Process method for optimizing classified concentration of titanium concentrate

Through the process method of combining dry magnetic separation and high voltage electrical separation, the titanium concentrate grading selection process is optimized, the limitations of dry screening are solved, the processing volume and sorting efficiency are improved, and the equipment and operation cost is reduced. , realizes the production of high-quality titanium concentrate.

CN118988738APending Publication Date: 2024-11-22WUDINGGUO TITANIUM METAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411289371.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing dry screening technology has problems such as low processing volume, large equipment footprint, high investment, complex process, and difficult operation in the titanium concentrate grading and selection process, and changes in the selected material particle size affect the sorting indicators.

Method used

Using a combination of dry magnetic separation and high voltage electrical separation, the selected raw materials are first dried and magnetically divided to obtain magnetic separation concentrate and tailings, and then 200 mesh screening of tailings, and fine-grained tailings are individually Magnetic and electrical separation are performed, and finally the concentrate and tailings are summarized to form high-quality concentrate and tailings.

Benefits of technology

The screening equipment and investment are reduced, the sorting efficiency is improved, the operating load is reduced, the sorting effect is avoided due to changes in particle size, and the production of high-quality titanium concentrate is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988738A_ABST
    Figure CN118988738A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of titanium concentrate processing, in particular to a process method for optimizing titanium concentrate grading concentration, which comprises the following steps: S1, drying selected raw materials, and performing dry magnetic separation to obtain magnetic separation concentrate and magnetic separation tailings; s2, the magnetic separation concentrate is subjected to high-voltage electric separation, and electric separation concentrate and electric separation tailings are obtained; s3, magnetic separation tailings and electric separation tailings are gathered and screened with 200 meshes; s4, the-200-mesh tailings are independently subjected to dry magnetic separation and high-voltage electric separation, and fine-fraction electric separation concentrate and fine-fraction electric separation tailings are obtained; and S5, the electric separation concentrates and the fine-fraction electric separation concentrates are gathered to form final high-quality electric separation concentrates, and the electric separation tailings and the fine-fraction electric separation tailings are gathered to form total tailings. According to the process method for optimizing titanium concentrate grading concentration, only tailings are screened, the material amount of dry screening is greatly reduced, screening equipment and investment can be greatly reduced, the separation process is shortened, and the same separation effect can be achieved. Few screening devices are used in the magnetoelectric concentration process, and consumption of materials such as screens is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium concentrate processing, and in particular to a process for optimizing the classification and selection of titanium concentrate. Background Art

[0002] Working material of dry magnetic separator: the motor reducer drives the separation drum to rotate through the V-belt, and the material is directly fed to the vibrating feeder through the feed port with controllable opening size, and is evenly distributed and fed to the magnetic field area on the upper part of the separation drum. Under the rotation of the separation drum, the magnetic particles and non-magnetic particles are subjected to different magnetic and centrifugal forces, and the strong magnetic particles, weak magnetic particles and non-magnetic particles have different movement trajectories. The strong magnetic and weak magnetic particles are adsorbed on the magnetic drum or deviate toward the magnetic drum, and finally enter the magnetic mineral receiving bucket; and the non-magnetic particles are not affected by the magnetic field force, so they are thrown into the non-magnetic product collection box under the action of centrifugal force, gravity, etc., thereby completing the separation of magnetic materials and non-magnetic materials.

[0003] Working principle of high voltage electric separator: It uses the difference in conductive properties of materials to separate conductors from non-conductor materials by mainly utilizing electric field force, supplemented by centrifugal force, gravity, mirror force and other combined effects in the corona-induction composite electric field. A negative high voltage DC is applied to the corona-induction composite electrode, and an ionized electric field is formed between the corona electrode and the grounded roller electrode. After the material enters the electric field, it is uniformly charged with negative charges. After contacting the roller, the material particles with good conductivity can quickly release the charges they carry through the grounded roller, and are electrically neutral or positive. Under the effects of the suction force of the induction electrode, the repulsion of the image charge, and the centrifugal force, they move parabolically away from the roller and fall into the conductor receiving trough; non-conductor material particles cannot release or release their charges very slowly, so they are adsorbed on the surface of the grounded roller, move at a uniform speed with the roller, and are forced to fall into the non-conductor receiving trough by the unloading brush; intermediate product particles with conductivity between conductors and non-conductors need a certain amount of time to release their charges, and when the adsorption force is not enough to counteract gravity, they fall into the intermediate product receiving trough. In this way, the materials are separated according to the difference between good and poor conductor performance.

[0004] Dry magnetic separation and high-voltage electric separation are generally used in the final selection process of titanium concentrate. The operation requires high concentrate yield, low tailings grade, high removal rate of impurities such as silicon, calcium and magnesium, and low titanium loss.

[0005] After grinding, grading and sorting, ilmenite is obtained into titanium rough concentrate. After the titanium rough concentrate is dried, dry strong magnetic and high-voltage electric separation are carried out to obtain the final titanium concentrate. However, in the process of dry magnetic separation and high-voltage electric separation, the material is affected by gravity and centrifugal force in addition to magnetic and electric field forces. There are large differences in the gravity and centrifugal force received by different particle sizes during the sorting process. Dry strong magnetic separation and high-voltage electric separation require that the particle size distribution of the selected minerals is concentrated. The titanium raw materials obtained by grinding and grading in the roughing plant have a wide particle size range, with a distribution of 40-800 mesh. The concentrate has high quality but low yield. Or the concentrate has high yield but the quality does not meet the requirements. Therefore, the industry generally adopts the process of selection after grading. The material is screened using screening equipment to obtain +200 mesh and -200 mesh materials, which are subjected to dry magnetic separation and electric separation respectively. Titanium concentrate products with high yield and high quality can be obtained. However, there are also many problems with graded magnetic and electric separation.

[0006] (1) Dry screening has great limitations and low processing capacity. The processing capacity of a single swing screen is only 2-3 tons per hour. The equipment occupies a large area, requires a large number of screening equipment, has high investment, complex process and difficult operation;

[0007] (2) Dry screening screens are prone to clogging and wear. Too many screening devices will result in frequent replacement of the screens, a large amount of employee operation, and high material consumption costs.

[0008] (3) The particle size of the selected materials is not fixed. It will change at any time due to factors such as deep mining in the mine and grinding and grading operations in the roughing plant. If graded and selected materials are carried out, it will be difficult to match the number of magnetic separators and electric separators corresponding to the coarse and fine particles. There may be a situation where the sorting index is affected by the mismatch of processing volume. Summary of the invention

[0009] The purpose of the present invention is to provide a process method for optimizing the grading and selection of titanium concentrate, so as to solve the problems that the dry screening proposed in the above background technology has great limitations, the processing capacity is low, the processing capacity of a single swing screen is only 2-3 tons per hour, the equipment occupies a large area, a large number of screening equipment are required, the investment is high, the process is complicated, and the operation is difficult.

[0010] To achieve the above object, the present invention provides a process for optimizing the classification and concentration of titanium concentrate, comprising the following steps:

[0011] S1, drying the selected raw materials and performing dry magnetic separation to obtain magnetic concentrate and magnetic tailings;

[0012] S2, the magnetic concentrate is subjected to high-voltage electrostatic separation to obtain electrostatic concentrate and electrostatic tailings;

[0013] S3, the magnetic separation tailings and the electrostatic separation tailings are collected and screened with 200 mesh to obtain +200 mesh tailings and -200 mesh tailings;

[0014] S4 and -200 mesh tailings are subjected to dry magnetic separation and high-voltage electrostatic separation to obtain fine-grained electrostatically separated concentrate and fine-grained electrostatically separated tailings;

[0015] S5. The electrostatically separated ore concentrate and the fine-grained electrostatically separated ore concentrate are combined to form the final high-quality electrostatically separated ore concentrate, and the electrostatically separated ore tailings and the fine-grained electrostatically separated ore tailings are combined to form the total tailings.

[0016] As a preferred embodiment of the present invention, the raw material selected in step S1 is ilmenite, with a TiO2 content of 46-48%, a moisture content of ≤0.5%, and a temperature of 40-50°C.

[0017] As a preferred embodiment of the present invention, the sorting parameters of the dry magnetic separation operation in step S1 are the coarse-grained titanium concentrate sorting parameters, the spacing between the separation plate and the drum is 6-10mm, the drum speed of the magnetic separator is 20-24HZ, the dry magnetic separation operation in step S1 has a magnetic concentrate yield of 95-96%, a TiO2 content of 46.5-48.5%, and a magnetic tailings yield of 4-5%.

[0018] As a preferred embodiment of the present invention, the high-voltage electric separation operation electric separator of step S2 is selected as a 6-roller electric separator, with 2 rollers on the upper, middle and lower sides, and the internal separation process is composed of one coarse and two fine separation processes. The separation parameters of the high-voltage electric separation operation of step S2 are the coarse-grade titanium concentrate separation parameters, the rotation speed of the upper, middle and lower rollers is 110-120HZ, the voltage is 22-24KV, the high-voltage electric separation operation of step S2 The electric separation concentrate yield is 80-85%, the TiO2 content is 47.5-49.5%, and the electric separation tailings yield is 15-20%.

[0019] As a preferred embodiment of the present invention, the screening raw materials of the screening operation of step S3 are the collection of magnetic separation tailings and electrostatic separation tailings, with a total yield of 20-25%, and the screening equipment is a swing screen with a screen size of 200 mesh. The screening operation of step S3 obtains +200 mesh tailings with a comprehensive yield of 6-8% and a TiO2 content of 25-30%; -200 mesh tailings with a comprehensive yield of 14-17% and a TiO2 content of 42-47%.

[0020] As a preferred embodiment of the present invention, the magnetic separation parameters of the -200 mesh material dry magnetic electrostatic separation operation in step S4 are the fine-grained titanium concentrate separation parameters, the spacing between the separation plate and the drum is 6-10mm, the drum speed of the magnetic separator is 28-32HZ, and the yield of fine-grained magnetic separation tailings is 1%, and the TiO2 content is 25-30%. The -200 mesh material dry magnetic electrostatic separation operation in step S4 is a 6-roller electrostatic separator, with 2 rollers on the upper, middle and lower sides, and the internal separation process is composed of one coarse and two fine processes. The separation parameters are the coarse-grained titanium concentrate separation parameters, the upper, middle and lower drum speeds are 180-200HZ, and the voltage is 22-24KV. The yield of fine-grained electrostatic tailings is 2%, and the TiO2 content is 25-30%.

[0021] As a preferred embodiment of the present invention, step S5 is a mixing operation of the electrostatically separated concentrate and the fine-grained electrostatically separated concentrate to form a final titanium concentrate after mixing, and the TiO2 content is 47.5-49.5% and the yield is 89-91%. Step S5 is a mixing operation of the electrostatically separated tailings and the fine-grained magnetic-electrostatically separated tailings to form a final tailings after mixing, and the TiO2 content is 25-30% and the yield is 9-11%.

[0022] As a preferred embodiment of the present invention, the drying process uses drying equipment, the dry magnetic separation in step S1 uses a first dry magnetic separator, the high-voltage electric separation in step S2 uses a first high-voltage electric separator, the screening process in step S3 uses screening equipment, the dry magnetic separation in step S4 uses a second dry magnetic separator, the high-voltage electric separation in step S4 uses a second high-voltage electric separator, and in step S5, the electric separation concentrate and the fine-grained electric separation concentrate are aggregated using a concentrate aggregation device, and the electric separation tailings and the fine-grained electric separation tailings are aggregated using a tailings aggregation device.

[0023] As a preferred embodiment of the present invention, the first dry magnetic separator is connected after the drying equipment, the first high-voltage electric separator is connected after the first dry magnetic separator, the screening equipment is connected to the tailings outlet ends of the first dry magnetic separator and the first high-voltage electric separator, the second dry magnetic separator is connected to the -200 mesh tailings outlet end of the screening equipment, and the second high-voltage electric separator is connected after the second dry magnetic separator.

[0024] As a preferred embodiment of the present invention, the concentrate aggregation equipment is connected to the concentrate outlet ends of the first high-voltage electric separator and the second high-voltage electric separator, and the tailings aggregation equipment is connected to the +200 mesh tailings outlet end of the screening equipment and the tailings outlet end of the second high-voltage electric separator.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. In the process method for optimizing the classification and selection of titanium concentrate, only the tailings are screened, and the amount of dry screening material is greatly reduced, which can greatly reduce the screening equipment and investment, shorten the sorting process and achieve the same sorting effect.

[0027] 2. In the process method for optimizing the grading and selection of titanium concentrate, the magneto-electric selection process uses less screening equipment, thus avoiding the consumption of materials such as screens.

[0028] 3. In the process method for optimizing the grading and selection of titanium concentrate, the magnetic and electric selection process is not affected by the change in the particle size of the selected raw materials, and the amount of -200 mesh selected raw materials can be controlled by controlling the amount of tailings before screening.

[0029] 4. In the process method for optimizing the grading and selection of titanium concentrate, the magnetic and electric selection process adopts the operation process of first selection and then classification, which greatly reduces the screening amount and reduces the screening process load. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the process flow of the present invention;

[0031] Figure 2 It is a schematic diagram of the structure of the device of the present invention;

[0032] The meaning of each number in the figure is:

[0033] 1. Drying equipment; 2. First dry magnetic separator; 3. First high-voltage electric separator; 4. Screening equipment; 5. Second dry magnetic separator; 6. Second high-voltage electric separator; 7. Concentrate aggregation equipment; 8. Tailings aggregation equipment. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The present invention provides a process for optimizing the classification and concentration of titanium concentrate, such as Figure 1-Figure 2 As shown, the following steps are included:

[0036] S1, drying the selected raw materials and performing dry magnetic separation to obtain magnetic concentrate and magnetic tailings;

[0037] S2, the magnetic concentrate is subjected to high-voltage electrostatic separation to obtain electrostatic concentrate and electrostatic tailings;

[0038] S3, the magnetic separation tailings and the electrostatic separation tailings are collected and screened with 200 mesh to obtain +200 mesh tailings and -200 mesh tailings;

[0039] S4 and -200 mesh tailings are subjected to dry magnetic separation and high-voltage electrostatic separation to obtain fine-grained electrostatically separated concentrate and fine-grained electrostatically separated tailings;

[0040] S5. The electrostatically separated ore concentrate and the fine-grained electrostatically separated ore concentrate are combined to form the final high-quality electrostatically separated ore concentrate, and the electrostatically separated ore tailings and the fine-grained electrostatically separated ore tailings are combined to form the total tailings.

[0041] In this embodiment, the raw material selected in step S1 is ilmenite, with a TiO2 content of 46-48%, a moisture content of ≤0.5%, and a temperature of 40-50°C.

[0042] Removing moisture from the raw materials through drying is beneficial to subsequent dry magnetic separation and high-voltage electrostatic separation. Dry magnetic separation can initially separate ilmenite particles with strong magnetism, while high-voltage electrostatic separation further utilizes the difference in electrical properties between ilmenite and other minerals to effectively remove non-ilmenite particles, thereby improving the TiO2 grade of the concentrate.

[0043] The magnetic and electrostatic tailings were not directly discarded, but were screened at 200 mesh. The tailings with smaller particle size of -200 mesh were subjected to dry magnetic separation and high-voltage electrostatic separation, and the ilmenite particles were further recovered to form fine-grained electrostatic concentrate. This step effectively reduced the waste of resources and increased the recovery rate of ilmenite.

[0044] Through screening, the material is divided into two parts: +200 mesh and -200 mesh, providing more accurate raw materials for subsequent dry magnetic separation and high-voltage electric separation. This particle size classification helps to improve the separation efficiency and product quality, making the final concentrate more uniform in particle size distribution.

[0045] The entire process, from drying to magnetic separation, electric separation, screening, and then to the collection of concentrates and tailings, is closely linked to form an efficient and continuous production line. This process design not only improves production efficiency, but also reduces energy consumption and costs.

[0046] This process focuses on resource recycling and environmental protection. Through refined sorting and screening, it maximizes the recovery of ilmenite particles and reduces the discharge of tailings. At the same time, drying also reduces the moisture content in the raw materials, which is beneficial to subsequent environmental protection treatment.

[0047] Specifically, the sorting parameters of the dry magnetic separation operation in step S1 are the coarse-grained titanium concentrate sorting parameters, the distance between the separation plate and the drum is 6-10mm, the drum speed of the magnetic separator is 20-24HZ, the dry magnetic separation operation in step S1 has a magnetic concentrate yield of 95-96%, a TiO2 content of 46.5-48.5%, and a magnetic tailings yield of 4-5%.

[0048] Furthermore, the high-voltage electric separation operation electric separator of step S2 is selected as a 6-roller electric separator, with 2 rollers on the upper, middle and lower parts, and the internal parts form a coarse and two fine separation processes. The sorting parameters of the high-voltage electric separation operation of step S2 are the coarse-grade titanium concentrate sorting parameters. The speed of the upper, middle and lower rollers is 110-120HZ, and the voltage is 22-24KV. The high-voltage electric separation operation of step S2 has an electric separation concentrate yield of 80-85%, a TiO2 content of 47.5-49.5%, and an electric separation tailings yield of 15-20%.

[0049] Furthermore, the screening raw materials of the screening operation of step S3 are the combination of magnetic separation tailings and electrostatic separation tailings, with a total yield of 20-25%. The screening equipment is a swing screen with a screen size of 200 mesh. The screening operation of step S3 obtains +200 mesh tailings with a comprehensive yield of 6-8% and a TiO2 content of 25-30%; -200 mesh tailings with a comprehensive yield of 14-17% and a TiO2 content of 42-47%.

[0050] Furthermore, the magnetic separation parameters of the -200 mesh material dry magnetic electrostatic separation operation in step S4 are the fine-grained titanium concentrate separation parameters, the spacing between the separation plate and the drum is 6-10mm, the drum speed of the magnetic separator is 28-32HZ, and the fine-grained magnetic separation tailings with a yield of 1% and a TiO2 content of 25-30% are obtained. The -200 mesh material dry magnetic electrostatic separation operation in step S4 is a 6-roller electrostatic separator, with 2 rollers on the upper, middle and lower sides, and a first coarse and two fine separation processes are formed inside. The separation parameters are the coarse-grained titanium concentrate separation parameters, the upper, middle and lower drum speeds are 180-200HZ, the voltage is 22-24KV, and the fine-grained electrostatic tailings with a yield of 2% are obtained, and the TiO2 content is 25-30%.

[0051] Furthermore, in step S5, the electrostatically separated concentrate and the fine-grained electrostatically separated concentrate are mixed to form a final titanium concentrate with a TiO2 content of 47.5-49.5% and a yield of 89-91%. In step S5, the electrostatically separated tailings and the fine-grained magnetic-electrostatically separated tailings are mixed to form a final tailings with a TiO2 content of 25-30% and a yield of 9-11%.

[0052] Furthermore, the drying process uses drying equipment 1, the dry magnetic separation in step S1 uses a first dry magnetic separator 2, the high-voltage electric separation in step S2 uses a first high-voltage electric separator 3, the screening process in step S3 uses screening equipment 4, the dry magnetic separation in step S4 uses a second dry magnetic separator 5, the high-voltage electric separation in step S4 uses a second high-voltage electric separator 6, and in step S5, the electric separation concentrate and the fine-grained electric separation concentrate are aggregated using a concentrate aggregation device 7, and the electric separation tailings and the fine-grained electric separation tailings are aggregated using a tailings aggregation device 8.

[0053] Furthermore, the first dry magnetic separator 2 is connected to the drying equipment 1, the first high-voltage electric separator 3 is connected to the first dry magnetic separator 2, the screening equipment 4 is connected to the tailings outlet ends of the first dry magnetic separator 2 and the first high-voltage electric separator 3, the second dry magnetic separator 5 is connected to the -200 mesh tailings outlet end of the screening equipment 4, and the second high-voltage electric separator 6 is connected to the second dry magnetic separator 5.

[0054] Furthermore, the concentrate aggregation equipment 7 is connected to the concentrate outlet ends of the first high-voltage electric separator 3 and the second high-voltage electric separator 6, and the tailings aggregation equipment 8 is connected to the +200 mesh tailings outlet end of the screening equipment 4 and the tailings outlet end of the second high-voltage electric separator 6.

[0055] The drying equipment 1 pre-treats the raw materials to remove moisture, providing good conditions for subsequent magnetic separation and electric separation. The first dry magnetic separator 2 and the second dry magnetic separator 5 respectively perform magnetic separation on the materials at different stages to effectively separate the magnetic substances; while the first high-voltage electric separator 3 and the second high-voltage electric separator 6 further purify the materials by utilizing the electrical property difference, so that the grade of the concentrate is significantly improved.

[0056] Fine screening: The introduction of screening equipment 4 realizes the particle size classification of materials, dividing the materials into two parts: -200 mesh and +200 mesh, providing more accurate raw materials for subsequent dry magnetic separation and high-voltage electric separation, which helps to improve sorting efficiency and product quality.

[0057] Maximizing resource utilization: Through the concentrate aggregation equipment 7 and tailings aggregation equipment 8, the concentrates and tailings at different stages are aggregated separately, which not only facilitates subsequent processing and utilization, but also reduces the waste of resources. In particular, the centralized processing of tailings is conducive to the recycling of resources and environmental protection.

[0058] Process optimization and automation: The entire technical process, from drying to magnetic separation, electric separation, screening, and then to the collection of concentrates and tailings, is closely linked to form an efficient and automated production line. This process design not only improves production efficiency, but also reduces labor costs and operational difficulty.

[0059] Finally, it should be noted that the electronic components of the concentrate aggregation equipment 7, tailings aggregation equipment 8, etc. in this embodiment are all universal standard parts or parts known to technical personnel in this field, and their structures and principles can be known to technical personnel in this field through technical manuals or through conventional experimental methods. In the idle part of this device, all the above-mentioned electrical components are connected by wires respectively. The specific connection means should refer to the working sequence between the electrical components in the above-mentioned working principle to complete the electrical connection, which are all well-known technologies in the field.

[0060] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A process for optimizing the classification and concentration of titanium concentrate, characterized by: The steps include: S1, drying the selected raw materials and performing dry magnetic separation to obtain magnetic concentrate and magnetic tailings; S2, the magnetic concentrate is subjected to high-voltage electrostatic separation to obtain electrostatic concentrate and electrostatic tailings; S3, the magnetic separation tailings and the electrostatic separation tailings are collected and screened with 200 mesh to obtain +200 mesh tailings and -200 mesh tailings; S4 and -200 mesh tailings are subjected to dry magnetic separation and high-voltage electrostatic separation to obtain fine-grained electrostatically separated concentrate and fine-grained electrostatically separated tailings; S5. The electrostatically separated ore concentrate and the fine-grained electrostatically separated ore concentrate are combined to form the final high-quality electrostatically separated ore concentrate, and the electrostatically separated ore tailings and the fine-grained electrostatically separated ore tailings are combined to form the total tailings.

2. The process for optimizing the classification and concentration of titanium concentrate according to claim 1, characterized in that: The raw material selected in step S1 is ilmenite, with a TiO2 content of 46-48%, a moisture content of ≤0.5%, and a temperature of 40-50°C.

3. The process for optimizing the classification and concentration of titanium concentrate according to claim 1 is characterized in that: The sorting parameters of the dry magnetic separation operation in step S1 are the coarse-grained titanium concentrate sorting parameters, the distance between the separation plate and the drum is 6-10mm, the drum speed of the magnetic separator is 20-24HZ, the dry magnetic separation operation in step S1 has a magnetic concentrate yield of 95-96%, a TiO2 content of 46.5-48.5%, and a magnetic tailings yield of 4-5%.

4. The process for optimizing the classification and concentration of titanium concentrate according to claim 1, characterized in that: The high-voltage electric separation operation electric separator of step S2 is a 6-roller electric separator, which has 2 rollers on the upper, middle and lower parts, and internally forms a coarse and two fine separation processes. The sorting parameters of the high-voltage electric separation operation of step S2 are the coarse-grade titanium concentrate sorting parameters. The speed of the upper, middle and lower rollers is 110-120HZ, and the voltage is 22-24KV. The high-voltage electric separation operation of step S2 has an electric separation concentrate yield of 80-85%, a TiO2 content of 47.5-49.5%, and an electric separation tailings yield of 15-20%.

5. The process for optimizing the classification and concentration of titanium concentrate according to claim 1 is characterized in that: The screening raw materials of the screening operation of step S3 are the magnetic separation tailings and the electrostatic separation tailings, with a total yield of 20-25%. The screening equipment is a swing screen with a screen size of 200 mesh. The screening operation of step S3 obtains +200 mesh tailings with a comprehensive yield of 6-8% and a TiO2 content of 25-30%; -200 mesh tailings with a comprehensive yield of 14-17% and a TiO2 content of 42-47%.

6. The process for optimizing the classification and concentration of titanium concentrate according to claim 1, characterized in that: The magnetic separation parameters of the -200 mesh material dry magnetic electrostatic separation operation in step S4 are the fine-grained titanium concentrate separation parameters, the spacing between the separation plate and the drum is 6-10mm, the drum speed of the magnetic separator is 28-32HZ, and the yield of fine-grained magnetic separation tailings is 1%, and the TiO2 content is 25-30%. The -200 mesh material dry magnetic electrostatic separation operation in step S4 is a 6-roller electrostatic separator, with 2 rollers on the upper, middle and lower sides, and the internal separation process is composed of one coarse and two fine processes. The separation parameters are the coarse-grained titanium concentrate separation parameters, the upper, middle and lower drum speeds are 180-200HZ, the voltage is 22-24KV, and the yield of fine-grained electrostatic tailings is 2%, and the TiO2 content is 25-30%.

7. The process for optimizing the classification and concentration of titanium concentrate according to claim 1 is characterized in that: In step S5, the electrostatically separated concentrate and the fine-grained electrostatically separated concentrate are mixed to form a final titanium concentrate with a TiO2 content of 47.5-49.5% and a yield of 89-91%. In step S5, the electrostatically separated tailings and the fine-grained magnetically separated tailings are mixed to form a final tailings with a TiO2 content of 25-30% and a yield of 9-11%.

8. The process for optimizing the classification and concentration of titanium concentrate according to claim 1, characterized in that: The drying process uses a drying device (1), the dry magnetic separation in step S1 uses a first dry magnetic separator (2), the high-voltage electric separation in step S2 uses a first high-voltage electric separator (3), the screening process in step S3 uses a screening device (4), the dry magnetic separation in step S4 uses a second dry magnetic separator (5), the high-voltage electric separation in step S4 uses a second high-voltage electric separator (6), the electric separation concentrate and the fine-grained electric separation concentrate are aggregated using a concentrate aggregation device (7) in step S5, and the electric separation tailings and the fine-grained electric separation tailings are aggregated using a tailings aggregation device (8).

9. The process for optimizing the classification and concentration of titanium concentrate according to claim 8, characterized in that: The first dry magnetic separator (2) is connected to the drying device (1), the first high-voltage electric separator (3) is connected to the first dry magnetic separator (2), the screening device (4) is connected to the tailings outlet ends of the first dry magnetic separator (2) and the first high-voltage electric separator (3), the second dry magnetic separator (5) is connected to the -200 mesh tailings outlet end of the screening device (4), and the second high-voltage electric separator (6) is connected to the second dry magnetic separator (5).

10. The process for optimizing the classification and concentration of titanium concentrate according to claim 9, characterized in that: The concentrate collection device (7) is connected to the concentrate outlet ends of the first high-voltage electric separator (3) and the second high-voltage electric separator (6), and the tailings collection device (8) is connected to the +200 mesh tailings outlet end of the screening device (4) and the tailings outlet end of the second high-voltage electric separator (6).

Citation Information

Patent Citations

  • Magnetic separation-electric separation combined titanium separation method

    CN113019658A

  • Comprehensive treatment method for titanium concentrate capable of being used as titanium chloride slag raw material

    CN113182076A

  • Sorting method for high-chromium ilmenite

    CN117101865A

  • Efficient intelligent dry-type pre-selection method for vanadium titano-magnetite

    CN117358600A

  • Method and device for treating a light weight shredder fraction containing metal parts

    EP0884107A2