Lead-zinc ore beneficiation method for improving valuable metal recovery rate

Through the process flow of combining magnetic separation and flotation, combined with multiple selection and sweep selection steps, the problems of low lead recovery rate and high lead content in the existing lead-zinc priority flotation process are solved, and the lead-to-lead content is achieved. The efficient recycling of zinc, silver and iron has improved economic benefits.

CN118988551AActive Publication Date: 2024-11-22扎兰屯市国森矿业有限责任公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411218811.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-22
Estimated Expiration
2044-09-02

AI Technical Summary

Technical Problem

The lead recovery rate in the existing lead-zinc priority flotation process is poor, and the lead content in zinc is high, and iron cannot be effectively recovered, resulting in unsatisfactory economic benefits.

Method used

A process flow combining magnetic separation and flotation, including magnetic separation and coarse selection after ball milling of raw ore, followed by multiple lead and zinc flotations, and the lead, zinc and iron concentrates are separated through multiple selection and sweep steps. , the specific process conditions include the use of a variety of agents and multiple selection and scanning steps.

Benefits of technology

It effectively improves the recovery rate of lead, zinc and silver, and obtains high-grade iron concentrate products, improving economic benefits, and achieving effective recycling of valuable metals without significantly adjusting the existing process flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988551A_ABST
    Figure CN118988551A_ABST
Patent Text Reader

Abstract

According to the lead-zinc ore beneficiation method capable of improving the valuable metal recovery rate, the technology that raw ore magnetic separation and magnetic roughing concentrate regrinding are conducted and then lead and zinc are independently reselected is adopted, and lead concentrate with the lead grade being 58.01%, the zinc content being 6.71%, the silver content being 6826.21 g / t, the lead recovery rate being 88.62% and the silver recovery rate being 85.15% can be obtained; the zinc concentrate with the zinc grade of 56.11%, the lead content of 0.22%, the silver content of 46.97 g / t and the zinc recovery rate of 96.24% is obtained; the yield is 1.18%, and the iron grade is 62.55%. The method has the advantages that the recovery rate of lead, zinc and silver can be effectively increased, an iron ore concentrate product with the yield of 1.18% and the iron grade of 62.55% is obtained at the same time, the recovery rate of lead, zinc and silver is increased, the iron ore concentrate is recovered, valuable metal is effectively recovered under the condition that an existing technological process is not greatly adjusted and transformed, and the method is suitable for industrial production. Therefore, the economic benefit is improved, and guidance and basis are provided for the next process transformation and process debugging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The invention relates to a ore dressing method, in particular to a lead-zinc ore dressing method for improving the recovery rate of valuable metals. Background technology:

[0002] The lead-zinc-silver polymetallic mine in the Erdaohe mining area of ​​our company is mined by open-pit mining, and the ore dressing adopts the lead-zinc priority flotation process. The flotation tailings are stored by dry discharge; since January 21, the concentrator has processed high-grade (lead + zinc = about 9%) ore, and the production indicators are not ideal. The results are shown in Table 1.

[0003] Table 1 Results of closed-circuit test of ABC area ore samples using on-site process flow%

[0004]

[0005] As can be seen from Table 1, the lead and zinc are recovered by the lead-zinc priority flotation process, and a lead concentrate with a lead grade of 57.52%, a zinc content of 6.65%, a silver content of 6892.31g / t, a lead recovery rate of 88.18%, and a silver recovery rate of 84.74% can be obtained; a zinc concentrate with a zinc grade of 55.71%, a lead content of 0.23%, a silver content of 48.63g / t, and a zinc recovery rate of 96.11% can be obtained. The disadvantages of the current process are mainly manifested in poor lead recovery rate, high lead content in zinc, the main loss of valuable lead metal in the zinc concentrate, and the inability to effectively recover the iron contained therein.

[0006] In order to reduce the inter-containment of lead and zinc concentrate, improve the mineral processing index and comprehensively recover iron, the company carried out a mineral processing test technology study on reducing the inter-containment of lead and zinc concentrate in the Erdaohe mining area and improving the mineral processing index. Without making major adjustments and modifications to the existing process flow, the company achieved the goal of increasing the recovery rate of lead, zinc and silver and recovering iron concentrate, thereby improving economic benefits, providing guidance and basis for the next step of process transformation and process debugging. Summary of the invention:

[0007] In order to solve the above problems, the object of the present invention is to provide a lead-zinc ore dressing method for improving the recovery rate of valuable metals.

[0008] The present invention is implemented by the following technical solutions:

[0009] A lead-zinc ore dressing method for improving the recovery rate of valuable metals comprises the following steps:

[0010] (1) The raw ore is ball-milled and then subjected to magnetic roughing to obtain magnetic roughing concentrate and magnetic roughing tailings; the ball-milling fineness is -200 mesh accounting for 60%; the process conditions of magnetic roughing are: the magnetic field intensity is 1500Oe;

[0011] (2) grinding the magnetic rougher concentrate obtained in step (1) and performing lead flotation to obtain a lead flotation concentrate and a lead flotation tailings;

[0012] (3) subjecting the lead flotation concentrate obtained in step (2) to zinc flotation to obtain zinc flotation concentrate and zinc flotation tailings;

[0013] (4) subjecting the zinc flotation concentrate obtained in step (3) to magnetic separation to obtain iron concentrate and magnetically separated ore;

[0014] (5) mixing the magnetic roughing tailings obtained in step (1) and the lead flotation tailings obtained in step (2) and performing lead roughing to obtain a lead roughing concentrate and a lead roughing tailings;

[0015] (6) regrinding the lead rougher concentrate obtained in step (5) and then performing lead concentration to obtain a lead concentrate;

[0016] (7) subjecting the lead roughing tailings obtained in step (5) to lead scavenging to obtain lead scavenging tailings;

[0017] (8) combining the lead scavenging tailings obtained in step (7) and the zinc flotation tailings obtained in step (3) and performing zinc roughing to obtain zinc roughing concentrate and zinc roughing tailings;

[0018] (9) subjecting the zinc rougher concentrate obtained in step (8) to zinc concentration to obtain zinc concentrate;

[0019] (10) The zinc roughing tailings obtained in step (8) are subjected to zinc scavenging to obtain tailings.

[0020] Furthermore, in the step (2), the fineness of the lead rougher concentrate after regrinding is -400 mesh>90%; the process conditions for lead flotation are: CaO=15g / t, butyl xanthate=1g / t, MIBC=50g / t.

[0021] Furthermore, in the step (3), the process conditions for zinc flotation are: CuSO4=5g / t, butyl xanthate=1g / t, MIBC=1g / t.

[0022] Furthermore, in the step (4), the process conditions for magnetic separation are: the magnetic field intensity is 1000Oe.

[0023] Furthermore, in the step (5), the process conditions for lead roughing are: CaO=1500g / t, Na2SO3=300g / t, ZnSO4=600g / t, W-1=30g / t, SN-9=40g / t, LW51=4g / t, MIBC=50g / t.

[0024] Furthermore, in the step (6), the fineness of the lead rougher concentrate reground is -400 mesh>90%; the process conditions for lead concentration are: CaO=500g / t, ZnSO4=800g / t, W-1=80g / t, SN-9=10g / t;

[0025] The lead concentration includes three concentrations, the first lead concentration tailings are returned to the step (5) to participate in the lead roughing again; the second lead concentration tailings participate in the first lead concentration again; the tertiary lead concentration tailings participate in the secondary lead concentration again; the tertiary lead concentration concentrate is the lead concentrate.

[0026] Furthermore, in step (7), the process conditions for lead scavenging are: SN-9 = 50 g / t, JR = 6 g / t, MIBC = 10 g / t;

[0027] The lead scavenging includes secondary scavenging, the concentrate of the primary lead scavenging is returned to the step (5) to participate in the lead roughing again; the concentrate of the secondary lead scavenging participates in the primary lead scavenging again.

[0028] Furthermore, in step (8), the process conditions for zinc roughing are: CaO=1500 g / t, LP=60 g / t, CuSO4=500 g / t, LW51=20 g / t, JR=65 g / t, MIBC=55 g / t;

[0029] The zinc roughing includes two zinc roughing processes, and the concentrates of the first zinc roughing process and the second zinc roughing process are combined to carry out zinc concentration.

[0030] Furthermore, in the step (9), the process conditions for zinc concentration are: CaO = 2300 g / t, LP = 120 g / t;

[0031] The zinc concentration includes four concentrations. The tailings of the first zinc concentration are returned to the step (8) to participate in the second zinc roughing. The tailings of the second zinc concentration participate in the first zinc concentration again. The tailings of the third zinc concentration participate in the second zinc concentration again. The tailings of the fourth zinc concentration participate in the third zinc concentration again. The concentrate of the fourth zinc concentration is the zinc concentrate.

[0032] Furthermore, in the step (10), the process conditions for zinc scavenging are: CuSO4=100g / t, JR=50g / t, LW51=15g / t, MIBC=10g / t;

[0033] The zinc scavenging includes secondary scavenging, the primary zinc scavenging concentrate is returned to the step (8) to participate in the secondary zinc roughing, the secondary zinc scavenging concentrate is re-participated in the primary zinc scavenging, and the secondary zinc scavenging tailings are the tailings.

[0034] Advantages of the present invention:

[0035] The present invention can effectively improve the recovery rates of lead, zinc and silver, and simultaneously obtain an iron concentrate product with a yield of 1.18% and an iron grade of 62.55%, thereby achieving the goal of improving the recovery rates of lead, zinc and silver and recovering the iron concentrate, and achieving the effective recovery of valuable metals without making major adjustments and modifications to the existing process flow, thereby improving the purpose of economic benefits, and providing guidance and basis for the next step of process modification and process debugging. Description of the drawings:

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 It is the process flow chart of Example 1;

[0038] Figure 2 The process flow chart of lead roughing of the lead flotation tailings and the roughing tailings in Example 1;

[0039] Figure 3 The process flow chart of zinc roughing from zinc flotation tailings and lead scavenging tailings in Example 1;

[0040] Figure 4 This is the process flow chart of Comparative Example 1. Specific implementation method:

[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Embodiment 1:

[0043] like Figure 1-3 A lead-zinc ore dressing method for improving the recovery rate of valuable metals shown in the figure comprises the following steps:

[0044] (1) The raw ore is ball-milled and then subjected to magnetic roughing to obtain magnetic roughing concentrate and magnetic roughing tailings; wherein the ball-milling fineness is -200 mesh accounting for 60%; the process conditions of magnetic roughing are: the magnetic field intensity is 1500Oe;

[0045] The semi-quantitative analysis results of X-ray fluorescence spectrum of the raw ore are shown in Table 2.

[0046] Table 2 X-ray fluorescence spectrum semi-quantitative analysis results of raw ore (%)

[0047]

[0048] The chemical analysis results of the raw ore are shown in Table 3.

[0049] Table 3 Chemical analysis results of raw ore (%)

[0050]

[0051] As can be seen from Table 2 and Table 3, the main components of the ore are Zn, O, Si, Ca, S, Fe, followed by Pb, Na, Mg, Al, Mn, etc. Among them, the valuable elements are mainly Pb, Zn, Ag, followed by Fe, S, etc.; the harmful element As was not detected in the spectrum analysis; the gangue mineral elements are mainly Si and Ca, with a small amount of Na, Mg, Al, Mn, etc.

[0052] (2) The magnetic rougher concentrate obtained in step (1) is regrinded and then subjected to lead flotation to obtain a lead flotation concentrate and a lead flotation tailing; wherein the fineness of the regrinded lead rougher concentrate is -400 mesh>90%; and the process conditions for lead flotation are: CaO=15g / t, butyrrolidone=1g / t, and MIBC=50g / t.

[0053] (3) subjecting the lead flotation concentrate obtained in step (2) to zinc flotation to obtain zinc flotation concentrate and zinc flotation tailings; wherein the process conditions for zinc flotation are: CuSO4 = 5 g / t, butyl xanthate = 1 g / t, and MIBC = 1 g / t.

[0054] (4) The zinc flotation concentrate obtained in step (3) is subjected to magnetic separation to obtain iron concentrate and magnetically separated ore; wherein the process conditions for magnetic separation are: the magnetic field intensity is 1000 Oe.

[0055] (5) The magnetic roughing tailings obtained in step (1) and the lead flotation tailings obtained in step (2) are mixed and then subjected to lead roughing to obtain a lead roughing concentrate and a lead roughing tailings; wherein the process conditions for the lead roughing are: CaO = 1500 g / t, Na2SO3 = 300 g / t, ZnSO4 = 600 g / t, W-1 = 30 g / t, SN-9 = 40 g / t, LW51 = 4 g / t, MIBC = 50 g / t.

[0056] (6) grinding the lead rougher concentrate obtained in step (5) and then performing lead concentration to obtain a lead concentrate; wherein the fineness of the lead rougher concentrate after grinding is -400 mesh>90%; the process conditions for lead concentration are: CaO=500g / t, ZnSO4=800g / t, W-1=80g / t, SN-9=10g / t;

[0057] Lead concentration includes three concentrations, the first lead concentration tailings are returned to step (5) to participate in lead roughing again; the second lead concentration tailings are re-participated in the first lead concentration; the third lead concentration tailings are re-participated in the second lead concentration; the third lead concentration concentrate is the lead concentrate; wherein,

[0058] The process conditions for primary lead concentration are: CaO = 500 g / t, ZnSO4 = 400 g / t, W-1 = 40 g / t, SN-9 = 10 g / t;

[0059] The process conditions for secondary lead concentration are: ZnSO4 = 200 g / t, W-1 = 20 g / t;

[0060] The process conditions for tertiary lead concentration are: ZnSO4 = 200 g / t, W-1 = 20 g / t;

[0061] (7) subjecting the lead roughing tailings obtained in step (5) to lead scavenging to obtain lead scavenging tailings; the process conditions for lead scavenging are: SN-9 = 50 g / t, JR = 6 g / t, MIBC = 10 g / t;

[0062] Lead scavenging includes secondary scavenging, the concentrate of the primary lead scavenging is returned to step (5) to participate in lead roughing again; the concentrate of the secondary lead scavenging is re-participated in the primary lead scavenging; wherein,

[0063] The process conditions for primary lead sweeping are: SN-9 = 30 g / t, JR = 2 g / t, MIBC = 10 g / t;

[0064] The process conditions for secondary lead scavenging are: SN-9 = 20g / t, JR = 3g / t;

[0065] (8) The lead scavenging tailings obtained in step (7) and the zinc flotation tailings obtained in step (3) are combined and then subjected to zinc roughing to obtain zinc roughing concentrate and zinc roughing tailings; the process conditions for zinc roughing are: CaO = 1500 g / t, LP = 60 g / t,

[0066] CuSO4=500g / t, LW51=20g / t, JR=65g / t, MIBC=55g / t;

[0067] Zinc roughing includes two zinc roughings. The concentrates of the first zinc roughing and the second zinc roughing are combined for zinc concentrating.

[0068] The process conditions for primary zinc roughing are: CaO = 1500 g / t, LP = 30 g / t, CuSO4 = 300 g / t, LW51 = 10 g / t, MIBC = 25 g / t;

[0069] The process conditions of secondary zinc roughing are: LP = 30g / t, CuSO4 = 200g / t, LW51 = 10g / t, JR = 65g / t, MIBC = 30g / t;

[0070] (9) The zinc rougher concentrate obtained in step (8) is subjected to zinc concentration to obtain a zinc concentrate; the process conditions for zinc concentration are: CaO = 2300 g / t, LP = 120 g / t;

[0071] Zinc concentration includes four concentrations, the tailings of the first zinc concentration are returned to step (8) to participate in the second zinc roughing, the tailings of the second zinc concentration are re-participated in the first zinc concentration, the tailings of the third zinc concentration are re-participated in the second zinc concentration, the tailings of the fourth zinc concentration are re-participated in the third zinc concentration, and the concentrate of the fourth zinc concentration is the zinc concentrate; wherein,

[0072] The process conditions for primary zinc concentration are: CaO = 1000 g / t, LP = 60 g / t;

[0073] The process conditions for secondary zinc concentration are: CaO = 800 g / t, LP = 40 g / t;

[0074] The process conditions for tertiary zinc concentration are: CaO = 500 g / t, LP = 20 g / t;

[0075] (10) subjecting the zinc roughing tailings obtained in step (8) to zinc scavenging to obtain tailings; the process conditions for zinc scavenging are: CuSO4=100 g / t, JR=50 g / t, LW51=15 g / t, MIBC=10 g / t;

[0076] Zinc scavenging includes secondary scavenging, the concentrate of primary zinc scavenging is returned to step (8) to participate in secondary zinc roughing, the concentrate of secondary zinc scavenging participates in primary zinc scavenging again, and the tailings of secondary zinc scavenging are tailings; wherein,

[0077] The process conditions for primary zinc scavenging are: CuSO4 = 100 g / t, JR = 30 g / t, LW51 = 10 g / t, MIBC = 10 g / t;

[0078] The process conditions for secondary zinc scavenging are: JR=20g / t, LW51=5g / t.

[0079] After ore dressing by the method of this embodiment, the results are shown in Table 4.

[0080] Table 4 Ore dressing results of this embodiment (%)

[0081]

[0082] As shown in Table 4, by adopting the process of ore magnetic separation-magnetic roughing concentrate regrinding and then separate lead and zinc reselection, a lead concentrate with a lead grade of 58.01%, a zinc content of 6.71%, a silver content of 6826.21g / t, a lead recovery rate of 88.62%, and a silver recovery rate of 85.15% can be obtained; a zinc concentrate with a zinc grade of 56.11%, a lead content of 0.22%, a silver content of 46.97g / t, and a zinc recovery rate of 96.24%; and an iron concentrate with a yield of 1.18% and an iron grade of 62.55%. Compared with the on-site process flow indicators, the lead recovery rate of this embodiment is increased by 0.44%, the zinc recovery rate is increased by 0.12%, and the silver recovery rate is increased by 0.41%, and an iron concentrate product with a yield of 1.18% and an iron grade of 62.55% is obtained at the same time.

[0083] Comparative Example 1:

[0084] The process flow chart and dosage of the comparative example are as follows Figure 4 As shown, the raw ore magnetic separation-magnetic roughing concentrate regrinding is adopted and then incorporated into the existing main process technology. The results are shown in Table 5.

[0085] Table 5 Ore dressing results of comparative example 1 (%)

[0086]

[0087] As shown in Table 5, by adopting the ore magnetic separation-magnetic roughing concentrate regrinding and incorporating into the existing main process technology, a lead concentrate with a lead grade of 57.40%, a zinc content of 6.81%, a silver content of 6772.60g / t, a lead recovery rate of 88.68%, and a silver recovery rate of 85.25% can be obtained; a zinc concentrate with a zinc grade of 55.53%, a lead content of 0.22%, a silver content of 47.40g / t, and a zinc recovery rate of 96.33%. Compared with the on-site process flow indicators, the lead recovery rate of this comparative example is increased by 0.50%, the zinc recovery rate is increased by 0.22%, and the silver recovery rate is increased by 0.51%, but the process flow cannot directly obtain iron concentrate products.

[0088] The other mineral processing indicators of this comparative example are better than those of Example 1. However, Example 1 can recover the iron contained in the original ore very well, while Comparative Example 1 cannot recover the iron.

[0089] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A lead-zinc ore dressing method for improving the recovery rate of valuable metals, characterized in that: The following steps are involved: (1) The raw ore is ball-milled and then subjected to magnetic roughing to obtain magnetic roughing concentrate and magnetic roughing tailings; the ball-milling fineness is -200 mesh accounting for 60%; the process conditions of magnetic roughing are: the magnetic field intensity is 1500Oe; (2) regrinding the magnetic rougher concentrate obtained in step (1) and performing lead flotation to obtain a lead flotation concentrate and a lead flotation tailings; (3) subjecting the lead flotation concentrate obtained in step (2) to zinc flotation to obtain zinc flotation concentrate and zinc flotation tailings; (4) subjecting the zinc flotation concentrate obtained in step (3) to magnetic separation to obtain iron concentrate and magnetically separated ore; (5) mixing the magnetic roughing tailings obtained in step (1) and the lead flotation tailings obtained in step (2) and performing lead roughing to obtain a lead roughing concentrate and a lead roughing tailings; (6) grinding the lead rougher concentrate obtained in step (5) and then performing lead concentration to obtain a lead concentrate; (7) subjecting the lead roughing tailings obtained in step (5) to lead scavenging to obtain lead scavenging tailings; (8) combining the lead scavenging tailings obtained in step (7) and the zinc flotation tailings obtained in step (3) and performing zinc roughing to obtain zinc roughing concentrate and zinc roughing tailings; (9) subjecting the zinc rougher concentrate obtained in step (8) to zinc concentration to obtain zinc concentrate; (10) The zinc roughing tailings obtained in step (8) are subjected to zinc scavenging to obtain tailings.

2. A lead-zinc ore dressing method for improving the recovery rate of valuable metals according to claim 1, characterized in that: In the step (2), the fineness of the lead rougher concentrate after regrinding is -400 mesh>90%; the process conditions for lead flotation are: CaO=15g / t, butyl xanthate=1g / t, MIBC=50g / t.

3. A lead-zinc ore dressing method for improving the recovery rate of valuable metals according to claim 1, characterized in that: In the step (3), the process conditions for zinc flotation are: CuSO4=5g / t, butyl xanthate=1g / t, MIBC=1g / t.

4. A lead-zinc ore dressing method for improving the recovery rate of valuable metals according to claim 1, characterized in that: In the step (4), the process conditions for magnetic separation are: the magnetic field intensity is 1000Oe.

5. A lead-zinc ore dressing method for improving the recovery rate of valuable metals according to claim 1, characterized in that: In the step (5), the process conditions for lead roughing are: CaO=1500g / t, Na2SO3=300g / t, ZnSO4=600g / t, W-1=30g / t, SN-9=40g / t, LW51=4g / t, MIBC=50g / t.

6. A lead-zinc ore dressing method for improving the recovery rate of valuable metals according to claim 1, characterized in that: In the step (6), the fineness of the lead rough concentrate re-grinded is -400 mesh>90%; the process conditions for lead concentration are: CaO=500g / t, ZnSO4=800g / t, W-1=80g / t, SN-9=10g / t; The lead concentration includes three concentrations, the first lead concentration tailings are returned to the step (5) to participate in the lead roughing again; the second lead concentration tailings participate in the first lead concentration again; the tertiary lead concentration tailings participate in the secondary lead concentration again; the tertiary lead concentration concentrate is the lead concentrate.

7. A lead-zinc ore dressing method for improving the recovery rate of valuable metals according to claim 1, characterized in that: In the step (7), the process conditions for lead scavenging are: SN-9 = 50 g / t, JR = 6 g / t, MIBC = 10 g / t; The lead scavenging includes secondary scavenging, the concentrate of the primary lead scavenging is returned to the step (5) to participate in the lead roughing again; the concentrate of the secondary lead scavenging participates in the primary lead scavenging again.

8. A lead-zinc ore dressing method for improving the recovery rate of valuable metals according to claim 1, characterized in that: In the step (8), the process conditions for zinc roughing are: CaO = 1500 g / t, LP = 60 g / t, CuSO4 = 500 g / t, LW51 = 20 g / t, JR = 65 g / t, MIBC = 55 g / t; The zinc roughing includes two zinc roughing processes, and the concentrates of the first zinc roughing process and the second zinc roughing process are combined to carry out zinc concentration.

9. A lead-zinc ore dressing method for improving the recovery rate of valuable metals according to claim 8, characterized in that: In the step (9), the process conditions for zinc concentration are: CaO = 2300 g / t, LP = 120 g / t; The zinc concentration includes four concentrations. The tailings of the first zinc concentration are returned to the step (8) to participate in the second zinc roughing. The tailings of the second zinc concentration participate in the first zinc concentration again. The tailings of the third zinc concentration participate in the second zinc concentration again. The tailings of the fourth zinc concentration participate in the third zinc concentration again. The concentrate of the fourth zinc concentration is the zinc concentrate.

10. A lead-zinc ore dressing method for improving the recovery rate of valuable metals according to claim 8, characterized in that: In the step (10), the process conditions for zinc scavenging are: CuSO4=100g / t, JR=50g / t, LW51=15g / t, MIBC=10g / t; The zinc scavenging includes secondary scavenging, the primary zinc scavenging concentrate is returned to the step (8) to participate in the secondary zinc roughing, the secondary zinc scavenging concentrate is re-participated in the primary zinc scavenging, and the secondary zinc scavenging tailings are the tailings.

Citation Information

Patent Citations

  • Method for comprehensively recovering valuable minerals from river course tailings

    CN103639038A

  • Beneficiation process of lead-zinc-silver ore and flotation reagent thereof

    CN106076604A

  • Beneficiation method for complex sulfide ore containing marmatite

    CN110180673A

  • Beneficiation method capable of improving zinc concentrate grade by utilizing magnetic-flotation combined process

    CN111632748A