Wooden molded article and method for manufacturing same

By dissolving cellulose in organic acids and precipitating and thermoforming, the problem of difficulty in shape changes and great environmental impact in the molding process of wood biomass molded products is solved, and the manufacturing of wood molded products with excellent mechanical characteristics and low energy load is achieved. , reducing environmental burden.

CN118984765APending Publication Date: 2024-11-19DAICEL CORP +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202280094691.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-04-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

It is difficult for existing wood biomass molded products to change shape during the molding process, and the resin or plastic used is derived from petroleum resources, resulting in significant environmental impact and insufficient mechanical characteristics and molding processability.

Method used

By dissolving cellulose or lignocellulose in organic acids and precipitating and thermoforming with water or alkali added, a wood-formed product with high-level structures is formed, avoiding the use of synthetic polymers, achieving low energy load and low environment The burden of forming process.

Benefits of technology

A wood molded product with excellent mechanical properties was obtained, with similar strength and elastic modulus as general resins, and efficient molding of biomass was achieved under low energy conditions, reducing the burden on the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005076379090000271
    Figure BDA0005076379090000271
  • Figure BDA0005076379090000281
    Figure BDA0005076379090000281
  • Figure BDA0005076379090000291
    Figure BDA0005076379090000291
Patent Text Reader

Abstract

The main component of the wood molded article is cellulose. The wood molded article has either one or both of (1) a flexural modulus of 4000 MPa or more and (2) a flexural strength of 50 MPa or more. Wood particles for use as a wood molded article material may include cellulose, hemicellulose, and lignin. The method for producing a wood molded article comprises: a step for obtaining a solution by dissolving a cellulose-containing raw material in an organic acid; a step for adding water or an alkali to the solution to precipitate a solid component; a step for recovering the solid component; and a step for thermoforming the recovered solid content. The main component of the solid component is cellulose.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a wooden molded product and a manufacturing method thereof. Background Art

[0002] In recent years, as concerns about environmental issues have increased, there has been a demand for the development of materials derived from biomass resources to replace materials derived from petroleum resources. In particular, it is desired to utilize woody biomass that does not compete with food and does not increase carbon dioxide in the atmosphere.

[0003] As thick-walled and hard molded products using wood biomass, there are resin-injected wood made by injecting resin into wood, acetylated wood made by acetylation of wood, wood plastic (WPC), etc. Both resin-injected wood and acetylated wood require the use of wood that has been pre-processed into a specified shape, and there is a problem that the shape cannot be greatly changed when manufacturing molded products (hereinafter referred to as "formed molding"). Wood plastic (WPC) is a composite material made of wood and plastic, and is usually made of wood powder and thermoplastic plastics as raw materials. For example, WPC is made by mixing wood powder from thinning materials of cedar trees, factory waste, etc. with plastic. Such WPC can be thermoformed and can be formed into a desired shape. However, like resin-injected wood, WPC uses resin or plastic derived from petroleum resources, so it is not 100% derived from biomass, and cannot completely eliminate the adverse effects on the environment after disposal and landfill.

[0004] Regarding molded products with low environmental impact using wood biomass, research is being conducted to improve molding processability. For example, Patent Document 1 (Japanese Patent Publication No. 7-276320) discloses a wood product, which is made by alkalizing wood powder, contacting it with a substance containing an allyl group to perform an allylation treatment, and then placing the obtained allylated wood powder into a mold and heating and pressurizing it to form it.

[0005] In patent document 2 (Japanese Patent Publication No. 2005-67064), a fiber-reinforced plastic is disclosed, which contains lignocellulosic fibers whose intracellular cavities have been eliminated as reinforcing agents. In patent document 2, epoxy resin is used as a matrix resin. In patent document 3 (Japanese Patent Publication No. 2016-169382), a lignocellulosic derivative is disclosed in which the α position of the phenylpropane unit constituting lignin is modified by at least one characteristic group selected from the group consisting of acyloxy, oxy and thiol. Patent document 3 records that various synthetic polymers can be added as matrix materials to the fibers or fiber aggregates containing the lignocellulosic derivative to manufacture molded products.

[0006] In addition, there is a technique called pulp molding, which uses a mold to shape a fiber material (pulp) obtained by dissolving plant fibers in water into a three-dimensional shape. Many proposals have been made for this technique. For example, Patent Document 4 (Japanese Patent Publication No. 2001-48151) discloses a pulp molded body obtained by papermaking, dehydrating, pressurizing, and drying a pulp slurry containing an agent that inhibits hydrogen bonds between pulp fibers. The molded body is described as having a density of 0.4 to 2 g / cm 3 , thickness 0.2~3mm.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 7-276320

[0010] Patent Document 2: Japanese Patent Application Publication No. 2005-67064

[0011] Patent Document 3: Japanese Patent Application Publication No. 2016-169382

[0012] Patent Document 4: Japanese Patent Application Publication No. 2001-48151 Summary of the invention

[0013] Problems to be solved by the invention

[0014] The woodwork product proposed in Patent Document 1 is obtained by adhering and solidifying wood powders in an allylated plastic shape by heating and pressurizing. Therefore, it is believed that the woodwork product described in Patent Document 1 does not have sufficient strength as a molded product. In addition, in the techniques of Patent Documents 2 and 3, in addition to lignocellulose, a matrix material as a synthetic polymer is also required. Therefore, the molded products described in Patent Documents 2 and 3 have a low biomaterial ratio.

[0015] The technology of Patent Document 4 is a technology for solidifying a slurry obtained by dispersing pulp in water to form a molded product (i.e., papermaking), which is merely an improved technology of conventional pulp molding. In the technology of Patent Document 4, cellulose fibers are held together only by hydrogen bonds, and it is difficult to obtain a molded product with a smooth surface. In addition, the gas permeability is also high, and it cannot replace conventional plastic products.

[0016] The present disclosure aims to provide a wood molded product (wood mold) which uses cellulose, particularly lignocellulose, and more preferably wood biomass as a raw material, has excellent moldability, and has improved mechanical properties.

[0017] Consider from other viewpoints, woody biomass etc. is made of natural macromolecular mixture called lignocellulose. Specifically, lignocellulose is made of macromolecules rich in aromatics such as cellulose and hemicellulose, two kinds of sugar macromolecules, and lignin. Cellulose, hemicellulose and lignin have different chemical properties respectively. Therefore, the processing difficulty of lignocellulose as the complex of these three components requires considerable chemical and mechanical energy for decomposition or separation to each component.

[0018] As a representative method for separating cellulose from wood cellulose, there is a cooking method. Specifically, chemicals (digesting agents) such as sodium sulfite and sodium hydroxide and auxiliary agents such as anthraquinone are added to wood chips for dissolution, thereby taking out wood fibers (cellulose fibers). By cooking, the lignin and resin components that fix the wood fibers are separated as a treatment agent black liquor (black liquor) and incinerated. The cellulose fibers taken out by the cooking method have a natural cellulose I type crystal structure, so it is difficult to dissolve in a solvent and has no thermoplasticity. In the past, there was no technology for shaping such cellulose fibers. As exemplified in References 1-3, only molded products in which cellulose fibers are partially derivatized and dispersed in a matrix of a synthetic polymer were proposed.

[0019] Therefore, another object of the present disclosure is to provide a technology for shaping raw materials such as woody biomass containing lignocellulose through a simple process under conditions of low energy load and environmental burden, and further to provide a method for manufacturing wood molded products without using synthetic polymers.

[0020] Solutions for solving problems

[0021] The present inventors have discovered that a molded product can be easily obtained by dissolving a raw material such as woody biomass containing cellulose or lignocellulose in an organic acid and then adding water or an alkali to precipitate the solid component and thermoforming it, thereby completing the wood molded product and production method disclosed herein.

[0022] That is, the wooden molded product of the present disclosure contains cellulose as a main component. The wooden molded product satisfies either or both of the following (1) and (2).

[0023] (1) The flexural modulus obtained in a flexural test in accordance with the provisions of ISO527-1 is 4000 MPa or more.

[0024] (2) The flexural strength obtained in a flexural test in accordance with the provisions of ISO527-1 is 50 MPa or more.

[0025] In one embodiment, the wooden molded product may further include lignin. The specific gravity of the wooden molded product including lignin is 0.5 g / cm 3above.

[0026] In another embodiment, the specific gravity of the wood molding can also be 0.9 g / cm 3 above.

[0027] Wood moldings can be detected in the infrared absorption spectrum at 1715-1720 cm -1 The area shows the absorption peak.

[0028] The wood-shaped product may further comprise a fibrous substance. The fibrous substance may also have a cellulose I-type crystal structure.

[0029] The wooden molded product may contain lignin in an amount of 15% by weight or more and 80% by weight or less of the total lignin.

[0030] The wooden molded product may further contain hemicellulose and lignin. The total lignin content of the wooden molded product may also be 20% by weight or more and 45% by weight or less. The composition ratio of polysaccharides obtained by sugar composition analysis of the wooden molded product may satisfy the following.

[0031] Dextran: 40% by weight or more and 80% by weight or less.

[0032] Xylan: 0.1 wt% to 3.0 wt% both inclusive.

[0033] Arabinan: 0.2 wt% to 3.0 wt%.

[0034] Mannan: 1.0 wt% or more and 5.0 wt% or less.

[0035] From another perspective, the present disclosure relates to wood particles used as molding materials for any of the above-mentioned wood molded products. In one embodiment, the wood particles contain cellulose, hemicellulose and lignin. The wood particles have an infrared absorption spectrum of 1715 to 1720 cm -1 The total lignin content in the wood particles is 20% by weight or more and 45% by weight or less. The composition ratio of polysaccharides obtained by sugar composition analysis of the wood particles satisfies the following conditions.

[0036] Dextran: 40% by weight or more and 80% by weight or less.

[0037] Xylan: 0.1 wt% to 3.0 wt% both inclusive.

[0038] Arabinan: 0.2 wt% to 3.0 wt%.

[0039] Mannan: 1.0 wt% or more and 5.0 wt% or less.

[0040] In another embodiment, the wood particles contain cellulose, hemicellulose and lignin. The cellulose has a cellulose I type crystal structure. The total lignin content in the wood particles is 10% by weight or more and 45% by weight or less. The composition ratio of the polysaccharides obtained by the sugar composition analysis of the wood particles satisfies the following.

[0041] Dextran: 55% by weight or more and 80% by weight.

[0042] Xylan: 0.1 wt% to 5.0 wt%.

[0043] Arabinan: 0.2 wt% to 1.0 wt%.

[0044] Mannan: 1.0 wt% or more and 3.0 wt% or less.

[0045] From another perspective, the method for producing the wood-based molded product includes the following steps: (1) dissolving a cellulose-containing raw material in an organic acid to obtain a cellulose-containing solution; (2) adding water or an alkali to the cellulose-containing solution to precipitate a solid component; (3) recovering the solid component; and (4) thermoforming the recovered solid component. The main component of the solid component is cellulose.

[0046] In the step of precipitating the solid content, the pH of the cellulose-containing solution may be adjusted to 3 or higher.

[0047] The recovered solid component may be thermoformed at a temperature of 60°C to 210°C and a pressure of 100 Pa to 400 Pa. The manufacturing method may further include a step of deliquifying the recovered solid component before thermoforming. The manufacturing method may further include a step of pulverizing the cellulose-containing raw material to obtain a cellulose-containing powder before dissolving the cellulose-containing raw material in the organic acid.

[0048] Beneficial Effects

[0049] In the wood-based molded product disclosed herein, the higher-order structure of cellulose derived from a cellulose-containing raw material, particularly woody biomass, is regenerated. Compared with wood, the wood-based molded product can have improved physical properties. Furthermore, the wood-based molded product can have strength and elastic modulus equivalent to general-purpose resins.

[0050] The lignocellulose contained in the woody biomass forms a strong high-level structure in which cellulose, hemicellulose, and lignin are intricately entangled. Specifically, in the lignocellulose, cellulose, which is a straight-chain polymer, forms a crystal structure through intramolecular and intermolecular hydrogen bonds to form strong microfibrils, hemicellulose such as xylan or glucomannan is entangled with it, and lignin, which is an irregular aromatic polymer, is filled in the gaps of the matrix of these polysaccharides to form a strong complex. Therefore, it is difficult to shape the woody biomass itself.

[0051] According to the manufacturing method disclosed in the present invention, the higher-order structure derived from cellulose, hemicellulose, etc. as raw materials is dissolved by dissolving in an organic acid, and then water molecules are removed from the precipitated solid components during the process of hot molding and dehydration, thereby regenerating the higher-order structure derived from the raw materials. According to the manufacturing method disclosed in the present invention, a low-environmental-burden wood molded product that does not contain synthetic polymers can be obtained from a cellulose-containing raw material or even a woody biomass through a simple process and under conditions of low energy load. This manufacturing method is useful in society. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 This is a photograph showing a wooden molded product (sheet) obtained by the production method according to one embodiment of the present disclosure.

[0053] Figure 2 This is a photograph showing a wooden molded product (sheet) obtained by a production method according to another embodiment of the present disclosure.

[0054] Figure 3A It is shown Figure 1 Electron microscope photograph of the surface state of a wood molding (magnification 50 times).

[0055] Figure 3B It is shown Figure 1 Electron microscope photograph of the surface state of a wood molding (magnification 1000 times).

[0056] Figure 4A It is shown Figure 2 Electron microscope photograph of the surface state of a wood molding (magnification 50 times).

[0057] Figure 4B It is shown Figure 2 Electron microscope photograph of the surface state of a wood molding (magnification 1000 times).

[0058] Figure 5 This is a photograph showing a wooden molded product (molded body) obtained by a production method according to still another embodiment of the present disclosure.

[0059] Figure 6This is a photograph showing the wooden molded product of Example 12.

[0060] Figure 7 This is a photograph showing the wooden molded product of Example 13.

[0061] Figure 8 This is a photograph showing the wooden molded product of Example 14.

[0062] Fig. 9 This is a photograph showing the molded product of Example 15.

[0063] Fig.10 This is a photograph showing the molded product of Example 16.

[0064] Fig.11 This is a photograph showing the molded product of Example 17. DETAILED DESCRIPTION

[0065] Hereinafter, an example of a preferred embodiment is specifically described. Each configuration and combination thereof in each embodiment is an example, and the configuration may be appropriately added, omitted, replaced, or otherwise modified without departing from the gist of the present disclosure. The present disclosure is not limited to the embodiments but only to the claims. In addition, each scheme disclosed in this specification may also be combined with any other feature disclosed in this specification.

[0066] It should be noted that in the present specification, "X to Y" indicating a range means "above X and below Y". In addition, unless otherwise noted, all test temperatures are room temperature (20°C ± 5°C). It should be noted that the weight percentage in the present disclosure means weight percent, not mass concentration.

[0067] [Wooden moldings]

[0068] As described below, the wooden molded product of the present disclosure can be produced using a raw material containing cellulose. The wooden molded product of the present disclosure is a concept that also includes a molded product composed only of cellulose.

[0069] The wooden molded product of the present invention comprises cellulose as an essential component. However, in addition to cellulose, the wooden molded product of the present invention may also comprise lignin. In addition, the wooden molded product may further comprise hemicellulose and / or lignin in addition to cellulose. In a preferred embodiment, the wooden molded product comprises cellulose, hemicellulose and lignin.

[0070] A wooden molded product containing lignin is obtained, for example, by using woody biomass as at least a part of the raw material containing cellulose. Woody biomass contains a certain amount of lignin and hemicellulose. The shrinkage of the molded product containing lignin during thermoforming is suppressed. The details will be described later. In the manufacturing process of the wooden molded product, the shrinkage effect generated when the hydrogen bonds of cellulose are reconstructed to form a higher-order structure by lignin interferes, and a molded product of a desired shape can be obtained. On the other hand, in the case of using only a raw material containing cellulose that does not contain lignin, by adjusting the precipitation conditions, molding conditions, etc. in the manufacturing process described later, a molded product in which the shrinkage is suppressed can be obtained.

[0071] The wood molded product of the present disclosure contains a component derived from a cellulose-containing raw material, i.e., cellulose as a main component. It should be noted that in the present disclosure, "main component" refers to a component whose content is at least 40% by weight. The content of cellulose in the wood molded product can be 80% by weight or more, 90% by weight or more, or 100% by weight.

[0072] The wooden molded product of the preferred embodiment may further contain lignin, and may further contain lignin and / or cellulose. The wooden molded product of this scheme can be obtained using a raw material containing lignocellulose having a high-level structure composed of cellulose, hemicellulose and lignin, such as wood biomass. In this case, the main components of the wooden molded product of the present disclosure may be cellulose, hemicellulose and lignin, and they may be contained in the form of lignocellulose. In addition, the total content of cellulose, hemicellulose and lignin in the wooden molded product (or as the content of lignocellulose) may be 60% by weight or more, 80% by weight or more, 90% by weight or more, or 100% by weight.

[0073] (Mechanical properties of wood moldings)

[0074] The wooden molded product of the present disclosure also has the following characteristics (1) or (2) or both.

[0075] (1) The flexural modulus obtained in a flexural test in accordance with the provisions of ISO527-1 is 4000 MPa or more.

[0076] (2) The flexural strength obtained in a flexural test in accordance with the provisions of ISO527-1 is 50 MPa or more.

[0077] For example, among general-purpose resins, ABS resin has a bending strength of 64 MPa and a bending pulp mold volume of 2500 MPa, polycarbonate (PC) has a bending strength of 85 MPa and a bending modulus of 2300 MPa, and polyethylene terephthalate (PET) has a bending strength of 76 to 103 MPa and a bending modulus of 2800 to 4200 MPa (https: / / www.plastic-kakou.net / material / plastic.html). In addition, for wood, the bending strength of paulownia is 34.3 MPa and the bending modulus is 4900 MPa, and the bending strength of cedar is 63.7 MPa and the bending modulus is 7350 MPa (https: / / www.toishi.info / sozai / woods / ). Therefore, it can be said that the wood molded product of the present disclosure that satisfies the above (1) and / or (2) has mechanical properties that are equal to or better than those of general-purpose resins, and further has properties that are comparable to those of wood.

[0078] When the flexural modulus (Young's modulus) of the wood molded product disclosed herein is 4000 MPa or more, it may be 4500 MPa or more, or 5000 MPa or more, depending on its use and shape, and may be 8000 MPa or less, or 7000 MPa or less. The flexural modulus disclosed herein may be 4000-8000 MPa, 4000-7000 MPa, 4500-8000 MPa, 4500-7000 MPa, 5000-8000 MPa, or 5000-7000 MPa.

[0079] When the bending strength (maximum stress) of the wood molded product disclosed herein is 50 MPa or more, it may be 55 MPa or more, or 60 MPa or more, depending on its use and shape, and may be 100 MPa or less, or 90 MPa or less. The bending strength (maximum stress) of the wood molded product may be 50 to 100 MPa, 50 to 90 MPa, 55 to 100 MPa, 55 to 90 MPa, 60 to 100 MPa, or 60 to 90 MPa.

[0080] The maximum elongation of the wood molded product in the bending test is 1.0% GL or more, and may be 1.5% GL or more, and may be 5.0% GL or less, and may be 4.5% GL or less. The maximum elongation of the wood molded product is 1.0-5.0% GL, and may be 1.0-4.5% GL, and may be 1.5-5.0% GL, and may be 1.5-4.5% GL.

[0081] In the present disclosure, the bending properties of the wood-molded product are measured by a bending test in accordance with the provisions of ISO527-1. In the bending test, a test piece formed into a specified size or a test piece machined by cutting or punching is used. Before the measurement, the test piece is humidified for 12 hours in an environment of 25°C and 50RH%. The measurement is carried out in a 3-point bending test with a bending speed of 2 mm / min.

[0082] The tensile properties of the wood molded product can be appropriately set according to its use and shape. For example, the tensile elastic modulus (Young's modulus) of the wood molded product can be 100 MPa or more, 200 MPa or more, or 3000 MPa or less. The tensile elastic modulus (Young's modulus) of the wood molded product can be 100 to 3000 MPa, or 200 to 3000 MPa.

[0083] The tensile strength (maximum stress) of the wood molded product may be 4.0 MPa or more, 6.0 MPa or more, 10.0 MPa or more, or 20.0 MPa or more, and 80.0 MPa or more, or 70.0 MPa or less. The tensile strength (maximum stress) of the wood molded product is 4.0 to 80.0 MPa, 4.0 to 70.0 MPa, 6.0 to 80.0 MPa, 6.0 to 70.0 MPa, 10.0 to 80.0 MPa, 10.0 to 70.0 MPa, 20.0 to 80.0 MPa, or 20.0 to 70.0 MPa.

[0084] The maximum elongation in the tensile test of the wood molded product may be 1.0% GL or more, or 1.5% GL or more, or 5.0% GL or less, or 4.5% GL or less. The maximum elongation may be 1.0 to 5.0% GL, or 1.0 to 4.5% GL, or 1.5 to 5.0% GL, or 1.5 to 4.5% GL.

[0085] In the present disclosure, the tensile properties of the wood molded product are measured by a tensile test according to ISO527-1. In the tensile test, a test piece processed into a specified size by punching is used. Before the measurement, the test piece is humidified for 12 hours under an environment of 25°C and 50RH%. The measurement is carried out at a tensile speed of 10 mm / min.

[0086] (Density of wooden moldings)

[0087] The wood molded product disclosed in the present invention has a high specific gravity. That is, the density of the wood molded product is high. The specific gravity of the wood molded product measured according to JIS Z8807 "Determination of density and specific gravity of solids" is preferably 0.5 g / cm3 More preferably 0.6 g / cm 3 More preferably, 0.8 g / cm 3 Above, particularly preferably 0.9 g / cm 3 In addition, the specific gravity of the wood molding is preferably less than 2.5 g / cm 3 , more preferably less than 2.0 g / cm 3 , especially preferably less than 1.5 g / cm 3 The specific gravity of wood moldings can be 0.5g / cm 3 Above and less than 2.5g / cm 3 , can be 0.6g / cm 3 Above and less than 2.5g / cm 3 , can be 0.8g / cm 3 Above and less than 2.5g / cm 3 , can be 0.9g / cm 3 Above and less than 2.5g / cm 3 , can be 0.9g / cm 3 Above and less than 2.0g / cm 3 , can also be 0.9g / cm 3 Above and less than 1.5g / cm 3 the following.

[0088] The density of the wood molded product can be adjusted, for example, by the pressure during the hot molding process in the manufacturing process. By pressing under high pressure, a high-density wood molded product can be obtained. By increasing the density of the wood molded product, there is a tendency for the mechanical strength to be improved. In order to obtain a wood molded product of the desired strength, in addition to the pressure during hot molding, the molding temperature, molding time, etc. can also be adjusted.

[0089] In addition, the density of the wood molded product can also be adjusted to an appropriate value according to its material. For example, when the wood molded product contains lignin as a constituent component, a relatively high strength can be obtained by forming a high-order structure. The density of the wood molded product containing lignin is 0.5 g / cm 3 Above and less than 2.5g / cm 3 , can be 0.5g / cm 3 Above and less than 1.5g / cm 3 , can be 0.5g / cm 3 Above and less than 1.3g / cm 3 By including lignin, a wooden molded product having a smooth surface can be obtained. The total lignin content of the wooden molded product can be 15% by weight or more and 80% by weight or less. The total lignin content will be described later.

[0090] (Infrared absorption spectrum of wooden moldings)

[0091] The wooden molded product disclosed herein can be shown in the infrared absorption spectrum at 1715-1720 cm -1 The range has an absorption peak with a peak top. Wave number 1715~1720cm -1 The absorption peak is due to the C=O stretching vibration. Specifically, it is the absorption peak caused by the C=O stretching vibration of the aldehyde group (formyl group). In the present disclosure, 1715 to 1720 cm -1 The presence of the absorption peak means that part or all of the hydroxyl groups of cellulose contained in the wood molded product are formylated.

[0092] As described later, the wooden molded product of the present invention is prepared by dissolving a cellulose-containing raw material in an organic acid and then precipitating the solid component by adding water or alkali for hot molding. When the cellulose-containing raw material is dissolved in an organic acid, formyl groups are introduced into a part or all of the hydroxyl groups of the cellulose. The formyl groups are saponified and restored to hydroxyl groups in a precipitation process by adding alkali. The hydroxyl groups contribute to the formation of hydrogen bonds. By reconstructing a higher-order structure based on the hydrogen bonds, a high-strength molded product can be obtained. On the other hand, in the case where all the formyl groups are completely saponified, especially in wooden molded products with a low lignin content, when the higher-order structure is reconstructed by hydrogen bonds, it will become a cause of deformation / shrinkage. Therefore, when using a cellulose-containing raw material with a low lignin content, it is preferred to contain at least a portion of formylated cellulose. By adding water instead of alkali in the precipitation process, a wooden molded product containing at least a portion of formylated cellulose can be obtained.

[0093] The wood molded product of the present disclosure may further contain a fibrous substance. By containing the fibrous substance, a wood molded product having excellent strength can be obtained. The presence of the fibrous substance in the wood molded product can be confirmed by observation under a scanning electron microscope.

[0094] The fibrous substance in the wooden molded product can be derived from the wood biomass used as the raw material. For example, it can be cellulose fibers that have not been crushed or damaged during the manufacturing process. In addition, the fibrous substance can be a dissolved residue in the dissolution process. According to the present disclosure, a uniform wooden molded product can be obtained in which such fibrous substance is also embedded in lignin and hemicellulose. In particular, in wooden molded products with a high lignin content, since the fibrous substance is embedded in the fibrous substance, a wooden molded product with a smoother surface can be obtained.

[0095] In the present disclosure, the fibrous substance may also be a substance having a cellulose type I crystal structure. The presence of a cellulose type I crystal structure can be confirmed by X-ray diffraction measurement. For example, there is a method of measuring a sample after freeze-drying a wooden molded product using an X-ray diffraction measuring device (e.g., "SmartLab" manufactured by Rigaku Corporation). Specifically, the measurement can be performed by powder X-ray diffraction using a non-reflective silicon plate. It is known that cellulose type I crystals having a parallel chain structure show high-intensity diffraction near 2θ=22.5°, near 16.7°, and near 14.8° through peak separation. Therefore, in the X-ray diffraction pattern measured for a sample collected from a wooden molded product, the presence or absence of a cellulose type I crystal structure can be determined by confirming the presence or absence of high-intensity diffraction peaks near 2θ=22.5°, near 16.7°, and near 14.8°.

[0096] (Total lignin content of wooden molded products)

[0097] As described above, the disclosed wooden molded product preferably contains lignin. By containing lignin, even when containing a fibrous substance having a cellulose I-type crystal structure, a wooden molded product with a smooth surface can be obtained. In addition, by containing a specified amount of lignin, cracks, breakages, etc. during hot forming can be suppressed. From this viewpoint, the total lignin amount of the wooden molded product can be more than 2% by weight, can be more than 5% by weight, can be more than 7% by weight, can be more than 10% by weight, can be more than 15% by weight, can be more than 20% by weight, can also be more than 21% by weight, in addition, can be less than 90% by weight, can be less than 89% by weight, can be less than 85% by weight, can be less than 80% by weight, can be less than 70% by weight, can be less than 50% by weight, can be less than 48% by weight, can be less than 45% by weight, and can also be less than 44% by weight.

[0098] For example, the total lignin content of the wooden molded product may be 2-90 wt%, 2-89 wt%, 2-85 wt%, 2-80 wt%, 2-50 wt%, 2-48 wt%, 2-45 wt%, 2-44 wt%, 5-90 wt%, 5-89 wt%, 5-85 wt%, 5-80 wt%, 5-50 wt%, 5-48 wt%, 5-45 wt%, 5-44 wt%, 7-90 wt%, 7-89 wt%, 7-85 wt%, 7-80 wt%, 7-50 wt%, 7-48 wt%, 7-45 wt%, 7-44 wt%, 10-90 wt%, 10-89 wt%, 10-85 wt%, 10-80 wt%, 10-50 wt%. %, 10-48 wt%, 10-45 wt%, 10-44 wt%, 15-90 wt%, 15-89 wt%, 15-85 wt%, 15-80 wt%, 15-50 wt%, 15-48 wt%, 15-45 wt%, 15-44 wt%, 20-90 wt%, 20-89 wt%, 20-85 wt%, 20-80 wt%, 20-50 wt%, 20-48 wt%, 20-45 wt%, 20-44 wt% and 21-90 wt%, 21-89 wt%, 21-85 wt%, 21-80 wt%, 21-50 wt%, 21-48 wt%, 21-45 wt%, 21-44 wt%. Preferably, the total lignin content of the wood molded product can be any one of 2 weight % or more and 90 weight %, 5 weight % or more and 89 weight % or more, 7 weight % or more and 85 weight % or more, 10 weight % or more and 85 weight % or more, 15 weight % or more and 80 weight % or more, 10 weight % or more and 50 weight % or more, 15 weight % or more and 48 weight % or more, 20 weight % or more and 45 weight % or more, and 21 weight % or more and 44 weight % or more.

[0099] The total lignin content in the wooden molded product can be adjusted by selecting a cellulose-containing raw material, particularly a woody biomass. For example, by selecting wood as a woody biomass containing a cellulose-containing raw material and adjusting its tree species and blending amount, the desired total lignin content can be controlled. By increasing the total lignin content, a wooden molded product with high hydrophobicity and a large contact angle can be obtained. In addition, by adjusting the total lignin content, the biodegradation rate of the wooden molded product can also be controlled. Wooden molded products with a large total lignin content tend to have a slow biodegradation rate, and wooden molded products with a small total lignin content tend to have a fast biodegradation rate. However, since lignin is also a wood component, it is ultimately biodegraded in the same manner as woody biomass. In addition, the wooden molded product disclosed in the present invention is formed by the reconstruction of the hydrogen bonds of cellulose. Therefore, in wooden molded products that are in a wet state for a long time, these hydrogen bonds are relaxed and easily acted upon by biodegradable enzymes, etc. For example, in the case where the wooden molded product disclosed in the present invention is used as an interior material for a car, it can be expected that it can be easily biodegraded by processing it into crumbs, etc. after the car is scrapped and making it in a wet state.

[0100] In addition, in this disclosure, the total amount of lignin in the wooden molded product is calculated as the total amount of acid-soluble lignin and acid-insoluble lignin. The quantitative method of the total amount of lignin will be described later in the Examples.

[0101] (Preferred components of wooden molded products)

[0102] The wooden molded product of the present disclosure may further contain hemicellulose together with lignin. When ordinary woody biomass is used as the cellulose-containing raw material, the wooden molded product may contain lignin and hemicellulose derived from the constitution of the woody biomass.

[0103] In a preferred embodiment, the wooden molded product contains cellulose, hemicellulose and lignin. When the total lignin content is 20 wt % or more and 45 wt % or less, the composition ratio of the polysaccharides obtained by sugar composition analysis may be as follows.

[0104] Dextran: 40% by weight or more and 80% by weight or less.

[0105] Xylan: 0.1 wt% to 3.0 wt% both inclusive.

[0106] Arabinan: 0.2 wt% to 3.0 wt%.

[0107] Mannan: 1.0 wt% or more and 5.0 wt% or less.

[0108] The sugar composition ratio of the wooden molded product can be controlled within a desired range by adjusting the type and proportion of the woody biomass in the cellulose-containing raw material. For example, the above-mentioned sugar composition ratio can be achieved by mixing an appropriate amount of woody biomass as a raw material with waste paper pulp substantially composed of cellulose. In addition, the sugar composition ratio of the wooden molded product can be adjusted by changing the conditions of the manufacturing process (e.g., the precipitation step).

[0109] The wood molded product may also contain an organic acid within the scope of not hindering the effect of the present disclosure. Examples of the organic acid include α-keto acids or carboxylic acids having a formyl group. The organic acid may be one or more selected from the group consisting of formic acid, glyoxylic acid, and pyruvic acid.

[0110] The amount of organic acid contained in the wood molded product is not particularly limited. For example, from the viewpoint of not damaging the mechanical properties and durability, the amount of the organic acid can be 10.0 wt % or less, 8.0 wt % or less, 6.0 wt % or less, 4.0 wt % or less, 1.0 wt % or less, 0.1 wt % or less, 100 ppm or less, and the lower limit thereof can be 0.

[0111] The shape of the wood molded product disclosed in the present invention is not particularly limited. For example, its thickness can be more than 1 mm, more than 5 mm, or more than 10 mm. The wood molded product can have physical properties similar to those of the cellulose-containing raw material, such as wood biomass, used as the raw material. Furthermore, it can also have physical properties that exceed those of the raw material. The wood molded product disclosed in the present invention can be used in the fields of medical care, clothing, residential equipment, etc., for example, as films, fibers, wallpapers, etc. that require functions such as antibacterial properties, ultraviolet absorption, and metal adsorption capacity.

[0112] [Wood pellets]

[0113] The wood particles of the present disclosure can be used as a molding material for the above-mentioned wood molded products. For example, the wood molded products of the present disclosure can be obtained by using the wood particles as a material and utilizing a known thermoforming technology of a thermosetting resin or a molding technology of pulp molding.

[0114] In the manufacturing process of the wood molded product described later, water or alkali is added to the solution formed by dissolving the cellulose-containing raw material in the organic acid, and the solid content recovered by precipitation can be used as the wood particles disclosed in the present invention. The wood particles may contain water. The amount of moisture contained in the wood particles is not particularly limited, but from the perspective of easily obtaining the wood molded product disclosed in the present invention, the solid content concentration of the wood particles can be 1% by weight or more, 5% by weight or more, 10% by weight or more, and 80% by weight or less, 60% by weight or less, or 50% by weight or less. The solid content concentration of the wood particles can be 1 to 80% by weight, 5 to 60% by weight, or 10 to 50% by weight.

[0115] Wood pellets can be packaged in moisture-proof packaging. The moisture-proof packaging can have a water vapor transmission rate of 50cc / m 2 · Less than 20 cc / m 2 · Days or less. By packaging the wood pellets in a moisture-proof package, the necessary time can be stored, and after the necessary time, the thermoforming described below can be provided. As long as the wood pellets have the above-mentioned moisture content, the wood pellets can also be compressed and packaged. For example, a device for compressing and packaging waste can be used to compress the wood pellets to 1 / 5 to 1 / 10 of the volume and package them in a moisture-proof package. By packaging in this way, the storage and transportation efficiency of the wood pellets is improved. The packaged wood pellets can be appropriately opened from the moisture-proof package and taken out for use.

[0116] From the viewpoint of storage stability, the pH of water contained in the wood pellets is preferably 6 or less, and is preferably 2 or more, and more preferably 3 or more. The water contained in the wood pellets may have a pH of 2 to 6, or may have a pH of 3 to 6. The pH can be adjusted by washing the solid component recovered by precipitation.

[0117] (Preferred embodiment 1 of wood particles)

[0118] In a preferred embodiment, the wood particles have a wavelength of 1715-1720 cm in the infrared absorption spectrum. -1 The wood particles of the embodiment 1 can be obtained, for example, by carrying out a step of precipitating a solid component from a solution prepared by dissolving a cellulose-containing raw material in an organic acid under incomplete saponification conditions during the production process of a wood molded product.

[0119] The wood particles of the first embodiment contain cellulose, hemicellulose and lignin, and the total lignin content is 20% by weight or more and 45% by weight or less. Within this range, the total lignin content is not completely saponified, thereby suppressing excessive shrinkage during the reconstruction of hydrogen bonds of hydroxyl groups. From this viewpoint, the total lignin content of the wood particles of the first embodiment can be 15% by mass or more and 48% by mass or less.

[0120] In the wood pellets of the embodiment 1, when the total lignin content is 20% by weight or more and 45% by weight or less, the composition ratio of polysaccharides obtained by sugar composition analysis can satisfy the following conditions.

[0121] Dextran: 40% by weight or more and 80% by weight or less.

[0122] Xylan: 0.1 wt% to 3.0 wt% both inclusive.

[0123] Arabinan: 0.2 wt% to 3.0 wt%.

[0124] Mannan: 1.0 wt% or more and 5.0 wt% or less.

[0125] Glucan is a polysaccharide mainly derived from cellulose, and xylan, arabinan, and mannan are polysaccharides derived from hemicellulose. By making the composition ratio of glucan derived from cellulose within the above range, the strength of the obtained wooden molded product is improved. On the other hand, in the case of containing polysaccharides derived from hemicellulose exceeding the above range, the wooden molded product is sometimes colored during thermoforming. In addition, in the case of mannan, which is a representative constituent sugar of hemicellulose, being less than the above range, the content of cellulose is relatively increased, and the wooden molded product is sometimes deformed / contracted during thermoforming.

[0126] (Preferred embodiment 2 of wood particles)

[0127] In another preferred embodiment, the wood pellets contain cellulose having a cellulose type I crystal structure. The cellulose may be contained as a fibrous substance. According to the wood pellets of embodiment 2 containing cellulose having a cellulose type I crystal structure, a wood molded product having excellent strength can be obtained.

[0128] The wood particles of the embodiment 2 contain cellulose, hemicellulose and lignin, and the total lignin content is 10 wt% or more and 45 wt% or less. For the wood particles, the composition ratio of polysaccharides obtained by sugar composition analysis can satisfy the following conditions.

[0129] Dextran: 55% by weight or more and 80% by weight or less.

[0130] Xylan: 0.1 wt% to 5.0 wt%.

[0131] Arabinan: 0.2 wt% to 1.0 wt%.

[0132] Mannan: 1.0 wt% or more and 3.0 wt% or less.

[0133] According to the wooden pallet in which the total lignin content is within the above range and the glucan, xylan, arabinan and mannan are in the above composition ratio, shrinkage during hot molding can be suppressed, and a wooden molded product with excellent strength and little coloration can be obtained.

[0134] [Method for producing wooden molded product]

[0135] The method for producing a wood-based molded product disclosed herein comprises: (1) dissolving a cellulose-containing raw material in an organic acid to obtain a cellulose-containing solution; (2) adding water or an alkali to the cellulose-containing solution to precipitate a solid component; (3) recovering the solid component; and (4) thermoforming the recovered solid component. The main component of the solid component is cellulose.

[0136] The cellulose-containing raw material may be a raw material consisting essentially of cellulose (such as pulp) or a raw material containing cellulose as lignocellulose. Preferably, it is woody biomass.

[0137] In the pulp having the same cellulose I type crystal structure as natural cellulose, the cellulose forms a firm high-order structure through hydrogen bonds, thereby hindering the excipient property. In addition, the main component of woody biomass is wood cellulose with a high-order structure composed of cellulose, hemicellulose and lignin. The whole wood cellulose is insoluble in solvents such as water and organic solvents under mild conditions due to its high-order structure. The inventors first found that by formylation of wood cellulose as the main component of woody biomass in organic acids, such as formic acid, the intramolecular and intermolecular hydrogen bonds brought by cellulose are hindered, and hemicellulose and lignin are solubilized and can be dissolved in organic acids under mild conditions. Furthermore, it is also found that this effect is also effective for cellulose-containing raw materials (such as pulp) containing cellulose I type crystal structure.

[0138] That is, in the manufacturing method of the present disclosure, the hydrogen bonds between the cellulose molecules and the lignin molecules are eliminated by esterifying (e.g., formylation) the cellulose-containing raw material in an organic acid. As a result, the cellulose-containing raw material is dissolved in the organic acid to obtain a cellulose-containing solution. In the case where the cellulose-containing raw material is wood cellulose containing lignin, the lignin is also dissolved in the organic acid. In addition, in the case where the cellulose-containing raw material contains hemicellulose, the hemicellulose is also dissolved in the organic acid. In other words, in the present disclosure, in addition to cellulose, the cellulose-containing solution may also contain lignin and hemicellulose. It should be noted that the main component of the wooden molded product of the present disclosure is cellulose.

[0139] Furthermore, the inventors of the present invention have found that by adding water or alkali to a cellulose-containing solution, a solid component containing cellulose is precipitated. It was found that by dehydration and hot forming, the liquid component (water, etc.) is lost from the solid component, the high-order structure formed by hydrogen bonds is reconstructed, and the original structure of cellulose is regenerated. Moreover, it was found that the physical properties (specific gravity, strength, etc.) of the molded product obtained by hot forming the recovered solid component are improved compared with the cellulose-containing raw material (such as woody biomass) used. As its mechanism, it is believed that the hydroxyl groups of cellulose are regenerated by saponification (deformylation), the intermolecular or intramolecular hydrogen bonds of cellulose are formed, and preferably hemicellulose and lignin are insolubilized to produce a high-order structure derived from natural products. According to this mechanism, in the manufacturing method disclosed in the present invention, petroleum-based chemicals with a large burden on the environment are not used, and a cellulose-containing raw material, preferably wood cellulose, and especially woody biomass is used as a raw material, and a wooden molded product with excellent moldability and characteristics comparable to general-purpose resins can be obtained.

[0140] Hereinafter, each step will be described in detail.

[0141] (1) A step of dissolving a cellulose-containing raw material in an organic acid to obtain a cellulose-containing solution.

[0142] In this step, in order to obtain a cellulose-containing solution (hereinafter sometimes referred to as "solution"), a cellulose-containing raw material is dissolved in an organic acid. The cellulose-containing raw material may contain cellulose, and may be a raw material containing cellulose as lignocellulose. Examples of raw materials containing cellulose mainly in the form of lignocellulose include woody biomass.

[0143] For example, the cellulose-containing raw material used in the present disclosure may be low-purity cellulose, high-purity cellulose, or dissolving pulp with high α-cellulose purity. In addition, waste paper pulp with not so high α-cellulose purity may also be used as the cellulose-containing raw material of the present disclosure. A preferred cellulose-containing raw material contains lignin in addition to cellulose. As such a cellulose-containing raw material, mechanical pulp is preferred, and woody biomass such as sawdust is more preferred.

[0144] These cellulose-containing raw materials may be used alone or in combination. For example, woody biomass and waste paper pulp may be mixed and used. As the cellulose-containing raw material, woody biomass containing lignin is particularly preferred.

[0145] (Wooden biomass)

[0146] Biomass generally refers to "renewable, organic resources derived from living organisms (excluding fossil fuels)". The woody biomass used in the production method of the present disclosure is not particularly limited, but preferably used is a material derived from wood such as broadleaf trees and coniferous trees containing a large amount of lignocellulose.

[0147] Lignocellulose refers to a mixture of natural polymers mainly composed of cellulose, hemicellulose and lignin. Depending on the type of woody biomass selected, the content of cellulose, hemicellulose and lignin is different, but in the manufacturing method disclosed herein, their composition is not particularly limited. Two or more woody biomasses containing woody cellulose of different compositions can be used as cellulose-containing raw materials. Within the scope of the effect of the present disclosure, herbaceous biomass such as bagasse, straw, and wheat bran can be used in combination. Woody biomass or herbaceous biomass can also be crushed and used as needed.

[0148] (pulp)

[0149] Pulp refers to a substance obtained by mechanically or chemically treating plant materials such as wood to extract cellulose. For example, mechanical pulp produced by directly or mechanically treating wood while subjecting it to heat treatment can be cited. Mechanical pulp is classified into ground wood pulp (GP), wood mechanical pulp (RGP), thermomechanical pulp (TMP), chemical thermomechanical pulp (CTMP), etc. according to the production method. Among them, ground wood pulp is preferred. In addition, chemical pulp obtained by chemically treating wood can be used as the cellulose-containing raw material of the present disclosure. Examples of chemical pulp include rayon pulp, dissolving pulp, etc. The pulp can also be crushed and used.

[0150] (Dissolved)

[0151] In this specification, "dissolution" refers to a state in which the shape of the plant material in the organic acid cannot be visually identified. The situation in which fibrous substances derived from lignocellulose are observed in the solution and the shape of the cellulose-containing raw material itself disappears through microscopic observation is defined as "dissolution". In addition, such a liquid in a "dissolved" state is defined as a "solution" in the present disclosure. The cellulose-containing raw material is preferably uniformly dissolved in the organic acid, but the cellulose-containing raw material may also be partially dissolved in the organic acid. In the case of partial dissolution, the insoluble components can be removed by filtration, etc. to obtain a cellulose-containing solution.

[0152] (Organic Acid)

[0153] As long as the effects of the present disclosure are obtained, the type of organic acid is not particularly limited, and a representative organic acid is a carboxylic acid. It may be an aliphatic carboxylic acid or an aromatic carboxylic acid. From the viewpoint of excellent solubility of wood powder, α-keto acids and carboxylic acids having a formyl group are preferred, and organic acids selected from the group consisting of formic acid, glyoxylic acid and pyruvic acid are particularly preferred. Formic acid that can be produced using wood gas (a mixed gas of carbon dioxide and hydrogen) as a raw material is particularly preferred.

[0154] The amount of organic acid mixed with the cellulose-containing raw material is appropriately selected according to the type and shape of the cellulose-containing raw material, the type of organic acid, etc. From the viewpoint of improving the dissolution efficiency, the amount of organic acid is preferably 4 parts by weight or more, and more preferably 9 parts by weight or more, relative to 1 part by weight of the cellulose-containing raw material. From the viewpoint of improving the manufacturing efficiency, the amount of organic acid is preferably 200 parts by weight or less, more preferably 100 parts by weight or less, and further preferably 49 parts by weight or less, relative to 1 part by weight of the cellulose-containing raw material. The amount of organic acid can be 4 to 200 parts by weight, 4 to 100 parts by weight, 4 to 49 parts by weight, 9 to 200 parts by weight, 9 to 100 parts by weight, or 9 to 49 parts by weight relative to 1 part by weight of the cellulose-containing raw material. As long as the effect of the present disclosure is obtained, the organic acid can be added directly to the cellulose-containing raw material or added to the cellulose-containing raw material as a solution of a desired concentration.

[0155] As long as a cellulose-containing solution is obtained, the dissolution conditions are not particularly limited and can be appropriately selected according to the type and shape of the cellulose-containing raw material, the type of organic acid, etc. From the viewpoint of high dissolution efficiency, the dissolution temperature is preferably 20° C. or higher, more preferably 30° C. or higher. From the viewpoint of energy saving, the preferred dissolution temperature is 100° C. or lower.

[0156] From the viewpoint of promoting dissolution, stirring treatment may be performed or stirring treatment accompanied by pulverization may be performed. By performing stirring treatment accompanied by pulverization in an organic acid, the cellulose-containing raw material can be dissolved under milder conditions. In other words, the production method disclosed in the present invention includes a step of stirring and dissolving while pulverizing the cellulose-containing raw material in an organic acid. As an apparatus for stirring treatment accompanied by pulverization, for example, a bead mill, a colloid mill, a disc refiner, a cone refiner, etc. can be cited.

[0157] (Voltage regulation)

[0158] In the manufacturing method disclosed in the present invention, before mixing the cellulose-containing raw material with the organic acid and / or after mixing the cellulose-containing raw material with the organic acid, there may be further a step of pressurizing or depressurizing using a pressure adjustment unit. It is speculated that in this pressure adjustment, the pressure fluctuation applied to the cellulose-containing raw material relaxes the firm high-order structure of cellulose, especially lignocellulose, and significantly improves the solubility in organic acids. By performing this pressure adjustment, dissolution can be carried out at a relatively low temperature, reducing the energy required for heating and / or heat preservation during dissolution. From the viewpoint of efficiently introducing the organic acid into the tissue of the cellulose-containing raw material through pressure fluctuations, it is preferred to pressurize or depressurize after adding the organic acid to the cellulose-containing raw material.

[0159] In the case of decompression, it is preferred to decompress within a range of 1.0 kPa or more and 10.0 kPa (absolute pressure). In addition, in the case of pressurization, it is preferred to pressurize within a range of 200 kPa or more and 1000 kPa or less (gauge pressure). In this specification, when a pressure lower than atmospheric pressure is indicated by a decompression process, an absolute pressure is used, and when a pressure higher than atmospheric pressure is indicated by a pressurization process, a gauge pressure based on atmospheric pressure is used.

[0160] The pressure regulating means for pressurizing and / or reducing pressure is not particularly limited, and the pressure can be adjusted to the above-mentioned pressure range by a known means such as an aspirator, an ejector, a compressor, a mechanical pump, etc.

[0161] (Containing cellulose solution)

[0162] The solid content concentration of the cellulose-containing solution obtained by dissolving the cellulose-containing raw material in the organic acid is preferably 0.5 (w / v)% or more, more preferably 1.0 (w / v)% or more, and further preferably 1.5 (w / v)% or more. From the viewpoint of easy production, the concentration of the solution is preferably 20 (w / v)% or less, more preferably 10 (w / v)% or less. More preferably, it is 0 (w / v)% or less. The solid content concentration of the cellulose-containing solution can be 0.5-20 (w / v)%, 0.5-10 (w / v)%, 0.5-8.0 (w / v)%, 1.0-20 (w / v)%, 1.0-10 (w / v)%, 1.0-8.0 (w / v)%, 1.5-20 (w / v)%, 1.5-10 (w / v)%, and 1.5-8.0 (w / v)%. The cellulose-containing solution may further contain known additives such as a pigment within a range not inhibiting the effects of the present disclosure.

[0163] (2) A step of adding water or an alkali to a cellulose-containing solution to precipitate a solid component.

[0164] In this step, water or alkali is added to the cellulose-containing solution obtained by dissolving the cellulose-containing raw material, so that the soluble cellulose, preferably lignocellulose, is regenerated and the insoluble solid component is precipitated. The main component of the solid component is cellulose. From the viewpoint of improving the yield in the recovery step of the solid and liquid components described later, the cellulose-containing solution can also be concentrated before this step. Known concentration methods such as evaporation concentration and reduced pressure concentration can be appropriately used.

[0165] In this step, water or alkali is added to the cellulose-containing solution, and part or all of the esterified cellulose is deesterified and insolubilized by hydrogen bonds formed by regenerated hydroxyl groups. When lignin and hemicellulose are present in the cellulose-containing solution, the deesterified cellulose is precipitated in a dispersed state in the matrix of lignin and hemicellulose. It should be noted that when formic acid is used in the previous step, cellulose is deformylated in this step.

[0166] By adding an alkali to a cellulose-containing solution, deesterification of esterified cellulose can be promoted. In other words, the esterified cellulose is saponified (hydrolyzed) by adding an alkali.

[0167] As long as the effects of the present disclosure can be obtained, the method for precipitating the solid component is not particularly limited. For example, the precipitation of the solid component can be a water mixing treatment, an alkali treatment, or a dialysis treatment. It is also possible to combine two or more selected from the water mixing treatment, the alkali treatment, and the dialysis treatment.

[0168] (Add water and mix)

[0169] In the present disclosure, "water addition and mixing treatment" means adding water (eg, distilled water) to a cellulose-containing solution and mixing to precipitate a solid component. During the precipitation process, the esterified cellulose may be partially hydrolyzed (saponified).

[0170] The amount of water added to the cellulose-containing solution is appropriately selected according to the solid content concentration in the solution. The amount of water added can be adjusted so that the pH of the cellulose-containing solution is 3 or more, preferably 5 or more, and more preferably 6 or more. For example, the amount of water in the water-adding and mixing treatment can be 100 times or more, 200 times or more, 1000 times or less, or 800 times or less of the volume of the cellulose-containing solution. There is no particular restriction on the temperature of the water-adding and mixing treatment, which is usually 10 to 50°C, and can be room temperature (20°C ± 5°C). In order to promote the reaction, stirring and mixing can be performed while heating or keeping warm.

[0171] (Alkali treatment)

[0172] In the present disclosure, "alkali treatment" refers to adding alkali to a solution containing cellulose to perform a hydrolysis (saponification) reaction. By promoting saponification by alkali treatment, the physical properties of the wood-molded product can be adjusted. It should be noted that in this process, as long as the solid content containing cellulose is precipitated, as long as the effect of the present disclosure can be obtained, an intentional saponification treatment is not necessary.

[0173] The alkali used in the alkali treatment is not particularly limited, and an alkali metal hydroxide, an alkaline earth metal hydroxide, a quaternary ammonium hydroxide, ammonia, etc. can be appropriately selected. Alkali metal hydroxides are preferred, and sodium hydroxide is preferably used. These alkalis can also be dissolved in a solvent such as water to adjust the concentration to a desired alkali solution, and then added to the cellulose-containing solution.

[0174] The temperature of the alkali treatment is not particularly limited as long as the effects of the present disclosure can be obtained, but is preferably 10° C. or higher, more preferably 20° C. or higher, from the viewpoint of promoting the hydrolysis reaction. From the viewpoint of suppressing coloration, the temperature of the alkali treatment is preferably 80° C. or lower, more preferably 60° C. or lower. In order to control the temperature within this range, the cellulose-containing solution may be subjected to the alkali treatment while being cooled.

[0175] As long as the precipitated solid content can be recovered, the pH of the treated solution is not particularly limited. For example, the solution after adding water or alkali can have a pH of 2.0 or above, a pH of 2.5 or above, or a pH of 3.0 or above. From the viewpoint of promoting the precipitation of the solid content, it is preferably a pH of 6.0 or above, and more preferably a pH of 7.0 or above. When the pH exceeds 11, it may sometimes react with the ester group of the esterified cellulose to form an alkali salt in excess. From this viewpoint, the pH is preferably less than 11.0, and more preferably less than pH 10.5.

[0176] (Dialysis treatment)

[0177] As a variation of this process, dialysis treatment can be cited. "Dialysis treatment" refers to contacting a cellulose-containing substance with a solvent through a semipermeable membrane (dialysis membrane) to precipitate a solid component. In detail, a cellulose-containing solution is placed inside the semipermeable membrane so that it is contacted with a solvent (e.g., distilled water) outside the semipermeable membrane. Due to the concentration gradient inside and outside the semipermeable membrane, distilled water penetrates into the semipermeable membrane, whereby a hydrolysis reaction is carried out, and the hydroxyl groups in the cellulose are regenerated to form intramolecular or intermolecular hydrogen bonds, which are precipitated as solid components. In addition, in the presence of lignin and hemicellulose in the cellulose-containing solution, hemicellulose and lignin are insoluble together with cellulose, generating a solid component containing a higher-order structure similar to lignocellulose. In order to promote the hydrolysis reaction, the solvent can be replaced at predetermined intervals.

[0178] In the dialysis treatment, the amount of solvent used relative to the cellulose-containing solution is appropriately selected according to the solid content concentration in the solution. For example, the amount of solvent in the dialysis treatment can be more than 100 times, more than 200 times, less than 1000 times, or less than 800 times the volume of the cellulose-containing solution. The temperature of the dialysis treatment is not particularly limited, and is usually 10 to 50°C, and can be room temperature (20°C ± 5°C). In order to promote the reaction, the dialysis treatment can be carried out while heating or keeping warm.

[0179] As long as the effect of the present disclosure can be obtained, the material of the semipermeable membrane used in the dialysis treatment is not particularly limited, and it can be a regenerated cellulose membrane or a synthetic polymer membrane. As synthetic polymer membranes, ethylene-vinyl alcohol copolymer membranes, acrylonitrile-sodium methyl propylene sulfonate copolymer membranes, polycarbonate-polyethylene glycol copolymer membranes, etc. can be exemplified. From the viewpoint of improving the yield, the molecular weight cut-off (Molecular Weight Cut Off) of the semipermeable membrane is preferably 1000 to 5000, and more preferably 1000 to 3500.

[0180] (3) Process of recovering solid content

[0181] In this step, solid-liquid separation is performed, and the solid content precipitated by adding water or alkali is recovered.

[0182] The method of separating and recovering solid components is not particularly limited, and suction filtration, centrifugation, etc. can be appropriately utilized. In the case of filtration, the filter material is not particularly limited, as long as it is a filter material that can filter solid components. For example, as a filter material, two filter papers equivalent to those specified in JIS P3801 "filter paper (for chemical analysis)" can be used. As these two filter papers, No. 131 made by ADVANTEC is exemplified. In the case of centrifugation, a swing rotor can be used, and the solid components are precipitated and recovered under the conditions of 4000G and about 10 minutes. In addition, a general solid-liquid separation device can also be used. As the solid-liquid separation device, a screw press, a roller press, a rotary drum screen, a belt screen, a vibrating screen, a multi-plate vibration filter, etc. can be listed.

[0183] The recovered solid component mainly contains cellulose. The solid component may include at least partially esterified (e.g., formylated) cellulose. When lignocellulose or woody biomass is used as a cellulose-containing raw material, the recovered solid component may include hemicellulose and lignin as well as cellulose (or esterified cellulose). The solid component may include at least partially esterified hemicellulose and at least partially esterified lignin.

[0184] In addition, in the recovered solid component, depending on the situation, it sometimes contains components derived from organic acids, components derived from alkalis, etc. Therefore, after solid-liquid separation, the solid component can be washed. Distilled water can be used for washing. After washing, it is preferably used to dehydrate the solid component using a known method. For example, the dehydration of the solid component can use a pool washer, a diffuser cleaning machine, a double-roll press, etc. It should be noted that in the previous process, water is added to the cellulose-containing solution to precipitate the solid component and the pH of the solution is roughly neutral to the desired weak acidity, and the washing process can be omitted. That is, it is also possible to perform only dehydration without washing. In this dehydration process, a known method can also be used. In addition, a device for solid-liquid separation, washing and dehydration can also be used at one time. As such a device, an extraction separator, a valveless filter, a suction filter, a disc separator, a disc valveless filter, a disc filter, etc. can be listed.

[0185] The solid components recovered in this process can be a part of the block-shaped solids. The solid components recovered in this process can also be stored and circulated as molding materials for wooden molded products. That is, the solid components recovered in this process can be used as the above-mentioned wood particles. The preferred embodiment of the wood particles is as described above. The wood particles can be used as molding materials for thermoforming described later. Furthermore, they can be used as materials for other known thermoforming and pulp molding.

[0186] (4) A step of thermoforming the solid component.

[0187] In this step, the solid content (preferably the dehydrated solid content) or the wood pellets recovered in the previous step are thermoformed to obtain a wooden molded product having a predetermined shape.

[0188] (Solid content)

[0189] The solid components used in this process can be any solid components recovered in the previous process. They can be solid components that have been dehydrated or not. Wood pellets adjusted to a moisture content suitable for storage or transportation can be used as molding materials in this process.

[0190] (Thermoforming)

[0191] "Thermoforming" refers to the use of a mold to give a specific shape to a material that has been softened by heating to a specified temperature. As long as the wooden molded product disclosed in the present invention can be obtained, there is no particular limitation on the thermoforming method, and vacuum forming, stamping forming, compressed air forming, etc. can be appropriately used. In the manufacturing method disclosed in the present invention, the solid components or wood particles recovered in the previous process can be heated in a state where they are placed in a specified mold, and can also be further pressurized as needed. In addition, after heating or after heating and pressurization, they can be formed (trimmed) into a specified shape using known methods such as cutting. Furthermore, in the case of processing into a complex shape, a preform can also be made in advance. That is, a preform is made in a state where the solid components or wood particles are not completely dried but plasticity is maintained. By compressing, heating, and drying the preform with a mold, a wooden molded product of a desired shape can be made.

[0192] The heating temperature during molding can be 60 to 210°C, 70 to 180°C, 80 to 150°C, or 90 to 140°C. When the molding temperature is lower than 60°C, the molding time becomes longer and the number of shots decreases. When the molding temperature exceeds 210°C, the molded product may be discolored.

[0193] The pressure during molding can be about 100 to 400 Pa. As an example of specific stamping conditions, a method of stamping at 400 kg for 30 minutes (first stamping) and then at 3000 kg for 60 minutes (second stamping) can be cited. That is, after a certain degree of pressure is applied by the first press, a higher pressure is applied by the second press to obtain a more uniform wooden molded product. It can also be a continuous process using the same mold in the first stamping and the second stamping. In addition, the first press can also be used to make a preform.

[0194] Thermoforming can use known thermoforming techniques for thermosetting resins. For example, transfer molding, injection molding, injection molding (casting), compression molding, etc. can be listed. In the thermoforming of thermosetting resins, since gas is generated from the molding material during curing, a process or design for exhausting the gas is performed, so it can also be preferably used in the thermoforming process of the present disclosure.

[0195] Pulp injection molding (PIM) can also be applied to the thermoforming of solid or wood particles recovered in the previous process. That is, the solid component or wood particles are filled into a mold, and the wood molded product of the present disclosure can be obtained by heating and pressurizing.

[0196] (dry)

[0197] As long as the effects disclosed herein can be obtained, the recovered solid components can be dried before and / or after thermoforming of the wooden molded product. In addition, the recovered solid components can also be deliquored. By drying, the physical properties (specific gravity, strength, etc.) of the wooden molded product are further improved. That is, during thermoforming, the reformation of hydrogen bonds of cellulose, etc. increases, and a high specific gravity and tough wooden molded product can be obtained. From the same point of view, by drying the wooden molded product, the reformation of hydrogen bonds caused by cellulose, etc. can be increased.

[0198] It should be noted that the dehydration can be performed by pressurizing the mold after the recovered solid components or wood particles are placed in the mold, or by making the inside of the mold negative pressure. The dehydration by pressurizing the mold and the dehydration by making the inside of the mold negative pressure can also be used together. In the dehydration by pressurizing the mold and / or the dehydration by making the inside of the mold negative pressure, the dehydration by heating can also be used together. In addition, the dehydration can be performed before the heating during the first pressing, or the dehydration can be performed simultaneously with the heating.

[0199] Specifically, the recovered solid components or wood particles can be placed in a mold and left to stand while maintaining weak pressure. Through this weak pressure, moisture is squeezed out of the solid components. A weak pressure of about 1 / 100 to 1 / 1000 of the pressure in the second press during the above-mentioned thermoforming is sufficient. In addition, in order to improve the dehydration / drying efficiency, the solid components can also be heated while maintaining weak pressure. As the drying temperature, it only needs to be about 50 to 90°C. The dehydration / drying time varies depending on the amount of solid components and the dehydration / drying conditions, for example, it only needs to be about 3 hours to 12 hours.

[0200] According to the manufacturing method disclosed in the present invention, a thick wooden molded product having a predetermined thickness can be obtained without being limited to the shape of a sheet or a film. Thus, various uses of raw materials containing cellulose, which have been limited in application in the past, can be developed.

[0201] (crushed)

[0202] It also depends on the cellulose-containing raw material used, but as an arbitrary process, before dissolving the cellulose-containing raw material in the organic acid, a process of crushing the cellulose-containing raw material to obtain a cellulose-containing powder can be further included. By crushing, the cellulose-containing raw material can be made more easily dissolved by the organic acid. In the case where the cellulose-containing raw material is pulp, beating can be performed. In addition, in the case where the cellulose-containing raw material is sawdust or the like, crushing can be performed. As a pulper, a disc mill, an ejector, a mill, etc. can be listed. As a pulverizer, a pulverizer, an absolute pulverizer, a shredder, a grinder, a turbine pulverizer, etc. can be listed. This process is effective, for example, when wood cellulose, especially wood biomass, is used as the cellulose-containing raw material. For example, in order to obtain a powder of wood biomass (hereinafter sometimes referred to as "wood powder"), the wood biomass is crushed.

[0203] When the pulverizing process is carried out using woody biomass as a raw material, it is preferred to use a device (also called a "medium crusher") that can pulverize materials of tens of mm in size into materials of several mm to several hundred μm, from the viewpoint that the structure of cellulose, lignin, etc. in the woody biomass is less damaged, and the crystallinity of cellulose, the antibacterial property unique to lignin, the ultraviolet absorption property, etc. are maintained even after pulverization.

[0204] From the viewpoint of good workability, the powder preferably does not contain particles with a particle size of less than 100 μm, and more preferably does not contain particles with a particle size of 80 μm or less. The particle size of the powder is measured by a sieving classification method using a JIS standard sieve.

[0205] For example, as a method for pulverizing woody biomass, compression pulverization, impact pulverization, shear pulverization, etc. can be used. Dry pulverization or wet pulverization can be used. Preferably, dry pulverization is used, which can pulverize to micrometer level and is low in cost.

[0206] From the viewpoint of reducing the energy and cost in the pulverizing process, preferred pulverizers include: jaw crusher, gyratory crusher, crushing roller, hammer mill, roller mill, shredder, hammer crusher, Wiley mill, etc. Two or more pulverizers may also be used in combination. Preferably, a Wiley mill that pulverizes by shearing and impact is used. The pulverization of wood biomass may be continuous or intermittent. Before pulverizing by a pulverizer, the wood biomass may be cut into small pieces (flaked) using known cutters, chippers, etc. It should be noted that these pulverizers may be used not only for wood biomass, but also for pulverizing pulp. For example, in the case of pulverizing pulp, a disc grinder, a turbine grinder, and a pulverizing device combining them may be preferably used.

[0207] Example

[0208] Hereinafter, the effects of the present disclosure will be described clearly by way of examples, but the present disclosure should not be interpreted in a limitative manner based on the description of the examples.

[0209] (Test 1)

[0210] [Example 1]-[Example 3]

[0211] The raw materials (woody biomass) shown in Table 1 were used to produce wood chips of Examples 1-3 in the following order. Specifically, small pieces of the raw material (woody biomass) were crushed using a Vierli grinder equipped with a 20-mesh sieve, and then classified using a JIS standard sieve. Particles that passed through a sieve with a mesh size of 500 μm and did not pass through a sieve with a mesh size of 355 μm were collected to obtain wood powder (particle size 355 to 500 μm).

[0212] The obtained wood powder was put into a vial with a capacity of 50 ml in the amount shown in Table 1, and 10 ml of formic acid (manufactured by Nacalai Tesque Co., Ltd.) with a concentration of 80% by weight was added to the vial under a nitrogen atmosphere. Next, the vial was placed in a reduced pressure dryer and allowed to stand for 30 minutes under a reduced pressure of -0.098 MPa, then heated to 40°C under normal pressure and stirred. After 6 days, it was visually confirmed that the wood powder disappeared and a uniform solution was obtained.

[0213] Next, while cooling the vial containing the solution with ice, a 10-normal sodium hydroxide aqueous solution was added dropwise under stirring to a pH shown in Table 1, thereby performing a saponification treatment. The dripping of the sodium hydroxide aqueous solution, the foaming of the solution, and the precipitation of solids were confirmed. The obtained sample was filtered under reduced pressure, and the filtration residue was washed with distilled water until the filtrate was neutral (pH 7-8), thereby recovering the precipitated solid component. After dehydrating the obtained solid component, wood chips were obtained by heating to 80°C under a load of 2.5 kg. The yield (%) calculated from the weight of the obtained sheet and the amount of wood powder added is shown in Table 1. A photograph of the appearance of the wood chips of Example 1 is shown in Figure 1 .

[0214] [Example 4]

[0215] The type of raw material (woody biomass) and dissolution conditions are shown in Table 1. The wood chips of Example 4 were obtained in the same manner as in Example 1-3 except that dialysis treatment was performed instead of saponification treatment and water was added. The appearance photograph of the wood chips of Example 4 is shown in Figure 2It should be noted that the dialysis treatment was performed as follows: the entire liquid containing the woody biomass was transferred to a dialysis membrane (trade name "Spectra / Pore 7, MWCO1000" manufactured by Funakoshi Co., Ltd.) and immersed in distilled water. The distilled water was replaced twice a day, and the dialysis treatment was continued until the distilled water became neutral (pH 7-8).

[0216] [proportion]

[0217] According to JIS Z 8807 "Determination of density and specific gravity of solids", the apparent density (g / cm 3 The average of the five measured values ​​is shown in Table 1.

[0218] [Scanning electron microscope observation]

[0219] The surface conditions of the wood chips of Examples 1 and 4 were observed using a scanning electron microscope. The surface conditions of Example 1 are shown in Figure 3 (magnification 50 times (3A), 1000 times (3B)). The surface conditions of Example 4 are shown in Figure 4 (magnification 50 times (4A), 1000 times (4B)).

[0220] [Table 1]

[0221]

[0222]

[0223] [Example 5]

[0224] Small pieces of cedar sapwood were pulverized using a Vierli grinder equipped with a 20-mesh screen and then classified using a JIS standard sieve. Particles that passed through a 1000 μm sieve but not through a 500 μm sieve were collected to obtain wood powder (particle size 500 to 1000 μm).

[0225] Next, in a nitrogen atmosphere, the wood powder was mixed with 80 ml of formic acid (manufactured by Nacalai Tesque) having a concentration of 80 wt % so that the wood powder concentration was 2% (w / v), and the mixture was allowed to stand under a reduced pressure of -0.098 MPa for 30 minutes. Then, the mixture was heated to 40°C and stirred for 8 days under normal pressure to obtain a wood powder solution. 60 ml of a 10-equivalent sodium hydroxide solution was added dropwise to the obtained solution under ice cooling to adjust the pH to 3.0. Then, the precipitated solid component was recovered by centrifugal separation (centrifugal force: 10,000 g, time: 10 minutes). After washing the solid component with ultrapure water for more than 5 times, it was put into a stainless steel mold (star shape), and heated to 80°C for 24 hours under a load of 2.5 kg to obtain the molded body of Example 5 (thickness: 3.65-5.7 mm, yield: 82.9 g). A photograph of the appearance of the molded body of Example 5 is shown in Figure 5 .

[0226] (Test 2)

[0227] [Example 6] - [Example 11]

[0228] The raw material (woody biomass) chips shown in Tables 2 and 3 were pulverized using a Vierge mill equipped with a 20-mesh sieve, and then classified using a JIS standard sieve. Particles that passed through a sieve with a mesh size of 1000 μm but not through a sieve with a mesh size of 500 μm were collected to obtain wood powder (particle size 500 to 1000 μm).

[0229] Next, the obtained wood powder was dissolved in 80% by weight formic acid (manufactured by Nacalai Tesque Co., Ltd.) in the same manner as in Example 1. Then, a saponification treatment was performed by dropping a 10-normal sodium hydroxide solution under ice cooling. The pH of the solution after the saponification treatment is shown in Tables 2 and 3. Each of the obtained samples was filtered under reduced pressure, and the filtration residue was washed with distilled water until the filtrate was neutral (pH 7-8), thereby recovering the solid content.

[0230] Next, the recovered solid components were added to 50 ml of distilled water to prepare dispersions. The obtained dispersions were filtered, and the solid components were recovered and heated at 80° C. for 24 hours under a load of 2.5 kg to obtain wood chips with a thickness of 20-50 μm.

[0231] [Comparative Example 1]-[Comparative Example 3]

[0232] The small pieces of raw materials (woody biomass) shown in Table 4 were pulverized using a Vierge mill equipped with a 20-mesh sieve and then classified using a JIS standard sieve. Particles that passed through a sieve with a mesh size of 1000 μm but not through a sieve with a mesh size of 500 μm were collected to obtain wood powder (particle size 500 to 1000 μm).

[0233] Next, each wood powder was dissolved in 80 wt% formic acid (manufactured by Nacalai Tesque Co., Ltd.) in the same manner as in Example 1. Next, the obtained solutions were cast onto glass paper, left to stand overnight in a covered petri dish at room temperature, and then decompressed for 3 hours to obtain sheets with a thickness of 20 to 50 μm. In Comparative Examples 1 to 3, the solution was not subjected to precipitation treatment (insolubilization treatment).

[0234] [Evaluation of tensile properties]

[0235] The sheets of Examples 6-11 and Comparative Examples 1-3 were punched into dumbbell shapes (No. 7 dumbbells) to make test pieces for tensile tests. In the tensile test, a tensile tester (trade name "Universal Tensile Tester (Tensilon) RTG-1310" manufactured by A&D Corporation) was used. The tensile test was carried out in accordance with the provisions of ISO527-1 (tensile speed: 2 mm / min, distance between clamps: 20 mm, distance between markings: 12 mm), and the maximum stress (unit: MPa), maximum elongation (unit: %) and elastic modulus (Young's modulus) (unit: MPa) of Examples 6-11 and Comparative Examples 1-3 were measured (temperature 23°C, humidity 50%). The average of the measured values ​​of 5 times is shown in the following Table 2-4.

[0236] [Table 2]

[0237] Example 6 Example 7 Example 8 raw material [-] eucalyptus Fir Sapwood Fir core material Particle size [μm] 500-1000 500-1000 500-1000 Sedimentation treatment [-] Saponification (pH 11) Saponification (pH 11) Saponification (pH 11) Maximum stress [MPa] 21.6 4.9 8.3 Maximum elongation [%] 3.4 1.8 1.4 Elastic modulus [MPa] 1063 372 813

[0238] [Table 3]

[0239]

[0240]

[0241] [Table 4]

[0242] Comparative Example 1 Comparative Example 2 Comparative Example 3 raw material [-] eucalyptus Fir Sapwood Fir core material Particle size [μm] 500-1000 500-1000 500-1000 Sedimentation treatment [-] - - - Maximum stress [MPa] 3.09 2.17 0.59 Maximum elongation [%] 1.16 1.19 1.10 Elastic modulus [MPa] 335 210 84

[0243] As shown in Table 1, according to the manufacturing method of the example, a high specific gravity wood molded product can be obtained without using petroleum-based chemicals with a large environmental burden. In addition, as shown in Tables 2-4, the wood molded products of the examples subjected to precipitation treatment by adding water or alkali have excellent mechanical properties compared to the molded products of the comparative examples.

[0244] (Test 3)

[0245] In Test 3, wooden molded articles of Examples 12 and 13 were produced using a cellulose-containing raw material that contained substantially no lignin and had an extremely low hemicellulose content.

[0246] [Example 12]

[0247] 18 g of cotton linters (manufactured by Southern Cellulose, α-cellulose content 99% or more) were weighed in a 1 L volumetric flask, and 500 g of formic acid (manufactured by Nacalai Tesque) with a concentration of 80% by weight was added. Then, a vacuum pump was connected to the volumetric flask to reduce the pressure for 30 minutes, and then 382 g of formic acid with a concentration of 80% by weight and a stirring bar were added, and stirred at 500 rpm for 7 days in an oil bath at 50° C., thereby obtaining a uniform solution (concentration 2% by weight, total weight 900 g).

[0248] The obtained solution is put into an eggplant-shaped flask with a capacity of 1L, and the solvent is removed by distillation using an evaporator until the total weight of the content is about 200g to obtain a concentrated solution. The concentrated solution is put into a conical flask with a capacity of 2L, and distilled water is added in a manner that the total volume of the liquid becomes about 1L. Then, while cooling the conical flask, vigorously stirring, 10 equivalents of sodium hydroxide aqueous solution are added until the pH of the content reaches about 12. It should be noted that the pH of the content is confirmed using a commercially available pH meter. Then, distilled water is added in a manner that the total volume becomes about 1.8L, and slowly stirred overnight at room temperature, thereby precipitating the solid component. After filtering the obtained treatment solution with filter paper (ADVANTEC No. 131, diameter 150mm), the filter residue is washed with distilled water until the filtrate is neutral (pH7-8). After the filter residue is suspended in 1L of distilled water, a swing rotor is used to centrifuge at 4000G for 10 minutes, thereby reclaiming the solid component of Example 12. The solid component of Example 12 was subjected to Fourier transform infrared spectroscopy (FTIR analysis). The results showed that the solid component of Example 12 had a strong infrared absorption spectrum at 1715-1720 cm -1 There is no absorption peak derived from the formyl group in the region.

[0249] [Example 13]

[0250] The solid component of Example 13 was obtained in the same manner as in Example 12, except that no alkali was added as a precipitation treatment. Specifically, the concentrated solution obtained in the same manner as in Example 12 was placed in a 2 L Erlenmeyer flask, and distilled water was added so that the total volume of the liquid was about 1 L. Then, distilled water was added so that the total volume of the liquid was about 1.8 L, and after slowly stirring overnight at room temperature, the solid component of Example 13 was recovered by filtration, washing, and centrifugation under the same conditions as in Example 12. Fourier transform infrared spectroscopy (FTIR analysis) was performed on the solid component of Example 13, and the results confirmed that at 1715 cm -1 The infrared absorption peak originating from the formyl group is shown at .

[0251] [Adjustment and physical properties of wood moldings]

[0252] The solid components of Examples 12 and 13 were respectively placed in a mold provided with a polypropylene sheet and compacted with a spatula. Next, after repeatedly pressing the KIMTOWEL wiping paper on the surface of the solid components for dehydration 5-6 times, a polypropylene sheet and a metal plate were placed on the solid components in sequence, placed in a hot press set at a temperature of 80°C, pressed at 400 kg for 30 minutes, and then pressed at 3000 kg for 60 minutes. Then, a block weighing 2.5 kg was placed on the molded body taken out of the mold, and dried overnight in a blower dryer at 80°C. Next, the molded body was dried under reduced pressure overnight while being placed on a silica gel plate, thereby obtaining the molded bodies of Examples 12 and 13. The appearance photographs of the molded bodies of Examples 12 and 13 are shown in the following figure. Figure 6 and 7 shown.

[0253] The yield (weight %) and specific gravity (g / cm 3 ) and contact angle (degrees) are shown in Table 5. The yield is calculated as the ratio of the weight of the molded body to the weight of the raw materials used. The method for measuring specific gravity is as described above. The contact angle is measured according to the following method.

[0254] [Contact angle]

[0255] The contact angle in the present disclosure is a dynamic contact angle, which measures the change in the contact angle just after the droplet has dripped. In the determination of the dynamic contact angle, the determination of time is necessary. A contact angle meter (made by Nickcorporation) is used in the contact angle determination. The contact angle is measured 3 times in a contact angle measurement mode with a maximum measurement time of 601 seconds (0-1 seconds and 1-601 seconds) to obtain an average value. The maximum contact angle of 0-1 seconds after adding distilled water is shown in Table 5.

[0256] [Table 5]

[0257] Example 12 Example 13 raw material [-] Cotton linters Cotton linters Sedimentation treatment [-] Saponification (pH 11) Add water and mix Yield [%] 94.9 95.1 proportion <![CDATA[[g / cm 3 ]]]> 1.16 1.18 Contact Angle [Spend] 25 27

[0258] As shown in Table 5, it was confirmed that a high-specific-gravity and hydrophilic wooden molded product can be obtained from a raw material containing cellulose as a main component.

[0259] [Test 4]

[0260] [Examples 14-16]

[0261] The raw materials (woody biomass) shown in Table 6 were crushed into small pieces using a Willy's grinder equipped with a 20-mesh sieve, and then classified using a JIS standard sieve. Particles that passed through a sieve with a mesh size of 1000 μm but not through a sieve with a mesh size of 500 μm were collected to obtain wood powder (particle size 500 to 1000 μm). In Table 5, the moisture content of the fir wood powder of Example 14 was 8.40% by weight, and the moisture content of the eucalyptus wood powder of Example 16 was 10.03% by weight.

[0262] Next, 18 g of the obtained wood powder was weighed in a plastic bottle with a volume of 1 L, and 500 g of formic acid (manufactured by Nacalai Tesque Co., Ltd.) with a concentration of 80 wt %. Next, a vacuum pump was connected to the medium bottle, and after decompression for 30 minutes, 382 g of formic acid with a concentration of 80 wt % and a stirrer were added, and stirred at 300 rpm for 7 days in an oil bath at 50° C. to obtain a uniform solution (wood powder concentration 2 wt %, total weight 900 g).

[0263] The obtained solution was put into an eggplant-shaped flask with a capacity of 1L, and the solvent was distilled off using an evaporator until the total weight of the contents was about 350g to obtain a concentrated solution. The concentrated solution was put into a 2L Erlenmeyer flask, and distilled water was added to make the total volume of the liquid about 1L. Then, distilled water was added in such a way that the total volume became about 1.8L, and the mixture was slowly stirred overnight at room temperature to precipitate the solid components. After filtering the obtained treated liquid with filter paper (ADVANTEC No. 131, 150mm diameter), the filtration residue was washed with distilled water until the filtrate was neutral (pH 7-8). After suspending the filtration residue in 1L of distilled water, the solid components of Examples 14 and 16 were recovered by centrifugation at 4000G for 10 minutes using a swing rotor. The solid components of Examples 14 and 16 were subjected to Fourier transform infrared spectroscopy (FTIR analysis), and it was confirmed that at 1720cm of the infrared absorption spectrum. -1 There is an infrared absorption peak of formyl group.

[0264] [Examples 15 and 17]

[0265] Using the raw materials shown in Table 6, as a precipitation treatment, the solid components of Examples 15 and 17 were obtained in the same manner as in Examples 14 and 16, except that an alkali was added for saponification. Specifically, the concentrated solution obtained in the same manner as in Examples 14 and 16 was placed in a 2L Erlenmeyer flask, and distilled water was added so that the total volume of the liquid was about 1L. Then, while cooling the Erlenmeyer flask, a 10-normal sodium hydroxide aqueous solution was added under stirring until the pH of the contents reached about 12. Next, distilled water was added in a manner such that the total volume was about 1.8L, and after slowly stirring overnight at room temperature, the solid components of Examples 15 and 17 were recovered by filtration, washing, and centrifugation under the same conditions as in Examples 14 and 16. It should be noted that the bagasse of Example 17 used sugarcane bagasse (water content 7.34% by weight).

[0266] [Adjustment and physical properties of wood moldings]

[0267] The solid components of Examples 14-17 were respectively placed in a mold provided with a polypropylene sheet and compacted with a medicine spoon. Next, after repeatedly pressing the KIMTOWEL wiping paper on the surface of the solid components for dehydration 5-6 times, a polypropylene sheet and a metal plate were placed on the solid components in sequence, and placed in a hot press set at a temperature of 80°C, and pressed at 0.65 MPa for 30 minutes and at 9 MPa for 60 minutes. Then, a block weighing 2.5 kg was placed on the molded body taken out of the mold, and dried overnight in a blower dryer at 80°C. Next, the molded body was dried under reduced pressure overnight while being placed on a silica gel plate, thereby obtaining the molded bodies of Examples 14-17. The appearance photographs of the molded bodies of Examples 14-17 are shown in Figure 8-11 The surfaces of the molded bodies of Examples 14 to 17 were smoother and less uneven than those of the molded bodies of Examples 12 and 13. In Examples 14 to 17, by using woody biomass as a raw material, lignin or hemicellulose filled the gaps between cellulose fibers, thereby achieving smoothness.

[0268] Yield (wt%), thickness (mm), specific gravity (g / cm 3 ), contact angle, ash content (wt%) and total lignin content (wt%) are shown in Table 6. The yield, specific gravity and contact angle were determined as described above. The ash content and total lignin content were determined according to the NREL method. The specific method is as follows.

[0269] [Ash content]

[0270] The samples collected from each molded body were placed in an electric furnace and treated according to the following temperature program: kept at 105° C. for 12 minutes, heated to 250° C. at 10° C. / min, kept at 250° C. for 30 minutes, heated to 575° C. at 20° C. / min, kept at 575° C. for 3 hours, and cooled to 105° C. The residue after treatment was weighed, and the ratio relative to the weight of the sample before treatment was calculated as the ash content (weight %).

[0271] [Total lignin content]

[0272] 300 mg of sample was collected from each molded body, crushed as needed, and put into a test tube together with 3.0 ml of sulfuric acid with a concentration of 72% by weight, and allowed to stand in a water bath at 30°C for hydrolysis. The sample that formed lumps every 5-10 minutes was crushed with a glass rod, and after standing for 60 minutes, 84 ml of deionized water was added to the test tube to adjust the sulfuric acid concentration to 4% by weight. Then, it was further hydrolyzed at 121°C for 1 hour in an autoclave. The obtained reaction solution was filtered, and the filtered residue was washed with water to obtain a filtrate containing acid-soluble lignin and a filtered residue containing acid-insoluble lignin. The amount of acid-insoluble lignin was obtained by measuring the dry weight of the filtered residue. In addition, for the obtained filtrate, 4% sulfuric acid was used as a reference cell, the absorbance at 205nm was measured, and the amount of acid-soluble lignin in the filtrate was calculated using an absorption coefficient of 110 (L / g·cm). The acid-insoluble lignin amount and the acid-soluble lignin amount were measured twice, respectively, and the average value was calculated. The total amount of the obtained acid-insoluble lignin and acid-soluble lignin was taken as the total lignin amount, and the ratios of each relative to the total weight of the measured sample are shown in Table 6.

[0273] [Table 6]

[0274]

[0275]

[0276] [Sugar composition analysis]

[0277] For the molded bodies of Examples 14-16, the sugar composition analysis was performed using the NREL method. In detail, samples were collected from each molded body, hydrolyzed under the same conditions as the analysis method for the total lignin amount, and the reaction liquid was filtered to obtain a filtrate. After adding an appropriate amount of calcium carbonate to the obtained filtrate for neutralization, centrifugal separation (centrifugal force: 10000g, time: 10 minutes) was performed to collect the supernatant. After filtering the supernatant with a filter with a pore size of 0.2μm, it was used for high performance liquid chromatography (HPLC determination) under the following measurement conditions.

[0278] Chromatographic columns: two Aminex HPX-87P (manufactured by Biorad).

[0279] Mobile phase: ultrapure water.

[0280] Flow rate: 0.6 ml / min.

[0281] Column temperature: 65°C.

[0282] Detector: Refractive Index Detector (RID).

[0283] Retention time: 50min.

[0284] Injection volume: 5μl.

[0285] For the six monosaccharides (cellobiose, glucose, xylose, galactose, arabinose, and mannan), a standard curve was prepared with a concentration range of 0.1-5.0 mg / ml. Based on the obtained HPLC measurement values, the content of each monosaccharide after hydrolysis in each molded body was determined, and converted into polysaccharides (glucan, xylan, galactan, arabinan, and mannan), respectively, to determine the sugar composition of Examples 14-16. The obtained results are shown in Table 7.

[0286] [Evaluation of tensile and flexural properties]

[0287] Test pieces (1 cm wide and 5 cm long) for tensile testing and bending testing were cut out from the molded bodies of Examples 14 to 16, respectively. The measuring device used was a "universal tensile testing machine (TENSILON) RTG-1310" manufactured by A&D Co., Ltd., and the tensile properties and bending properties were measured in accordance with the provisions of ISO527-1 (temperature 23°C, humidity 50%). The measuring conditions are as follows. The results are shown in Table 7 below.

[0288] Tensile test

[0289] Load sensor: 1000N.

[0290] Tensile speed: 10 mm / min.

[0291] Distance between fixtures: 20mm.

[0292] Bending test (three-point bending test)

[0293] Load sensor: 1000N.

[0294] Bending speed: 2 mm / min.

[0295] Distance between pivot points: 30mm.

[0296] [Table 7]

[0297]

[0298]

[0299] From the results of Test 4, it can be confirmed that in the examples obtained with cellulose-containing raw materials, especially wood biomass as raw materials, smooth wood molded products with few cracks and deformations can be obtained. In addition, as shown in Table 7, it is confirmed that the bending properties (maximum stress and elastic modulus) of the wood molded products of Examples 14-17 are equal to or higher than those of general-purpose resins such as ABS resin (bending strength 64MPa, bending modulus 2500MPa) and polycarbonate (bending strength 85MPa, bending modulus 2300MPa). According to the above evaluation results, the superiority of the present disclosure is obvious. The manufacturing method disclosed in the present disclosure can be applied to the utilization of various plant-based biomass.

Claims

1. A wooden molded product comprising cellulose as a main component and satisfying any one or both of the following (1) and (2): (1) The flexural modulus obtained in the flexural test according to ISO527-1 is 4000 MPa or more; (2) The flexural strength obtained in a flexural test in accordance with the provisions of ISO527-1 is 50 MPa or more.

2. The wooden molded product according to claim 1, wherein: The wooden molded product further comprises lignin, and the specific gravity of the wooden molded product is 0.5 g / cm 3 above.

3. The wooden molded product according to claim 1 or 2, wherein: The specific gravity of the wooden molded product is 0.9 g / cm 3 above.

4. The wooden molded product according to claim 1 or 2, wherein: In its infrared absorption spectrum, at 1715-1720cm -1 The area shows the absorption peak.

5. The wooden molded product according to claim 1 or 2, wherein: The wooden molded product further comprises a fibrous substance having a cellulose I-type crystal structure.

6. The wooden molded product according to claim 1, wherein: The wooden shaped product further comprises lignin, The total lignin content is 15% by weight or more and 80% by weight or less.

7. The wooden molded product according to claim 1, wherein: The wooden molded product also contains hemicellulose and lignin, The total lignin content is 20% by weight or more and 45% by weight or less, The composition ratio of polysaccharides obtained by sugar composition analysis satisfies the following conditions: Dextran: 40% by weight or more and 80% by weight or less, Xylan: 0.1 wt% or more and 3.0 wt% or less, Arabinan: 0.2 wt% or more and 3.0 wt% or less, Mannan: 1.0 wt% or more and 5.0 wt% or less.

8. A wood particle, which is a molding material for the wood molded product according to claim 1 or 2, The wood particles contain cellulose, hemicellulose and lignin, In the infrared absorption spectrum of the wood particles, at 1715-1720 cm -1 The region shows an absorption peak. The total lignin content is 20% by weight or more and 45% by weight or less, The composition ratio of polysaccharides obtained by sugar composition analysis satisfies the following conditions: Dextran: 40% by weight or more and 80% by weight or less, Xylan: 0.1 wt% or more and 3.0 wt% or less, Arabinan: 0.2 wt% or more and 3.0 wt% or less, Mannan: 1.0 wt% or more and 5.0 wt% or less.

9. A wood particle, which is a molding material for the wood molded product according to claim 1 or 2, The wood particles contain cellulose, hemicellulose and lignin, The cellulose has a cellulose I type crystal structure, The total lignin content is 10% by weight or more and 45% by weight or less, The composition ratio of polysaccharides obtained by sugar composition analysis satisfies the following conditions: Dextran: 55% by weight or more and 80% by weight or less, Xylan: 0.1 wt% or more and 5.0 wt% or less, Arabinan: 0.2 wt% or more and 1.0 wt% or less, Mannan: 1.0 wt% or more and 3.0 wt% or less.

10. A method for manufacturing a wooden molded product, which is the method for manufacturing a wooden molded product according to claim 1, comprising: A step of dissolving the cellulose-containing raw material in an organic acid to obtain a cellulose-containing solution; A step of adding water or alkali to the cellulose-containing solution to precipitate solid components; a step of recovering the solid component; and The recovered solid component is subjected to a thermoforming step, wherein: The main component of the solid component is cellulose.

11. The method for producing a wooden molded product according to claim 10, wherein: In the step of precipitating the solid content, the pH of the cellulose-containing solution is adjusted to 3 or higher.

12. The method for producing a wooden molded product according to claim 10 or 11, wherein: The recovered solid component is put into a mold and thermoformed at a temperature of 60° C. to 210° C. and a pressure of 100 Pa to 400 Pa.

13. The method for producing a wooden molded product according to claim 10 or 11, wherein: The method further comprises: a step of deliquoring the recovered solid components before thermoforming.

14. The method for producing a wooden molded product according to claim 10 or 11, wherein: The method further includes the step of pulverizing the cellulose-containing raw material to obtain cellulose-containing powder before dissolving the cellulose-containing raw material in the organic acid.

Citation Information

Patent Citations

  • Method of manufacturing cellulose acetate, high temperature steam reactor vessel used in the same method, and superheated steam generator used in the same method

    CN101062956A

  • Method to decompose the natural structure of biomass

    CN101283143A

  • Efficient method for separating lignocellulosic raw material

    CN105507051A

  • Processing method for separating out lignin from biomass efficiently

    CN106079000A

  • Cellulose acetate and method for producing cellulose acetate

    CN109952320A