, the present invention performs electroplating on the pattern surface of the patterned first semi-finished product to obtain a metal layer film to obtain a second semi-finished product. In the present invention, the thickness of the metal layer film is preferably 2.0 to 10 μm, more preferably 4.0 to 8.0 μm. The present invention has no special requirements for the specific implementation of the electroplating.

[0059] After obtaining the second semi-finished product, the present invention removes the photoresist from the second semi-finished product and then performs etching and cutting in sequence to obtain the thin film circulator chip. In the present invention, the specific implementation method of removing the photoresist is preferably washing with a degumming agent. The degumming agent is preferably acetone. After removing the photoresist, the degumming second semi-finished product is obtained. The etching preferably includes the following steps: etching the metal seed layer film, the bottom layer film and the compatible layer film of the degumming second semi-finished product in sequence. When the thin film circulator chip also includes a buffer layer transition layer, the etching preferably includes the following steps: etching the metal seed layer film, the transition layer film, the bottom layer film and the compatible layer film of the degumming second semi-finished product in sequence. The etching method of the metal seed layer film, the transition layer film and the bottom layer film is preferably wet etching or dry etching. The etching method of the compatible layer film is dry etching by plasma impact. The present invention has no special requirements for the specific implementation method of the etching. The cutting is preferably scribing.

[0060] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0061] In the following embodiments and comparative examples, the metal film adhesion test was carried out in accordance with the National Military Standard of the People's Republic of China GJB 548C-2021 "Microelectronic Device Tests and Procedures" Method 2011. The qualified standard was a tensile force value ≥ 7.6 gf and the film layer did not fall off.

[0062] Example 1

[0063] Step 1: Clean the ferrite substrate with anhydrous ethanol or analytical grade acetone for 15 to 30 minutes using an ultrasonic method or a megasonic method, and blow dry with filtered compressed air or nitrogen.

[0064] Step 2: Bake the ferrite substrate at 130°C for 80 minutes.

[0065] Step 3: Place the ferrite substrate into the chamber of the magnetron sputtering machine and heat it at 300°C for 150 minutes.

[0066] Step 4: Magnetron sputtering deposition of Fe 25 Co 25 Ni 50 Alloy thin film (sputtering temperature 300℃, sputtering vacuum degree 0.5Pa), using Fe 25 Co 25 Ni 50 Alloy target, depositing Fe on ferrite substrate 25 Co 25 Ni 50 Alloy film, thickness is 0.5μm.

[0067] Step 5: Deposit NiCr film by magnetron sputtering with a thickness of 0.1 μm.

[0068] Step 6: Deposit Ni film by magnetron sputtering with a thickness of 1.5 μm.

[0069] Step 7: Deposit Au film by magnetron sputtering, the thickness of the Au film is 0.25 μm.

[0070] Step 8: Prepare a pattern of the circulator chip on the surface of the Au film by photoresist and photolithography, where the photoresist is retained in some areas of the photoresist pattern and the surface of the Au film is exposed in some areas;

[0071] Step 9: Electroplating Au film with adhesive, the thickness of Au film layer is 4μm;.

[0072] Step 10: Stripping, clean the photoresist on the surface, and use acetone to clean the stripping.

[0073] Step 11: Etch the Au film deposited by magnetron sputtering in step 7 by dry etching.

[0074] Step 12: Etch the Au film deposited by magnetron sputtering in step 7 and the Fe film deposited in step 4 in sequence. 25 Co 25 Ni 50 Thin films above alloy films.

[0075] Step 13: Etching Fe 25 Co 25 Ni 50 Alloy film, the etching method is dry etching by plasma impact.

[0076] Step 14: Obtain a thin film circulator chip by cutting.

[0077] The thin film circulator chip prepared in this embodiment was bonded using a gold wire with a diameter of 50 μm, and an adhesion test was performed. The tensile force value was between 26 gf, and the metal film on the surface of the circulator chip did not fall off, and the adhesion was qualified.

[0078] The test sample prepared in this example was heat-dried at 350°C for 5 minutes. Figure 5 As shown, there is no blistering on the surface of the metal film.

[0079] Example 2

[0080] The preparation method is basically the same as that of Example 1, except that the alloy target material used in the fourth step is a FeCo alloy target to obtain a thin film circulator chip.

[0081] The membrane-type circulator chip prepared in this embodiment was bonded with a gold wire having a diameter of 50 μm, and the adhesion test was performed. The results are as follows: Figure 7 As shown, the tensile force value is between 20gf, the metal film on the surface of the circulator chip does not fall off, and the adhesion is qualified.

[0082] The test sample prepared in this embodiment was heat-dried at 350° C. for 5 minutes, and no blistering occurred on the surface of the metal film.

[0083] Example 3

[0084] The preparation method is basically the same as that of Example 1, except that the alloy target material used in the fourth step is a FeNi alloy target to obtain a thin film circulator chip.

[0085] The membrane-type circulator chip prepared in this embodiment was bonded with a gold wire having a diameter of 50 μm, and the adhesion test was performed. The results are as follows: Figure 8As shown, the tensile force value is between 22gf, the metal film on the surface of the circulator chip does not fall off, and the adhesion is qualified.

[0086] The sample to be tested prepared in this embodiment was heat-dried at 350° C. for 5 minutes, and no blistering occurred on the surface of the metal film.

[0087] Example 4

[0088] The preparation method is basically the same as that of Example 1, except that the alloy target material used in the fourth step is a CoNi alloy target to obtain a thin film circulator chip.

[0089] The membrane-type circulator chip prepared in this embodiment was bonded with a gold wire having a diameter of 50 μm, and the adhesion test was performed. The results are as follows: Fig. 9 As shown, the tensile force value is between 18gf, the metal film on the surface of the circulator chip does not fall off, and the adhesion is qualified.

[0090] The sample to be tested prepared in this embodiment was heat-dried at 350° C. for 5 minutes, and no blistering occurred on the surface of the metal film.

[0091] Comparative Example 1

[0092] The preparation method is basically the same as that of Example 1, except that: the Fe deposited in the fourth step 25 Co 25 Ni 50 The thickness of the alloy film was 0.005 μm, and a thin film type circulator chip was obtained.

[0093] The membrane-type circulator chip prepared in this comparative example was bonded with a gold wire having a diameter of 50 μm, and the adhesion test was performed. The results are as follows: Fig.10 As shown, the tensile force value is between 8gf, but the metal film on the surface of the circulator chip falls off and the adhesion is unqualified.

[0094] Comparative Example 2

[0095] The preparation method is basically the same as that of Example 1, except that: the Fe deposited in the fourth step 25 Co 25 Ni 50 The thickness of the alloy film was 2 μm, and a thin film type circulator chip was obtained.

[0096] The membrane-type circulator chip prepared in this comparative example was bonded with a gold wire having a diameter of 50 μm, and the adhesion test was performed. The results are as follows: Fig.11 As shown, the tensile force value is between 6.0gf, and there are samples with a tensile force value lower than 7.6gf, which means the adhesion is unqualified.

[0097] It can be seen from the above embodiments that the present invention sets a compatibility layer on the surface of the ferrite substrate, and by reasonably selecting the material of the compatibility layer, the composition of the compatibility layer and the ferrite substrate is similar, thereby improving the adhesion between the compatibility layer and the ferrite substrate, thereby ultimately improving the adhesion between the metal layer and the ferrite substrate. Therefore, the thin film circulator chip provided by the present invention is subjected to heat treatment or external force, and the metal layer does not have the problems of blistering, peeling and falling off. At the same time, in the present invention, the thickness of the compatibility layer is 0.01 to 1.0 μm. The thickness of the compatibility layer cannot be too small or too large. When the thickness of the compatibility layer is less than 0.01 μm, the compatibility layer will be discontinuous and will not have the effect of improving adhesion; when the thickness of the compatibility layer is greater than 1.0 μm, the electrical performance of the device will be reduced.

[0098] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A thin film circulator chip, characterized in that: It comprises a ferrite substrate, and a compatibility layer, a primer layer, a metal seed layer and a metal layer are sequentially arranged on the surface of the ferrite substrate; the compatibility layer comprises one or more layers of a FeCoNi alloy layer, a FeCo alloy layer, a FeNi alloy layer and a CoNi alloy layer.

2. The thin film circulator chip according to claim 1, characterized in that: The compatibility layer has a thickness of 0.01 to 1.0 μm.

3. The thin film circulator chip according to claim 1 or 2, characterized in that: The primer layer includes one or more layers of a Ti layer, a TiW layer and a NiCr layer; the thickness of the primer layer is 0.01-0.5 μm.

4. The thin film circulator chip according to claim 1 or 2, characterized in that: The metal seed layer includes an Au layer or an Ag layer; the thickness of the metal seed layer is 0.01-0.5 μm.

5. The thin film circulator chip according to claim 1 or 2, characterized in that: The metal layer includes an Au layer or an Ag layer.

6. The thin film circulator chip according to claim 1 or 2, characterized in that: The thin film circulator chip further comprises a transition layer disposed between the primer layer and the metal seed layer, wherein the transition layer comprises a Ni layer and / or a Cu layer; and the thickness of the transition layer is 0.5 to 5.0 μm.

7. The method for preparing a thin film circulator chip according to any one of claims 1 to 6, characterized in that: The following steps are involved: Using a physical vapor deposition method, a compatible layer film, a base film and a metal seed layer film are sequentially deposited on the surface of a ferrite substrate to obtain a first semi-finished product; After coating a photoresist on the surface of the metal seed layer film of the first semi-finished product, photolithography is performed to form a pattern of a circulator chip on the surface of the first semi-finished product to obtain a patterned first semi-finished product; Electroplating is performed on the pattern surface of the patterned first semi-finished product to obtain a metal layer film, thereby obtaining a second semi-finished product; After removing the photoresist from the second semi-finished product, etching and cutting are performed in sequence to obtain the thin film circulator chip.

8. The preparation method according to claim 7, characterized in that: The deposition method of the compatible layer film is magnetron sputtering, and the target material used in the magnetron sputtering is an alloy target, and the alloy target includes one or more of a FeCoNi alloy target, a FeCo alloy target, a FeNi alloy target and a CoNi alloy target.

9. The preparation method according to claim 8, characterized in that: The conditions of the magnetron sputtering include: a sputtering temperature of 100 to 400° C. and a sputtering vacuum of 0.1 to 10 Pa.

10. The preparation method according to claim 7, characterized in that: The thickness of the metal layer film is 2.0-10 μm.