Method and apparatus for producing silicon single crystal, and method for producing silicon wafer

By taking and processing the mirror image of the quartz crucible and quantitatively evaluating its deformation and eccentricity, the reduction in the quality of silicon single crystals and the risk of accidents caused by crucible deformation is solved, and the yield rate of silicon wafers is improved.

CN118984892APending Publication Date: 2024-11-19SUMCO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380032892.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-08
Filing Date
2023-02-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the prior art, quartz crucibles are prone to deformation at high temperatures, resulting in a decrease in the quality of silicon single crystals and the risk of accidents in the crystallisation and lifting process, and there is a lack of a method for quantitatively evaluating deformation.

Method used

By taking a mirror image of the quartz crucible at a specified time interval, using image processing technology to capture the position change of the crucible, calculate its deformation or eccentricity, use pixel longitudinal luminance differential value to detect the deformation of the upper end of the crucible, and set the detection line to evaluate The amount of change in the crucible.

Benefits of technology

An objective quantitative evaluation of the deformation and eccentricity of the quartz crucible is achieved, which prevents the reduction of the quality of silicon single crystals and accidents caused by the deformation of the crucible, and improves the yield rate of the silicon wafer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984892A_ABST
    Figure CN118984892A_ABST
Patent Text Reader

Abstract

[Problem] To provide a method and a device for producing a silicon single crystal with which it is possible to quantitatively evaluate the deformation, the presence or absence of eccentricity, or the size of deformation and eccentricity of a quartz crucible. [Solution] The present invention is a method for producing a silicon single crystal in which a silicon single crystal is pulled up from a silicon melt (2) in a quartz crucible (11), the method comprising: acquiring, at predetermined time intervals, an image including a mirror image (11M) of the quartz crucible (11) reflected on a melt surface (2a) of the silicon melt (2); deformation or eccentricity of the quartz crucible 11 is evaluated on the basis of a time change in the position of a mirror image 11M of the quartz crucible 11 reflected by a plurality of images acquired during at least one rotation of the quartz crucible 11.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method and apparatus for producing a silicon single crystal using the Czochralski method (CZ method), and more particularly to a method for evaluating deformation or eccentricity of a quartz crucible. In addition, the present invention relates to a method for producing a silicon wafer using such a silicon single crystal. Background Art

[0002] Most silicon wafers that become substrate materials for semiconductor devices are manufactured by processing silicon single crystal ingots manufactured using the CZ method. In the CZ method, polycrystalline silicon raw materials are melted in a quartz crucible to generate silicon melt, a seed crystal is immersed in the silicon melt, and the seed crystal is slowly pulled up while the quartz crucible and the seed crystal are rotated, thereby growing a large single crystal at the lower end of the seed crystal. According to the CZ method, the yield rate of large-diameter silicon single crystals can be improved.

[0003] A quartz crucible is a container made of quartz glass that holds molten silicon. Therefore, the quartz crucible is required to be highly durable, not deforming at high temperatures above the melting point of silicon and being able to withstand long-term use. If the quartz crucible is deformed during the crystallization pulling process, the shape and quality of the silicon single crystal will change. In the most serious case, the crucible wall will contact the structure in the furnace and cause an accident. In order to prevent such accidents from happening, it is preferred to monitor the deformation of the quartz crucible. For example, Patent Document 1 describes a method for detecting the deformation of the crucible based on the rapid change in the height of the molten liquid surface accompanying the change in the volume of the crucible.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2021-109826 Summary of the invention

[0007] Problems to be solved by the invention

[0008] In the raw material melting process of heating and melting the polysilicon raw material in the quartz crucible, a large heat load is applied to the quartz crucible due to the radiant heat from the heater, so the upper end of the quartz crucible is prone to tilting inward. When such a crucible deformation occurs, the crucible contacts the heat shield during the single crystal pulling process, and the crystallization pulling process cannot be continued. In addition, even if the crystallization pulling process can be continued, the convection of the silicon melt in the quartz crucible changes, which becomes the main cause of oxygen anomalies in the silicon single crystal. Therefore, it is necessary to confirm the deformation of the crucible during the crystallization pulling process, especially in the raw material melting process that is prone to cause crucible deformation. However, in the past, there was only a method for staff to make judgments by visually observing the furnace, and there was no method for quantitatively evaluating the deformation of the crucible.

[0009] The present invention has been made in view of the above problems, and its object is to provide a method and apparatus for producing a silicon single crystal and a method for producing a silicon wafer that can quantitatively evaluate the presence or absence of deformation and eccentricity of a quartz crucible or the magnitude of the deformation and eccentricity.

[0010] Solutions to Solve Problems

[0011] In order to solve the above-mentioned problems, a method for producing a silicon single crystal according to the present invention is a method for producing a silicon single crystal by pulling a silicon single crystal from a silicon melt in a quartz crucible, characterized in that an image including a mirror image of the quartz crucible reflected on a melt surface of the silicon melt is obtained at a predetermined time interval, and deformation or eccentricity of the quartz crucible is evaluated based on a temporal change in the position of the mirror image of the quartz crucible reflected in a plurality of images obtained while the quartz crucible rotates at least once. According to the present invention, shape changes caused by deformation and eccentricity of the quartz crucible can be objectively captured, and accidents caused by deformation of the quartz crucible and reduction in quality of the silicon single crystal can be prevented before they occur.

[0012] According to the method for manufacturing a silicon single crystal of the present invention, it is preferred that the position of the upper end of the aforementioned quartz crucible is detected based on the mirror image of the aforementioned quartz crucible, and the deformation amount or eccentricity of the aforementioned upper end is calculated based on the temporal change of the position of the aforementioned upper end. In this way, the deformation of the upper end of the quartz crucible and the degree of eccentricity of the crucible can be objectively evaluated. In addition, the deformation of only the upper end of the quartz crucible, which has no effect on the height change of the melt surface, can also be evaluated.

[0013] According to the method for producing a silicon single crystal of the present invention, the upper end of the quartz crucible is preferably detected based on the differential value of the vertical brightness of the pixels in the image, thereby objectively evaluating the degree of deformation and eccentricity of the upper end of the quartz crucible.

[0014] According to the method for manufacturing a silicon single crystal of the present invention, it is preferred that a detection line for the position of the upper end portion is set in a plane including the optical axis of a camera that captures the image, and the amount of change of the quartz crucible is calculated based on the temporal change of the position of the mirror image of the quartz crucible on the detection line. In this way, the amount of change of the quartz crucible can be easily calculated.

[0015] The method for manufacturing a silicon single crystal according to the present invention preferably calculates the amount of change of the quartz crucible based on the plurality of images obtained during a period from a raw material melting step of melting the silicon raw material in the quartz crucible to a liquid contact step of bringing the seed crystal into contact with the silicon melt. Since a large heat load is applied to the quartz crucible in the raw material melting step, the upper end of the quartz crucible is prone to collapse. By calculating the amount of change of the quartz crucible in such a raw material melting step, accidents caused by deformation of the quartz crucible and a decrease in the single crystal yield can be prevented before they occur.

[0016] In addition, the silicon single crystal manufacturing apparatus according to the present invention is characterized by comprising: a quartz crucible for holding silicon melt; a heater disposed around the quartz crucible and heating the silicon melt; a crucible driving mechanism for rotating and lifting the quartz crucible; a crystallization pulling mechanism for pulling a silicon single crystal from the silicon melt; a heat shield disposed above the quartz crucible so as to surround the silicon single crystal pulled from the silicon melt; a camera for photographing a melt surface of the silicon melt visible through an opening of the heat shield from obliquely above; and an image processing unit for processing images photographed by the camera, wherein the camera acquires images including a mirror image of the quartz crucible reflected on the melt surface at predetermined time intervals, and the image processing unit evaluates deformation or eccentricity of the quartz crucible based on temporal changes in the position of the mirror image of the quartz crucible reflected in a plurality of images acquired while the quartz crucible rotates at least one revolution. According to the present invention, it is possible to objectively detect the shape change caused by the deformation and eccentricity of the quartz crucible, and prevent accidents caused by the deformation of the quartz crucible and the reduction in the quality of the silicon single crystal from happening.

[0017] In the present invention, the image processing unit preferably detects the position of the upper end of the quartz crucible based on the mirror image of the quartz crucible, and calculates the deformation or eccentricity of the upper end based on the temporal change of the position of the upper end, thereby being able to objectively evaluate the deformation of the upper end of the quartz crucible and the degree of eccentricity of the crucible.

[0018] In the present invention, the image processing unit preferably detects the upper end of the quartz crucible based on a differential value of the vertical brightness of pixels in the image, thereby objectively evaluating the degree of deformation and eccentricity of the upper end of the quartz crucible.

[0019] In the present invention, the image processing unit preferably sets a detection line for the position of the upper end portion in a plane including an optical axis of a camera that captures the image, and calculates the amount of change of the quartz crucible based on a temporal change in the position of the mirror image of the quartz crucible on the detection line. In this way, the amount of change of the quartz crucible can be easily calculated.

[0020] In the present invention, the image processing unit preferably calculates the amount of change of the quartz crucible based on the plurality of images acquired during a period from a raw material melting step of melting the silicon raw material in the quartz crucible to a liquid contact step of bringing the seed crystal into contact with the silicon melt. By calculating the amount of change of the quartz crucible in such a raw material melting step, accidents and reductions in single crystal yields caused by deformation of the quartz crucible can be prevented before they occur.

[0021] Furthermore, the method for manufacturing a silicon wafer according to the present invention is characterized in that the silicon single crystal manufactured by the method for manufacturing a silicon single crystal according to the present invention is processed to manufacture a silicon wafer. According to the present invention, the manufacturing yield of the silicon wafer can be improved.

[0022] Effects of the Invention

[0023] According to the present invention, a method and apparatus for producing a silicon single crystal and a method for producing a silicon wafer can be provided, which can quantitatively evaluate the presence or absence of deformation and eccentricity of a quartz crucible and the magnitude of the deformation and eccentricity.

[0024] Brief description of the attached figure

[0025] Figure 1 1 is an explanatory diagram of a method for producing a silicon single crystal according to an embodiment of the present invention, and is a schematic cross-sectional view showing the configuration of a single crystal production apparatus.

[0026] Figure 2 1 is a flowchart showing a process of manufacturing a silicon single crystal according to the present embodiment.

[0027] Figure 3 It is a schematic cross-sectional view showing the shape of a silicon single crystal ingot.

[0028] Figure 4 This is a diagram for explaining a method of monitoring deformation of a quartz crucible, and is a conceptual diagram of a CZ pulling furnace in a raw material melting step.

[0029] Figure 5 (a) and (b) are schematic diagrams of images captured by a camera of silicon melt in a quartz crucible, wherein (a) shows a state where the upper end of the quartz crucible is not deformed, and (b) shows a state where the upper end of the quartz crucible is deformed.

[0030] Figure 6 It is an explanatory diagram of a method for determining the position of the upper end portion of a quartz crucible.

[0031] Figure 7 : is a graph showing an example of the measurement results of the deformation amount of the quartz crucible, wherein the horizontal axis represents the crucible rotation angle (degrees), and the vertical axis represents the position of the edge of the crucible mirror image (pixel). DETAILED DESCRIPTION

[0032] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0033] Figure 1 1 is an explanatory diagram of a method for producing a silicon single crystal according to an embodiment of the present invention, and is a schematic cross-sectional view showing the configuration of a single crystal production apparatus.

[0034] like Figure 1As shown, the single crystal manufacturing apparatus 1 includes a water-cooled chamber 10, a quartz crucible 11 for holding a silicon melt 2 in the chamber 10, a graphite crucible 12 for holding the quartz crucible 11, a rotating shaft 13 for supporting the graphite crucible 12, a crucible driving mechanism 14 for rotating and lifting the quartz crucible 11 via the rotating shaft 13 and the graphite crucible 12, a heater 15 arranged around the graphite crucible 12, a heat insulating material 16 arranged outside the heater 15 and along the inner surface of the chamber 10, a heat shield 17 arranged above the quartz crucible 11, a pulling wire 18 arranged above the quartz crucible 11 and coaxially with the rotating shaft 13, a crystal pulling mechanism 19 arranged above the chamber 10, a camera 20 for photographing the inside of the chamber 10, an image processing unit 21 for processing an image photographed by the camera 20, and a control unit 22 for controlling each part of the single crystal manufacturing apparatus 1.

[0035] The chamber 10 is composed of a main chamber 10a and a slender cylindrical pulling chamber 10b connected to the upper opening of the main chamber 10a. A quartz crucible 11, a graphite crucible 12, a heater 15 and a heat shield 17 are arranged in the main chamber 10a. A gas inlet 10c for introducing an inert gas (purge gas) such as argon and a dopant gas into the chamber 10 is arranged in the pulling chamber 10b, and a gas exhaust port 10d for exhausting the atmospheric gas in the chamber 10 is arranged at the lower part of the main chamber 10a. In addition, a peep window 10e is arranged at the upper part of the main chamber 10a so that the growth status of the silicon single crystal 3 can be observed.

[0036] The quartz crucible 11 is a container made of quartz glass having a cylindrical side wall and a curved bottom. In order to maintain the shape of the quartz crucible 11 softened by heating, the graphite crucible 12 is closely attached to the outer surface of the quartz crucible 11 and is held in a manner of wrapping the quartz crucible 11. The quartz crucible 11 and the graphite crucible 12 constitute a double-layered crucible that supports the silicon melt 2 in the chamber 10.

[0037] The graphite crucible 12 is fixed to the upper end of the rotating shaft 13, and the lower end of the rotating shaft 13 passes through the bottom of the chamber 10 and is connected to the crucible driving mechanism 14 provided outside the chamber 10. The graphite crucible 12, the rotating shaft 13, and the crucible driving mechanism 14 constitute a crucible driving mechanism for rotating and lifting the quartz crucible 11. The rotation and lifting of the quartz crucible 11 driven by the crucible driving mechanism 14 are controlled by the control unit 22.

[0038] The heater 15 is used to melt the silicon raw material filled in the quartz crucible 11 and generate the silicon melt 2 while maintaining the molten state of the silicon melt 2. The heater 15 is a carbon resistance heating heater, and is provided so as to surround the quartz crucible 11 in the graphite crucible 12. Furthermore, a heat insulating material 16 is provided outside the heater 15 so as to surround the heater 15, thereby improving the heat preservation in the chamber 10. The output power of the heater 15 is controlled by the control unit 22.

[0039] A heat shield 17 is provided to suppress temperature fluctuations of the silicon melt 2 and provide appropriate heat distribution near the crystal growth interface, while preventing the silicon single crystal 3 from being heated by radiation heat from the heater 15 and the quartz crucible 11. The heat shield 17 is a substantially cylindrical member made of graphite, and is provided to cover the upper region of the silicon melt 2 except for the pulling path of the silicon single crystal 3.

[0040] The diameter of the opening 17a at the lower end of the heat shield 17 is larger than the diameter of the silicon single crystal 3, thereby ensuring the pulling path of the silicon single crystal 3. In addition, the outer diameter of the lower end of the heat shield 17 is smaller than the diameter of the quartz crucible 11, and the lower end of the heat shield 17 is located inside the quartz crucible 11. Therefore, even if the upper end of the quartz crucible 11 is raised to a position higher than the lower end of the heat shield 17, the heat shield 17 will not interfere with the quartz crucible 11.

[0041] The amount of the melt in the quartz crucible 11 decreases as the silicon single crystal 3 grows. The quartz crucible 11 is raised so that the gap between the melt surface 2a and the heat shield 17 (gap value h G ) is constant, thereby suppressing the temperature variation of the silicon melt 2, while making the flow rate of the gas flowing near the melt surface 2a constant and controlling the evaporation amount of the dopant from the silicon melt 2. By such gap control, the stability of the crystal defect distribution, oxygen concentration distribution, resistivity distribution, etc. of the silicon single crystal 3 in the pulling axis direction can be improved.

[0042] A metal wire 18 serving as a pulling axis of the silicon single crystal 3 and a crystallization pulling mechanism 19 for pulling the silicon single crystal 3 by winding the metal wire 18 are provided above the quartz crucible 11, and they constitute a crystallization pulling mechanism for pulling the silicon single crystal 3. The crystallization pulling mechanism 19 has a function of rotating the silicon single crystal 3 together with the metal wire 18. The crystallization pulling mechanism 19 is controlled by the control unit 22. The crystallization pulling mechanism 19 is arranged above the pulling chamber 10b, and the metal wire 18 extends from the crystallization pulling mechanism 19 through the pulling chamber 10b to the bottom, and the front end of the metal wire 18 reaches the internal space of the main chamber 10a. Figure 1The silicon single crystal 3 in the process of being grown is shown suspended on the wire 18. When the silicon single crystal 3 is pulled up, the wire 18 is slowly pulled up while the quartz crucible 11 and the silicon single crystal 3 are rotated, thereby growing the silicon single crystal 3.

[0043] The camera 20 is installed outside the chamber 10. The camera 20 is, for example, a CCD camera, and images the inside of the chamber 10 through a viewing window 10e formed on the chamber 10. The camera 20 is installed at a predetermined angle relative to the vertical direction, and the camera 20 has a camera axis (optical axis) that is inclined relative to the pulling axis of the silicon single crystal 3. That is, the camera 20 images the upper region of the quartz crucible 11 including the circular opening 17a of the heat shield 17 and the melt surface 2a of the silicon melt 2 from obliquely above.

[0044] The camera 20 is connected to the image processing unit 21, and the image processing unit 21 is connected to the control unit 22. In the pulling process of the silicon single crystal 3, the image processing unit 21 calculates the crystal diameter near the solid-liquid interface based on the outline pattern of the single crystal reflected in the image captured by the camera 20. In addition, the image processing unit 21 calculates the distance (gap value h) from the heat shield 17 to the melt surface based on the position of the mirror image of the heat shield 17 reflected on the melt surface in the image captured by the camera 20. G ).

[0045] The control unit 22 controls the crystal diameter by controlling the crystal pulling speed based on the crystal diameter data obtained from the image captured by the camera 20. Specifically, when the measured value of the crystal diameter is greater than the target diameter, the crystal pulling speed is increased, and when the measured value of the crystal diameter is less than the target diameter, the pulling speed is reduced. In addition, the control unit 22 controls the crystal length data of the silicon single crystal 3 obtained by the sensor output of the crystal pulling mechanism 19 and the gap value h obtained from the image captured by the camera 20. G The movement amount (crucible rising speed) of the quartz crucible 11 is controlled by adjusting the liquid level (liquid surface level) so as to achieve a predetermined gap value.

[0046] Figure 2 : is a flow chart showing the manufacturing process of silicon single crystal according to this embodiment. Figure 3 It is a schematic cross-sectional view showing the shape of a silicon single crystal ingot.

[0047] like Figure 2As shown, the manufacturing process of the silicon single crystal according to the present embodiment includes: a raw material melting step S11 of heating the silicon raw material in the quartz crucible 11 with the heater 15 to generate a silicon melt 2; a crucible deformation detection step S12 of evaluating whether the quartz crucible 11 is deformed or the size of the deformation due to the influence of the raw material melting step S11; a liquid contact step S13 of lowering the seed crystal installed at the front end of the metal wire 18 to contact the silicon melt 2; and a crystallization growth step (S14 to S17) of slowly pulling up the seed crystal to grow a single crystal while maintaining the contact state with the silicon melt 2.

[0048] like Figure 2 and Figure 3 As shown, in the crystal growth process, the following are performed in sequence: a necking step S14 for forming a neck portion 3a with a narrowed crystal diameter to eliminate dislocations; a shoulder growth step S15 for forming a shoulder portion 3b whose crystal diameter gradually increases as the crystal grows; a main body growth step S16 for forming a main body 3c that maintains a specified crystal diameter; and a tail growth step S17 for forming a tail portion 3d whose crystal diameter gradually decreases as the crystal grows.

[0049] Thereafter, a cooling step S18 is performed to separate the silicon single crystal 3 from the melt surface 2a and cool the silicon single crystal 3. Figure 3 The silicon single crystal ingot 3I shown has a neck portion 3a, a shoulder portion 3b, a main body portion 3c and a tail portion 3d. The silicon single crystal ingot 3I is subjected to peripheral grinding, slicing, polishing, etching, double-side grinding, single-side grinding, cleaning and other processes in sequence to manufacture a silicon wafer.

[0050] In the present embodiment, the melt surface 2a of the silicon melt 2 in the quartz crucible 11 is photographed by the camera 20 between the raw material melting step S11 and the liquid contact step S13, and the deformation of the quartz crucible 11 is detected based on the change of the image of the quartz crucible 11 reflected by the image captured by the camera 20 (crucible deformation detection step S12). The reason for performing the deformation detection of the quartz crucible 11 between the raw material melting step S11 and the liquid contact step S13 is that it becomes difficult to capture the image of the quartz crucible 11 reflected on the melt surface 2a due to the presence of the silicon single crystal 3 after the shoulder growth step S15. In addition, if the sign of a large deformation of the quartz crucible 11 can be detected at an early stage, it is also easy to determine whether to continue / stop the crystal pulling.

[0051] Figure 4 This is a diagram for explaining a method of detecting deformation of the quartz crucible 11 , and is a conceptual diagram of a CZ pulling furnace in the raw material melting step S11 .

[0052] like Figure 4As shown, in order to detect the deformation of the quartz crucible 11 in the raw material melting step S11, the melt surface 2a is photographed by the camera 20. The camera 20 can photograph the melt surface 2a of the silicon melt 2 which can be seen through the opening 17a of the heat shield 17. Since the heat shield 17 is present between the camera 20 and the quartz crucible 11, the camera 20 cannot directly capture the real image of the quartz crucible 11. The mirror image 11M of the quartz crucible 11 is reflected on the melt surface 2a, but if the upper end 11e of the quartz crucible 11 falls inward, the position of the edge of the mirror image 11M of the quartz crucible 11 reflected on the melt surface 2a also changes, so the deformation of the quartz crucible 11 can be detected based on the change of the mirror image 11M of the quartz crucible 11.

[0053] When the raw material melting step S11 is started, the solid silicon raw material gradually melts and the amount of the silicon melt 2 increases. Since the amount of the silicon melt 2 is temporarily small and the solid raw material remains after the raw material melting step S11 is started, the image of the quartz crucible 11 reflected on the melt surface 2a cannot be accurately captured by the camera 20. In addition, since a large heat load has not been applied to the quartz crucible 11, the quartz crucible 11 will not be greatly deformed. When the melting of the raw material proceeds to a certain extent and the amount of the silicon melt 2 in the quartz crucible 11 becomes sufficient, the deformation of the quartz crucible 11 can be detected because the edge of the image of the upper end 11e of the quartz crucible 11 is reflected on the melt surface 2a. In addition, when the amount of the silicon melt 2 increases sufficiently, the deformation of the quartz crucible 11 due to the influence of the heat load becomes visible.

[0054] When the quartz crucible 11 is at a relatively high position, the distance from the lower end of the heat shield 17 to the melt surface 2a (gap value h G ) is small, the mirror image of the upper end portion 11e of the quartz crucible 11 is blocked by the heat shield 17, and the edge of the mirror image cannot be observed. However, when the quartz crucible 11 is sufficiently lowered, the edge of the mirror image of the upper end portion 11e of the quartz crucible 11 can be included in the field of view of the camera 20. Therefore, in the crucible deformation detection step S12, it is desirable to set the melt surface 2a at a lower position than in the crystal growth step (particularly the main body growth step S16) to calculate the deformation amount of the quartz crucible 11.

[0055] Figure 5 (a) and (b) are schematic diagrams of images captured by a camera 20 that captures the melt surface 2a of the silicon melt 2 in the quartz crucible 11, wherein (a) represents an image when the upper end of the quartz crucible 11 is not deformed, and (b) represents an image when the upper end of the quartz crucible 11 is deformed.

[0056] like Figure 5As shown in (a) and (b), the melt surface 2a of the silicon melt 2 in the quartz crucible 11 can be observed through the opening 17a of the heat shield 17 provided above the quartz crucible 11. In the image captured by the camera 20, the blackened area is the real image 17R of the heat shield 17, and the area inside the opening 17a of the heat shield 17 is the melt surface 2a.

[0057] Since the melt surface 2a is a mirror surface, the upper end of the quartz crucible 11 and the upper end of the heater 15 are reflected on the melt surface 2a. In real space, the upper end of the heater 15 is located above the upper end of the quartz crucible 11, and the positional relationship between the quartz crucible 11 and the heater 15 reflected on the melt surface 2a is reversed up and down, and the lower side in the captured image corresponds to the upper side in real space. Therefore, the edge of the mirror image of the quartz crucible 11 is located above the edge of the mirror image of the heater 15. The area between the arc-shaped edge line E1 of the heat shield 17 and the arc-shaped edge line E2 of the upper end of the quartz crucible 11 is the mirror image 11M of the quartz crucible 11, and the area between the arc-shaped edge line E2 of the upper end of the quartz crucible 11 and the arc-shaped edge line E3 of the upper end of the heater 15 is the mirror image 15M of the heater 15.

[0058] like Figure 5 As shown in (a), the edge line E2 of the mirror image 11M of the upper end 11e of the undeformed quartz crucible 11 is in a beautiful arc shape. Figure 4 When the upper end 11e of the quartz crucible 11 is tilted inward, Figure 5 As shown in (b), the mirror image 11M of the upper end 11e of the quartz crucible 11 changes in an arc shape, and a portion of the edge line E2 of the mirror image 11M moves downward in the longitudinal direction (Y direction) of the image. Since the quartz crucible 11 rotates at a certain speed, the position of the upper end of the quartz crucible 11 moves downward when observed on the preset detection line L0. Therefore, by measuring the position change of the intersection point P2 of the edge line E2 of the mirror image 15M of the quartz crucible 11 and the detection line L0 during one rotation of the quartz crucible 11, the deformation amount of the upper end 11e of the quartz crucible 11 can be calculated.

[0059] The detection line L0 is preferably set within a plane including the optical axis of the camera 20. Thus, the deformation amount of the upper end portion 11e of the quartz crucible 11 can be easily calculated.

[0060] Figure 6 It is an explanatory diagram of a method for determining the position of the edge of the mirror image of the quartz crucible 11 .

[0061] like Figure 6As shown in FIG. 1 , the position of the edge of the mirror image of the quartz crucible 11 on the detection line L0 can be obtained from the differential value of the luminance distribution in the longitudinal direction (Y direction) of the captured image. When observing the luminance distribution in the longitudinal direction of the captured image (the upper graph), it can be seen that at the boundary position P1 (refer to FIG. 1 ) between the real image 17R of the heat shield 17 and the mirror image 11M of the quartz crucible 11, the edge of the mirror image of the quartz crucible 11 is located at the boundary position P2 (refer to FIG. 1 ). Figure 5 The luminance of (a) and (b) changes greatly, and also changes greatly at the boundary position P2 between the mirror image of the quartz crucible 11 and the mirror image of the heater 15 .

[0062] Therefore, if the differential value of the brightness distribution in the longitudinal direction (Y direction) of the captured image is obtained, two brightness peaks are obtained as shown in the following graph. The occurrence position of the first brightness peak corresponds to the position P1 of the lower end of the heat shield 17, and the occurrence position of the second brightness peak corresponds to the position P2 of the mirror edge of the quartz crucible 11. The position P2 of the mirror edge of the upper end of the quartz crucible 11 obtained in this way is measured at a predetermined capturing cycle (sampling cycle) during one rotation of the quartz crucible 11, and the deformation amount of the upper end 11e of the quartz crucible 11 can be obtained based on the change amount of the position P2 of the mirror edge.

[0063] The shooting cycle (shooting interval) of the image is preferably an angular spacing that cannot be divided into 360 degrees. For example, if it is an integer value, a value other than a divisor of 360 such as 7 degrees and 11 degrees can be listed. In the case of measuring with an angular spacing that is evenly divisible by 360 degrees, the data of the same angle after the second turn of the crucible also becomes an accumulation of data, and the data that cannot fill the gap in the angular spacing. On the other hand, in the case of measuring with an angular spacing that cannot be divided into 360 degrees such as a 7-degree spacing, the angle after the second turn becomes an angle that fills the gap of a multiple of 7, so data of 1 degree spacing can be obtained when rotating 7 times. In addition, the shorter the shooting cycle of the image, the more it can improve the measurement accuracy of the deformation amount of the upper end 11e of the quartz crucible 11, but the processing burden of the image increases. Therefore, the lower limit value of the shooting cycle of the image can be determined according to the crucible rotation speed and the capacity of the image processing device. For example, it can also be set to more than 0.5 degrees. In addition, the upper limit value of the shooting cycle of the image can be set to less than 15 degrees, or less than 10 degrees, for example.

[0064] As described above, since the deformation amount of the upper end portion 11e of the quartz crucible 11 is obtained based on the deviation of the longitudinal position of the mirror edge during one rotation of the quartz crucible 11, it is impossible to obtain the correct deformation amount when the entire circumference of the crucible is inverted. Figure 5As shown in (b), the inward collapse of the quartz crucible 11 occurs locally and hardly occurs over the entire circumference of the crucible. Therefore, even with the above method, the deformation amount of the crucible can be accurately obtained. In addition, if the pixel position when the crucible is not deformed is obtained in advance as a reference value, the correct deformation amount can be obtained even when the entire circumference of the crucible collapses.

[0065] In order to eliminate measurement errors and accurately obtain the deformation amount of the upper end portion 11e of the quartz crucible 11, it is preferable to obtain an average value of a plurality of measurement values. Therefore, it is preferable to obtain N measurement results of the deformation amount of the quartz crucible 11 based on a plurality of images captured while the quartz crucible 11 continuously rotates N times, and obtain an average value of these N measurement results.

[0066] Figure 7 The graph shows an example of the measurement results of the position of the mirror image edge of the upper end of the quartz crucible 11 rotating at a constant speed. The horizontal axis represents the crucible rotation angle (degrees), and the vertical axis represents the pixel position (pixel) of the mirror image edge of the quartz crucible.

[0067] like Figure 7 As shown in the figure, it can be seen that the position of the mirror image edge of the quartz crucible 11 in the Y direction changes in the vertical direction during one rotation of the quartz crucible 11, and becomes the maximum at positions of about 30°, 150° and 270°, and becomes the minimum at positions of about 110°, 220° and 330°. In addition, it can be seen that the maximum change amount of the mirror image edge of the crucible in the vertical direction is about 60 pixels. In this way, the deformation amount of the quartz crucible 11 can be obtained based on the change of the mirror image of the quartz crucible 11.

[0068] The deformation amount of the quartz crucible 11 obtained from the above-mentioned captured image is the number of pixels (pixel). In order to convert it into the deformation amount (millimeter) in the actual space, unit conversion is required. The method of unit conversion is not particularly limited. For example, it can be obtained based on the correspondence between the number of pixels moved per unit time when a point at the upper end of the quartz crucible 11 moves due to the rotation of the crucible and the actual movement distance per unit time obtained from the diameter and rotation speed of the quartz crucible 11. That is, it is assumed that a point on the mirror edge of the quartz crucible 11 moves from a certain coordinate point A to another coordinate point B. On the other hand, the movement distance of a point at the upper end of the quartz crucible 11 in the actual space can be obtained based on the diameter and rotation speed of the quartz crucible. Therefore, by making the number of pixels between AB in the captured image correspond to the movement distance in the actual space, the distance in the actual space of each pixel can be obtained.

[0069] The deformation amount of the quartz crucible 11 is measured, and as a result, when the deformation amount exceeds a threshold value, the control unit 22 can output an alarm through sound or screen display, thereby calling the attention of the staff.

[0070] As described above, according to the method for manufacturing a silicon single crystal of the present embodiment, the melt surface 2a of the silicon melt 2 in the quartz crucible 11 visible through the opening 17a of the heat shield 17 is obtained by using the camera 20, and the deformation amount of the quartz crucible 11 is calculated based on the time change of the mirror image 11M of the quartz crucible 11 reflected on the melt surface 2a, so that the probability of an accident caused by the deformation of the quartz crucible 11 can be predicted and prevented. In addition, by feeding back the influence of the crystal pulling conditions on the deformation of the quartz crucible 11, the deformation of the crucible can be prevented.

[0071] In addition, the silicon single crystal manufacturing apparatus according to the present embodiment includes a camera 20 for photographing the melt surface 2a of the silicon melt 2 in the quartz crucible 11 visible through the opening 17a of the heat shield 17 from obliquely above, and an image processing unit 21 for processing the image photographed by the camera 20. The camera 20 acquires a plurality of images including the mirror image of the quartz crucible 11 reflected on the melt surface 2a of the silicon melt 2 at predetermined time intervals while the quartz crucible 11 rotates at least once. The image processing unit 21 calculates the deformation amount of the quartz crucible 11 based on the time change of the mirror image 11M of the quartz crucible 11 reflected in each of the plurality of images. Therefore, the probability of an accident caused by the deformation of the quartz crucible 11 can be predicted and prevented. In addition, by feeding back the influence of the crystal pulling conditions on the deformation of the quartz crucible 11, the deformation of the crucible can be prevented.

[0072] As mentioned above, although the preferred embodiment of the present invention is described, the present invention is not limited to the above-mentioned embodiment, and various changes can be made without departing from the scope of the present invention, and it is needless to say that these are also included in the scope of the present invention.

[0073] For example, in the above embodiment, the case where the deformation amount caused by the inward collapse of the upper end portion 11e of the quartz crucible 11 is calculated is described, but the present invention is not limited to the calculation of such deformation amount, and can also be applied to the case where the height deviation of the upper end portion 11e in the circumferential direction occurs due to the sinking of the quartz crucible 11. In addition, it can also be used as a method for calculating the eccentricity amount in the case where the central axis of the quartz crucible 11 deviates from the rotation center axis and rotates eccentrically. In this case, the eccentricity amount of the quartz crucible 11 can be calculated based on the periodic deviation of the position of the mirror edge synchronized with the rotation period of the crucible.

[0074] In the above-mentioned embodiment, the image of the quartz crucible 11 is photographed during the period from the raw material melting step S11 to before the liquid contact step S13 is started to calculate the deformation amount of the quartz crucible 11. However, the measurement period of the deformation amount of the quartz crucible 11 according to the present invention is not limited to the period from the raw material melting step S11 to before the liquid contact step S13 is started, but can be performed at any time when the edge of the image of the quartz crucible 11 reflected on the melt surface 2a can be photographed. In addition, when the image of the quartz crucible 11 can be photographed during crystal pulling, the deformation amount of the quartz crucible 11 can be continuously detected.

[0075] Furthermore, the detection of the deformation amount of the quartz crucible according to the present invention can also be applied to the so-called multiple pulling method. The multiple pulling method is a method in which, after pulling a silicon single crystal, silicon raw material is additionally supplied to the same quartz crucible and melted, and a silicon single crystal is pulled from the obtained silicon melt. By repeating such a raw material supply process and a single crystal pulling process, a plurality of silicon single crystals are manufactured from one quartz crucible. In the melting process of the additionally supplied raw material, by using the method for calculating the deformation amount of the crucible according to the present invention, it is possible to objectively determine whether the multiple pulling can continue.

[0076] In the above embodiment, the camera 20 for measuring the crystal diameter and the gap value is used to obtain an image for detecting the deformation amount of the quartz crucible 11, but the present invention is not limited to such a configuration, and a dedicated camera different from the camera for diameter measurement, etc. may be used to capture an image of the melt surface 2a.

[0077] Explanation of symbols

[0078] 1 Single crystal manufacturing equipment

[0079] 2 Silicon Molten Liquid

[0080] 2a Melt surface

[0081] 3 Silicon single crystal

[0082] 3I Silicon Single Crystal Ingot

[0083] 3a Neck constriction

[0084] 3b Shoulders

[0085] 3c Main body

[0086] 3d tail

[0087] 10 Chamber

[0088] 10a Main chamber

[0089] 10b Pulling chamber

[0090] 10c Gas inlet

[0091] 10d Gas exhaust port

[0092] 10e Peep Window

[0093] 11 Quartz Crucible

[0094] 11M Mirror image of quartz crucible

[0095] 12 Graphite Crucible

[0096] 13 Rotation axis

[0097] 14 Crucible drive mechanism

[0098] 15 Heater

[0099] Mirror image of 15M heater

[0100] 16 Insulation Materials

[0101] 17 Thermal Shield

[0102] 17R Real image of thermal shield

[0103] 17a Opening of heat shield

[0104] 18 Wire

[0105] 19 Wire winding mechanism

[0106] 20 Camera

[0107] 21 Image Processing Department

[0108] 22 Control Department

[0109] E1 Edge line of the real image of the heat shielding component

[0110] E2 Mirrored edge line of the quartz crucible

[0111] E3 heater mirror edge line

[0112] L0 test line

[0113] S11 Raw material melting process

[0114] S12 Crucible deformation detection process

[0115] S13 Liquid contact process

[0116] S14 Neck shrinking process

[0117] S15 Shoulder cultivation process

[0118] S16 Main body cultivation process

[0119] S17 Tail Cultivation Process

[0120] S18 Cooling process

Claims

1. A method for producing a silicon single crystal, which is a method for producing a silicon single crystal by pulling a silicon single crystal from a silicon melt in a quartz crucible, characterized in that: An image including a mirror image of the quartz crucible reflected on a melt surface of the silicon melt is acquired at a predetermined time interval, and deformation or eccentricity of the quartz crucible is evaluated based on a temporal change in the position of the mirror image of the quartz crucible as shown in a plurality of images acquired while the quartz crucible rotates at least one revolution.

2. The method for manufacturing a silicon single crystal according to claim 1, wherein the position of the upper end of the quartz crucible is detected based on the mirror image of the quartz crucible, and the deformation amount or eccentricity of the upper end is calculated based on the time change of the position of the upper end.

3. The method for producing a silicon single crystal according to claim 2, wherein the upper end of the quartz crucible is detected based on a differential value of a longitudinal luminance of a pixel in the image.

4. A method for manufacturing a silicon single crystal according to any one of claims 1 to 3, wherein a detection line for the position of the upper end portion is set in a plane including the optical axis of a camera that captures the image, and the amount of change of the quartz crucible is calculated based on the time change of the position of the mirror image of the quartz crucible on the detection line.

5. The method for manufacturing a silicon single crystal according to any one of claims 1 to 3, wherein the amount of change in the quartz crucible is calculated based on the plurality of images acquired during a period from a raw material melting step of starting to melt the silicon raw material in the quartz crucible to a liquid contact step of starting to bring the seed crystal into contact with the silicon melt.

6. A silicon single crystal manufacturing device, characterized in that: have: A quartz crucible to hold molten silicon; A heater, which is arranged around the quartz crucible to heat the silicon melt; A crucible driving mechanism for rotating and lifting the aforementioned quartz crucible; A crystallization pulling mechanism for pulling a silicon single crystal from the aforementioned silicon melt; a heat shield disposed above the quartz crucible so as to surround the silicon single crystal pulled out from the silicon melt; a camera that photographs a melt surface of the silicon melt visible through the opening of the heat shield from obliquely above; and an image processing unit for processing the image captured by the aforementioned camera, The camera acquires an image including a mirror image of the quartz crucible reflected on the melt surface at a predetermined time interval. The image processing unit evaluates deformation or decentering of the quartz crucible based on temporal changes in positions of mirror images of the quartz crucible reflected in a plurality of images acquired while the quartz crucible rotates at least once.

7. The silicon single crystal manufacturing device according to claim 6, wherein the image processing unit detects the position of the upper end of the aforementioned quartz crucible based on the mirror image of the aforementioned quartz crucible, and calculates the deformation or eccentricity of the aforementioned upper end based on the time change of the position of the aforementioned upper end.

8. The silicon single crystal manufacturing apparatus according to claim 7, wherein the image processing unit detects the upper end of the quartz crucible based on a differential value of a longitudinal luminance of a pixel in the image.

9. A silicon single crystal manufacturing device according to any one of claims 6 to 8, wherein the image processing unit sets a detection line for the position of the upper end portion in a plane including the optical axis of a camera that captures the image, and calculates the amount of change of the quartz crucible based on the time change of the position of the mirror image of the quartz crucible on the detection line.

10. The silicon single crystal manufacturing apparatus according to any one of claims 6 to 8, wherein the image processing unit calculates the amount of change of the quartz crucible based on the plurality of images acquired during a period from a raw material melting step of starting to melt the silicon raw material in the quartz crucible to a liquid contact step of starting to bring the seed crystal into contact with the silicon melt.

11. A method for manufacturing a silicon wafer, characterized in that: The silicon single crystal produced by the method for producing a silicon single crystal according to any one of claims 1 to 3 is processed to produce a silicon wafer.