PCBA processing technology

By introducing multi-layer inspection and strict production line arrangement in the PCBA processing technology, the problem of incomplete parts repair in the prior art has been solved, and the effect of improving product quality and production efficiency has been achieved.

CN118984543APending Publication Date: 2024-11-19SUZHOU YINGUANG ELECTRONIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310527425.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the existing PCBA processing technology, when the printing visual inspection and pre-furnace comparison visual inspection and subsequent IC/FCT tests and quality inspection fail, the parts are not completely repaired, resulting in the problem of low pass rate.

Method used

Multi-layer inspection and strict production line layout, including material preparation, solder paste inspection, automatic patching, reflow soldering, AOI inspection, visual confirmation, first-piece inspection, mass production, three-proof coating, wave soldering, functional testing and QA inspection ensures that when the part finds a problem, it will return directly to the previous step of the possible problem for trimming, reducing the possibility of a problem again.

Benefits of technology

Through multi-layer inspection and strict production line layout, product quality is improved, finished product production time is shortened, production efficiency is accelerated, and the pass rate of parts is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984543A_ABST
    Figure CN118984543A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of PCBA (Printed Circuit Board Assembly) processing, and discloses a PCBA processing technology which comprises the following steps: S1, firstly preparing materials, inspecting the prepared materials and then feeding; and S2, the printed solder paste is checked, then automatic surface mounting is carried out, visual inspection is carried out after automatic surface mounting is completed, if the parts do not pass the visual inspection process, the parts need to be corrected and fed back, the machine is adjusted, and the previous step is returned. According to the PCBA processing technology, the steps which possibly have problems in the production and processing of the PCBA are put forward one by one, then visual inspection is specially added, the visual inspection can be manual inspection or infrared inspection, if parts are unqualified, the parts can be directly put forward for repair, the repair is not returned to the previous step but returned to the foremost step which possibly have the problems, and the production efficiency of the PCBA is greatly improved. And the possibility that problems possibly occur again is reduced, and the purpose of improving the product quality is achieved through multi-layer inspection in cooperation with a tight and strict production line.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of PCBA processing, and in particular to a PCBA processing technology. Background Art

[0002] Printed circuit boards, also known as printed circuit boards, are important electronic components, support bodies for electronic components, and providers of circuit connections for electronic components. Because they are made using electronic printing technology, they are called "printed" circuit boards. Before the advent of printed circuit boards, the interconnection between electronic components was achieved by direct connection of wires to form a complete circuit. Now, circuit panels only exist as effective experimental tools, and printed circuit boards have become an absolute dominant position in the electronics industry.

[0003] In order for a circuit board to function, it cannot be completed with just a bare PCB. The bare board needs to be mounted, plugged in and soldered with components. This step-by-step process is called PCBA.

[0004] The basic process of the existing circuit board is material delivery - substrate baking - board loading machine - solder paste printer - printing visual inspection - high-speed placement machine - general placement machine - visual inspection before reflow soldering - reflow soldering - visual inspection before furnace comparison - installation of plug-in - wave soldering - IC / FCT test - assembly visual inspection - quality inspection - storage. For details, please refer to the attached Figure 1 In this process, the re-inspection steps are printing visual inspection, pre-furnace comparative visual inspection, and subsequent IC / FCT testing and quality inspection. If the corresponding link fails, it will return to the previous step for repair. There is a situation where the problem is not solved even after returning to the previous step, resulting in a low subsequent parts qualification rate.

[0005] It can be seen that a PCBA processing technology is needed to solve the problem that the re-inspection step in the above process mentioned in the above background technology is in the printing visual inspection and the pre-furnace comparative visual inspection as well as the subsequent IC / FCT test and quality inspection. If the corresponding link is unqualified, it will return to the previous step for rework. There is a situation where the problem is not solved even if it returns to the previous step, resulting in a low subsequent parts qualification rate. Summary of the invention

[0006] The object of the present invention is to provide a PCBA processing technology to solve the problem that the re-inspection step in the above process proposed in the above background technology is in the printing visual inspection and the pre-furnace comparative visual inspection as well as the subsequent IC / FCT test and quality inspection. If the corresponding link is unqualified, it will return to the previous step for rework. There is a situation that the problem is not solved even if it returns to the previous step, resulting in a low subsequent parts qualification rate.

[0007] In order to solve the above technical problems, the present invention provides the following technical solutions: a PCBA processing technology, comprising the following steps:

[0008] S1: Prepare materials first, check the prepared materials and then load them;

[0009] S2: Check the printed solder paste, then perform automatic placement, and perform visual inspection after the automatic placement is completed. If it fails during the visual inspection, the parts need to be calibrated and feedback to the production technology and machine adjustment is given, and then return to the previous step;

[0010] S3: The parts that pass the reflow soldering will then be visually confirmed after passing the AOI inspection. If it is confirmed that the parts do not pass, they need to be labeled as defective and repaired, and then return to the AOI inspection. The parts that pass the first piece inspection will be carried out. If they do not pass, the line will be stopped and the parts will be returned to the loading step. The parts that pass the inspection can be produced in batches.

[0011] S4: Apply three-conformal coating on the front of the part, and then install the DIP plug-in;

[0012] S5: wave soldering is performed after installation, and post-soldering and cleaning are performed after soldering;

[0013] S6: Then carry out PQC inspection. If the inspection passes, carry out functional test. If the functional test fails, the line needs to be stopped. If the functional test passes, the program can be burned. Then the reverse side is coated with three anti-corrosion coating. After the coating is completed, QA inspection is carried out. If the QA inspection fails, return to the PQA inspection step for repair.

[0014] S7: The parts can be packaged and put into storage.

[0015] Preferably, during the material inspection process in S1, the materials that need to be inspected include substrates, solder paste, plug-ins, three-proof paste and others, as well as the participating equipment and machinery.

[0016] Preferably, the solder paste in S2 comprises the following raw materials: 40-60% alloy solder powder, 2-6% activator, 5-10% thixotropic agent, 20-27% resin, 10-15% solvent and 1-5% additive, wherein the alloy solder powder is one or more of tin, silver-copper, tin-silver-bismuth, tin-copper, tin-bismuth, tin-lead and tin-lead-silver; the activator is an organic acid or an organic amine; the thixotropic agent is an amide-based paraffin of a hydroxy fatty acid; the resin is one or more combinations of rosin, phenolic resin, acrylic resin, modified epoxy resin and polyethylene glycol; the solvent is ethanol or isopropanol; and the additives include a pH regulator, a wetting agent, a flame retardant and others.

[0017] Preferably, the alloy solder powder is spherical in shape, has a small surface area and a low degree of oxidation, and the particle size of the alloy solder powder is selected to be 200-400 meshes, and includes the following preparation process:

[0018] Step 1: Select a certain proportion of raw materials and sieve out the alloy solder powder of appropriate size;

[0019] Step 2: Mix the alloy solder powder with a certain amount of resin and solvent, stir evenly, then add the heated activator and thixotropic agent to dissolve and mix, cool while stirring to precipitate the paraffin, and then add the additives to mix;

[0020] Step 3: Pour the mixed solution into a solder paste dispenser for drying, so that the solvent in the solder paste evaporates and the resin forms a solid;

[0021] Step 4: Check the fluidity and viscosity of the solder paste. If adjustment is needed, add the appropriate amount of solvent and resin again;

[0022] Step 5: Put the prepared solder paste into the refrigerator. When using, the solder paste must be taken out of the refrigerator and warmed up for at least 4 hours. After warming up, the solder paste must be stirred for 3-10 minutes before use.

[0023] Preferably, a metal scraper is used to print the solder paste in S2, and a placement machine is used for automatic placement during automatic placement. The placement machine includes a high-speed placement machine and a multi-function placement machine. The components are accurately installed in fixed positions on the printed circuit board using a program edited by the equipment, and then the placement is accurately performed. In S2, the transportation environment adopts a heating environment, which can melt the solder paste on the pad, so that the surface mount components and the PCB pad are firmly combined together through the solder paste alloy.

[0024] Preferably, the visual inspection process and visual confirmation process in S2 and S3 may be performed by manual vision or infrared vision.

[0025] Preferably, a three-proof coating machine is used in S4, and coating is performed in a selective coating manner to coat the positions that need coating.

[0026] Preferably, the step of applying conformal coating in S4 comprises:

[0027] Step 1: Clean and dry the board to remove moisture and water. Before painting, you should first brush the dust, moisture and rosin on the surface of the PCBA board to remove them so that the three-proof paint can adhere well to the surface of the circuit board:

[0028] Step 2: Choose the right brush according to the product size and layout of the components on the board, pour the conformal paint into the container, and then use the brush to apply appropriate glue evenly to the circuit board:

[0029] Step 3: When brushing, the PCBA board should be placed as flat as possible. There should be no dripping after brushing. The brushing should be flat and there should be no exposed parts. The brushing thickness should be between 0.1-0.3mm.

[0030] Preferably, the baking conditions in step 1 are: 60° C., 30-40 minutes, and it is best to apply the coating while hot after taking it out of the oven. In step 2, the coating area should be larger than the area occupied by the device to ensure that the device and the pad are fully covered. In step 3, heating can be used after coating to accelerate the curing of the coating.

[0031] Preferably, the coating operation in S4 and S6 should be carried out at a temperature not lower than 16° C. and a relative humidity lower than 75%. PCB, as a composite material, absorbs moisture, so it needs to be dehumidified. Pre-drying and vacuum drying can remove most of the moisture.

[0032] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0033] First, the present invention proposes the steps where problems may occur in the production and processing of PCBA one by one by setting up the pre-furnace visual inspection and repair steps, AOI inspection and repair steps, first-piece inspection and repair steps, QA inspection and repair steps, etc., and then specially adds visual inspection, which can be manual or infrared. If a part is unqualified, it will be directly proposed for repair. The repair does not return to the previous step, but returns to the first step where the problem may occur, and re-trim it to reduce the possibility of the problem occurring again. The purpose of improving product quality is achieved through multi-layer inspection and tight and strict production lines.

[0034] Second, the present invention realizes a tight and strict production process by arranging material preparation, material inspection, loading, solder paste printing, solder paste inspection, automatic patch, visual inspection before furnace, reflow soldering, AOI inspection, visual confirmation, first piece inspection, batch production, front three-proof coating, DIP plug-in, wave soldering, post-soldering cleaning, PQC inspection, functional testing, back three-proof coating, QA inspection and packaging and warehousing. The production steps are reasonably arranged, which can shorten the production time of finished products and speed up product production efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a flowchart of the existing PCBA board processing used for comparison in the present invention;

[0036] Figure 2 The figure is a process flow chart of the PCBA board of the present invention. DETAILED DESCRIPTION

[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] See also Figure 1-2 , a PCBA processing technology, comprising the following steps:

[0039] S1: Prepare materials first, check the prepared materials and then load them;

[0040] S2: Check the printed solder paste, then perform automatic placement, and perform visual inspection after the automatic placement is completed. If it fails during the visual inspection, the parts need to be calibrated and feedback to the production technology and machine adjustment is given, and then return to the previous step;

[0041] S3: The parts that pass the reflow soldering will then be visually confirmed after passing the AOI inspection. If it is confirmed that the parts do not pass, they need to be labeled as defective and repaired, and then return to the AOI inspection. The parts that pass the first piece inspection will be carried out. If they do not pass, the line will be stopped and the parts will be returned to the loading step. The parts that pass the inspection can be produced in batches.

[0042] S4: Apply three-conformal coating on the front of the part, and then install the DIP plug-in;

[0043] S5: wave soldering is performed after installation, and post-soldering and cleaning are performed after soldering;

[0044] S6: Then carry out PQC inspection. If the inspection passes, carry out functional test. If the functional test fails, the line needs to be stopped. If the functional test passes, the program can be burned. Then the reverse side is coated with three anti-corrosion coating. After the coating is completed, QA inspection is carried out. If the QA inspection fails, return to the PQA inspection step for repair.

[0045] S7: The parts can be packaged and put into storage.

[0046] Example 1

[0047] The solder paste in S2 includes the following raw materials: 57% alloy solder powder, 3% activator, 5% thixotropic agent, 22% resin, 10% solvent and 3% additives. The alloy solder powder is a mixed powder of silver, copper and tin-lead, the activator is an organic acid, the thixotropic agent is an amide paraffin of hydroxy fatty acid, the resin is a mixture of rosin and modified epoxy resin, the solvent is ethanol, and the additives include PH regulator, wetting agent and flame retardant.

[0048] The following steps are involved:

[0049] Step 1: Select a certain proportion of raw materials and sieve out the alloy solder powder of appropriate size;

[0050] Step 2: Mix the alloy solder powder with a certain amount of resin and solvent, stir evenly, then add the heated activator and thixotropic agent to dissolve and mix, cool while stirring to precipitate the paraffin, and then add the additives to mix;

[0051] Step 3: Pour the mixed solution into a solder paste dispenser for drying, so that the solvent in the solder paste evaporates and the resin forms a solid;

[0052] Step 4: Check the fluidity and viscosity of the solder paste. If adjustment is needed, add the appropriate amount of solvent and resin again;

[0053] Step 5: Put the prepared solder paste into the refrigerator. When using, the solder paste must be taken out of the refrigerator and warmed up for at least 4 hours. After warming up, the solder paste must be stirred for 3-10 minutes before use.

[0054] In this embodiment, more alloy solder powder and less other additives are used, so that the final solder paste product is thicker, the quality is more stable, and it is not easy to collapse or peel off the structure, which is suitable for use in larger PCBA boards.

[0055] The use of solder paste is indispensable in the patch processing technology. Solder paste is a slurry or paste formed by uniformly mixing alloy solder powder and paste flux. Solder paste is an indispensable welding material in SMT process and is widely used in reflow soldering. It is one of the more important electronic auxiliary materials in the electronics industry. Alloy solder powder is also called tin powder. It has many ingredients. The quality of solder powder directly affects the performance of solder paste. The appropriate ratio can be selected according to practical conditions; the solvent is the solvent of the flux component. It plays a uniform role in the stirring process of the paste solder and has a certain impact on the life of the paste solder; the resin mainly plays the role of improving the adhesion of the solder paste, and has the role of protecting and preventing the re-oxidation of the PCB after welding. This component plays an important role in the fixation of components; the thixotropic agent mainly adjusts the viscosity and printing performance of the cream, and plays a role in preventing tailing, adhesion and other phenomena during the printing process; the activator mainly plays the role of removing the oxides on the surface of the PCB copper film pad and the welding part of the component, and has the effect of reducing the surface tension of tin and lead; the additive is a substance with special physical and chemical properties added to meet the needs of the welding process and process environment. Due to different process conditions and requirements for the flux itself, the types and amounts of additives are also different.

[0056] Example 2

[0057] The solder paste in S2 includes the following raw materials: 40% alloy solder powder, 5% activator, 10% thixotropic agent, 27% resin, 15% solvent and 3% additives. The alloy solder powder is tin-lead-silver, the activator is organic amine, the thixotropic agent is amide paraffin of hydroxy fatty acid, the resin is a mixture of phenolic resin and acrylic resin, the solvent is isopropyl alcohol, and the additives include PH regulator and flame retardant.

[0058] The following steps are involved:

[0059] Step 1: Select a certain proportion of raw materials and sieve out the alloy solder powder of appropriate size;

[0060] Step 2: Mix the alloy solder powder with a certain amount of resin and solvent, stir evenly, then add the heated activator and thixotropic agent to dissolve and mix, cool while stirring to precipitate the paraffin, and then add the additives to mix;

[0061] Step 3: Pour the mixed solution into a solder paste dispenser for drying, so that the solvent in the solder paste evaporates and the resin forms a solid;

[0062] Step 4: Check the fluidity and viscosity of the solder paste. If adjustment is needed, add the appropriate amount of solvent and resin again;

[0063] Step 5: Put the prepared solder paste into the refrigerator. When using, the solder paste must be taken out of the refrigerator and warmed up for at least 4 hours. After warming up, the solder paste must be stirred for 3-10 minutes before use.

[0064] In this embodiment, less alloy solder powder and more resin are used, and the final solder paste product has better fluidity and melts faster in a hot environment, which is suitable for use on smaller PCBA boards.

[0065] The particle size of the alloy solder powder is selected to be 200-400 mesh. The smaller the particle size of the alloy solder powder, the greater the viscosity. If the particle size is too large, the bonding performance of the solder paste will deteriorate. If the particle size is too fine, the surface area will increase and the surface oxygen content will increase, so it is not suitable to use it.

[0066] Example 3

[0067] The solder paste in S2 includes the following raw materials: 50% alloy solder powder, 5% activator, 5% thixotropic agent, 20% resin, 12% solvent and 3% additives. The alloy solder powder is a mixed powder of tin-bismuth and tin-lead, the activator is an organic amine, the thixotropic agent is an amide paraffin of hydroxy fatty acid, the resin is a mixture of modified epoxy resin and polyethylene glycol, the solvent is isopropyl alcohol, and the additives include PH regulator, wetting agent and flame retardant.

[0068] The following steps are involved:

[0069] Step 1: Select a certain proportion of raw materials and sieve out the alloy solder powder of appropriate size;

[0070] Step 2: Mix the alloy solder powder with a certain amount of resin and solvent, stir evenly, then add the heated activator and thixotropic agent to dissolve and mix, cool while stirring to precipitate the paraffin, and then add the additives to mix;

[0071] Step 3: Pour the mixed solution into a solder paste dispenser for drying, so that the solvent in the solder paste evaporates and the resin forms a solid;

[0072] Step 4: Check the fluidity and viscosity of the solder paste. If adjustment is needed, add the appropriate amount of solvent and resin again;

[0073] Step 5: Put the prepared solder paste into the refrigerator. When using, the solder paste must be taken out of the refrigerator and warmed up for at least 4 hours. After warming up, the solder paste must be stirred for 3-10 minutes before use.

[0074] In this embodiment, a moderate alloy solder powder and a moderate resin are used, and the final solder paste product has both fluidity and stability. The melting speed in a hot environment and a normal temperature environment is comparable. It is not picky about the use occasion and is suitable for general PCBA boards.

[0075] The process of applying the three-proof paint includes the following coating methods: Dipping: It is more economical for large equipment, but the thickness after coating will be affected by factors such as dipping temperature, time, withdrawal speed, vertical flow time, whether to add air knife... and sometimes it is affected by the characteristics of some components, so dipping is not allowed; Spraying: It is more economical for small and medium-sized equipment. When using spraying, it is like spraying paint. The uniformity of coating depends on the relative movement speed, spraying position, spraying pressure, and whether there are higher parts. In addition, the bottom of the parts cannot be sprayed, and additional treatment may be required; Brushing: It is more economical for small equipment. When coating, it is easy to cause uneven coating due to the proficiency of coating skills. In addition, you should also pay attention to the problem of brush hair loss. The bottom of the parts is also more difficult to coat.

[0076] Therefore, selective coating is a more appropriate coating method, which is much more convenient than manual coating.

[0077] When applying conformal coating to PCB, all connectors, sockets, switches, heat sinks (sheets), heat dissipation areas, etc. are not allowed to be coated with conformal coating. Masking tape must be used to cover and protect them when applying. If you want to get a thicker coating, you can apply two thinner layers of coating. The second layer can only be applied after the first layer is completely dry.

[0078] While embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and alterations may be made to the embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A PCBA processing technology, characterized in that: The following steps are involved: S1: Prepare materials first, check the prepared materials and then load them; S2: Check the printed solder paste, then perform automatic placement, and perform visual inspection after the automatic placement is completed. If it fails during the visual inspection, the parts need to be calibrated and feedback to the production technology and machine adjustment is given, and then return to the previous step; S3: The parts that pass the reflow soldering will then be visually confirmed after passing the AOI inspection. If it is confirmed that the parts do not pass, they need to be labeled as defective and repaired, and then return to the AOI inspection. The parts that pass the first piece inspection will be carried out. If they do not pass, the line will be stopped and the parts will be returned to the loading step. The parts that pass the inspection can be produced in batches. S4: Apply three-conformal coating on the front of the part, and then install the DIP plug-in; S5: wave soldering is performed after installation, and post-soldering and cleaning are performed after soldering; S6: Then carry out PQC inspection. If the inspection passes, carry out functional test. If the functional test fails, the line needs to be stopped. If the functional test passes, the program can be burned. Then the reverse side is coated with three anti-corrosion coating. After the coating is completed, QA inspection is carried out. If the QA inspection fails, return to the PQA inspection step for repair. S7: The parts can be packaged and put into storage.

2. A PCBA processing technology according to claim 1, characterized in that: During the material inspection process in S1, the materials that need to be inspected include substrates, solder paste, plug-ins, three-proof paste and others, as well as the participating equipment and machinery.

3. A PCBA processing technology according to claim 1, characterized in that: The solder paste in S2 includes the following raw materials: 40-60% alloy solder powder, 2-6% activator, 5-10% thixotropic agent, 20-27% resin, 10-15% solvent, and 1-5% additives, wherein the alloy solder powder is one or more of tin, silver-copper, tin-silver-bismuth, tin-copper, tin-bismuth, tin-lead, and tin-lead-silver; the activator is an organic acid or an organic amine; the thixotropic agent is an amide-based paraffin of a hydroxy fatty acid; the resin is one or more combinations of rosin, phenolic resin, acrylic resin, modified epoxy resin, and polyethylene glycol; the solvent is ethanol or isopropanol; and the additives include a pH regulator, a wetting agent, a flame retardant, and others.

4. A PCBA processing technology according to claim 3, characterized in that: The alloy solder powder is spherical in shape, has a small surface area and a low oxidation degree, and the particle size of the alloy solder powder is selected to be 200-400 meshes, and includes the following preparation process: Step 1: Select a certain proportion of raw materials and sieve out the alloy solder powder of appropriate size; Step 2: Mix the alloy solder powder with a certain amount of resin and solvent, stir evenly, then add the heated activator and thixotropic agent to dissolve and mix, cool while stirring to precipitate the paraffin, and then add the additives to mix; Step 3: Pour the mixed solution into a solder paste dispenser for drying, so that the solvent in the solder paste evaporates and the resin forms a solid; Step 4: Check the fluidity and viscosity of the solder paste. If adjustment is needed, add the appropriate amount of solvent and resin again; Step 5: Put the prepared solder paste into the refrigerator. When using, the solder paste must be taken out of the refrigerator and warmed up for at least 4 hours. After warming up, the solder paste must be stirred for 3-10 minutes before use.

5. A PCBA processing technology according to claim 1, characterized in that: In the S2, a metal scraper is used to print the solder paste, and a placement machine is used for automatic placement. The placement machine includes a high-speed placement machine and a multi-function placement machine. The program edited by the equipment is used to accurately install the components on the fixed position of the printed circuit board, and then the placement is accurately performed. In S2, the transportation environment adopts a heating environment, which can melt the solder paste on the pad, so that the surface mount components and the PCB pad are firmly combined together through the solder paste alloy.

6. A PCBA processing technology according to claim 1, characterized in that: The visual inspection process and visual confirmation process in S2 and S3 may be performed by manual vision or infrared vision.

7. A PCBA processing technology according to claim 1, characterized in that: The S4 uses a three-proof coating machine, and adopts a selective coating method to coat the positions that need coating.

8. A PCBA processing technology according to claim 1, characterized in that: The coating of conformal coating in S4 includes: Step 1: Clean and dry the board to remove moisture and water. Before painting, you should first brush the dust, moisture and rosin on the surface of the PCBA board to remove them so that the three-proof paint can adhere well to the surface of the circuit board: Step 2: Choose the right brush according to the product size and layout of the components on the board, pour the conformal paint into the container, and then use the brush to apply appropriate glue evenly to the circuit board: Step 3: When brushing, the PCBA board should be placed as flat as possible. There should be no dripping after brushing. The brushing should be flat and there should be no exposed parts. The brushing thickness should be between 0.1-0.3mm.

9. A PCBA processing technology according to claim 8, characterized in that: The baking conditions in step 1 are: 60° C., 30-40 minutes. It is best to apply the coating while it is hot after taking it out of the oven. In step 2, the coating area should be larger than the area occupied by the device to ensure that the device and the pad are fully covered. In step 3, heating can be used after coating to accelerate the curing of the coating.

10. A PCBA processing technology according to claim 1, characterized in that: The coating operation in S4 and S6 should be carried out under the conditions of not less than 16°C and relative humidity less than 75%. PCB, as a composite material, absorbs moisture, so it is necessary to do dehumidification treatment. Pre-drying and vacuum drying can remove most of the moisture.