Production method for improving surface hardness of 300-series austenitic stainless steel
Through thermal continuous annealing, reversible cold rolling mill rolling, recrystallization annealing and annealing treatment, combined with electrolytic pickling or argon protective annealing, the problem that the existing process cannot meet customers' high hardness needs, and the hardness of 300 series stainless steel is achieved Significant improvement.
Patent Information
- Application Number
- CN202411213693.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
The existing production process cannot meet customers' demand for higher hardness of 300 series austenitic stainless steel.
Through hot continuous annealing, reversible cold rolling mill rolling, recrystallization annealing, degreasing and cold continuous annealing, combined with neutral salt electrolysis and nitric acid electrolytic acid cleaning, or cover annealing under argon protection, gradually increase by 300 The hardness of stainless steel.
The hardness of 300 series stainless steel has been significantly improved to meet customers' needs for higher hardness, and the hardness improvement range is 10HV-100HV.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of stainless steel production, and in particular to a production method for improving the surface hardness of 300 series austenitic stainless steel. Background Art
[0002] 300 series stainless steel is a type of steel that is easily cold-deformed and strengthened. By rolling on a 20-roll reversible cold rolling mill, it can quickly increase hardness and strength, while retaining sufficient plasticity, toughness, and good corrosion resistance in atmospheric environments. However, due to different customer needs, 300 series stainless steel with a higher hardness is required, and the current production process cannot meet customer needs. Summary of the invention
[0003] In view of the above technical problems, the present invention provides a production method for improving the surface hardness of 300 series austenitic stainless steel.
[0004] In order to achieve the above object, the technical solution of the present invention is as follows: A production method for improving the surface hardness of 300 series austenitic stainless steel, comprising the following steps: S1. 300 series hot-rolled black coil stainless steel is subjected to hot continuous annealing and pickling at an annealing temperature of 1050°C-1200°C to obtain a solid solution stainless steel coil; S2. Rolling the solid solution stainless steel coil by a 20-roller reversible cold rolling mill, with a total reduction ratio of ≥10%, to obtain intermediate rolling hardened stainless steel; S3, performing recrystallization annealing and pickling on the intermediate rolling hardened stainless steel, the annealing temperature is 1050°C-1200°C, and 300 series stainless steel after recrystallization annealing and pickling is obtained; S4. The 300 series stainless steel after recrystallization annealing and pickling is subjected to final hardness rolling on a 20-roller reversible cold rolling mill, and the final hardness reduction rate is controlled to be 6%-60%, so as to obtain a 300 series stainless steel final rolling process hardened steel coil; S5. Degrease the 300 series stainless steel hard coils at a degreasing temperature of 38°C-45°C; S6. The degreased steel coil is subjected to cold continuous annealing, and then pickled by neutral salt electrolysis + nitric acid electrolysis, or the degreased steel coil is placed in a bell-type annealing furnace filled with argon protection for annealing, and finally a stainless steel hard product with a hardness increased by 10HV-100HV is obtained.
[0005] Among them, in the step S6, specifically, the degreased steel coil is subjected to cold continuous annealing at 300°C-750°C, the annealing speed is 10m / min-100m / min, and then subjected to neutral salt electrolysis + nitric acid electrolysis pickling, the neutral salt current is 1000A-8000A, the concentration is 100g / L-300g / L, the nitric acid current is 1000A-6000A, the concentration is 100g / L-300g / L, the temperature is 40-60°C, or the degreased steel coil is placed in a bell-type annealing furnace filled with argon protection, annealed at 300°C-750°C, kept warm for 2h-48h and taken out of the furnace, and finally a stainless steel hard product with a hardness increased by 10HV-100HV is obtained.
[0006] The beneficial effects of the present invention are as follows: the 301 stainless steel, 301L stainless steel and 304 stainless steel after recrystallization annealing and pickling are subjected to cold working hardening rolling to obtain 300 series stainless steel hard products, and the hardness of the hard products is further improved to the hardness range required by customers after heat treatment. DETAILED DESCRIPTION
[0007] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0008] Example 1 A production method for improving the surface hardness of 300 series austenitic stainless steel, comprising the following steps: S1. Perform hot continuous annealing and pickling on 600 mm wide 300 series hot-rolled black coil stainless steel at an annealing temperature of 1050° C. to obtain a solid solution stainless steel coil; S2, rolling the solid solution stainless steel coil through a 20-roller reversible cold rolling mill with a total reduction rate of 10% to obtain intermediate rolling hardened stainless steel; S3, performing recrystallization annealing and pickling on the intermediate rolling hardened stainless steel, the annealing temperature is 1050° C., to obtain 300 series stainless steel after recrystallization annealing and pickling; S4, the 300 series stainless steel after recrystallization annealing and pickling is subjected to final hardness rolling on a 20-roller reversible cold rolling mill, and the final hardness reduction rate is controlled to be 6%, so as to obtain a 300 series stainless steel final rolling process hardened steel coil; S5. Degrease the 300 series stainless steel hard coils at a degreasing temperature of 38°C; S6. The degreased steel coil is subjected to cold continuous annealing, and then pickled by neutral salt electrolysis + nitric acid electrolysis, or the degreased steel coil is placed in a bell-type annealing furnace filled with argon protection for annealing, and finally a stainless steel hard product with a hardness increased by 10HV is obtained.
[0009] Among them, in the step S6, specifically, the degreased steel coil is subjected to cold continuous annealing at 300°C, the annealing speed is 10m / min, and then subjected to neutral salt electrolysis + nitric acid electrolysis pickling, the neutral salt current is 1000A, the concentration is 100g / L, the nitric acid current is 1000A, the concentration is 100g / L, and the temperature is 40°C, or the degreased steel coil is placed in a bell-type annealing furnace filled with argon protection, annealed at 300°C, and kept warm for 2h before being taken out of the furnace.
[0010] Example 2 A production method for improving the surface hardness of 300 series austenitic stainless steel, comprising the following steps: S1. Perform hot continuous annealing and pickling on 1600 mm wide 300 series hot-rolled black coil stainless steel at an annealing temperature of 1200°C to obtain a solid solution stainless steel coil; S2, rolling the solid solution stainless steel coil through a 20-roller reversible cold rolling mill with a total reduction rate of 10% to obtain intermediate rolling hardened stainless steel; S3, performing recrystallization annealing and pickling on the intermediate rolling hardened stainless steel, the annealing temperature is 1200° C., and 300 series stainless steel after recrystallization annealing and pickling is obtained; S4, the 300 series stainless steel after recrystallization annealing and pickling is subjected to final hardness rolling on a 20-roller reversible cold rolling mill, and the final hardness reduction rate is controlled to be 60%, so as to obtain a 300 series stainless steel final rolling process hardened steel coil; S5. Degrease the 300 series stainless steel hard coils at a degreasing temperature of 45°C; S6. The degreased steel coil is subjected to cold continuous annealing, and then pickled by neutral salt electrolysis + nitric acid electrolysis, or the degreased steel coil is placed in a bell-type annealing furnace filled with argon protection for annealing, and finally a stainless steel hard product with a hardness increased by 100HV is obtained.
[0011] Specifically, in step S6, the degreased steel coil is subjected to cold continuous annealing at 750°C, the annealing speed is 100m / min, and then subjected to neutral salt electrolysis + nitric acid electrolysis pickling, the neutral salt current is 8000A, the concentration is 300g / L, the nitric acid current is 6000A, the concentration is 300g / L, and the temperature is 60°C, or the degreased steel coil is placed in a bell-type annealing furnace filled with argon protection, annealed at 750°C, and kept warm for 48h before being taken out of the furnace.
[0012] Example 3 S1. 1265mm wide 301 hot-rolled black coil stainless steel is subjected to hot continuous annealing and pickling at an annealing temperature of 1100°C; S2, rolling on a 20-roller reversing cold rolling mill with a total reduction of 50%; S3, cold continuous annealing and pickling of the intermediate rolling hardened stainless steel, the annealing temperature is 1100°C; S4, the 301 stainless steel after recrystallization annealing and pickling is subjected to final hardness rolling on a 20-roller reversible cold rolling mill, and the final hardness reduction rate is controlled to be 20%; S5. Degrease the 300 series stainless steel hard coils at a degreasing temperature of 38°C; S6. After degreasing, the steel coil is subjected to cold continuous annealing at 700°C with an annealing speed of 10m / min, and then subjected to neutral salt electrolysis + nitric acid electrolysis pickling, with a neutral salt current of 3000A, a concentration of 120g / L, a nitric acid current of 2000A, a concentration of 100g / L, and a temperature of 41°C, to finally obtain a stainless steel hard product with a hardness increase of 30HV.
[0013] Example 4 S1. Perform hot continuous annealing and pickling on 1540mm wide 304 hot-rolled black coil stainless steel, with the annealing temperature at 1180℃; S2, rolling on a 20-roller reversing cold rolling mill with a total reduction of 45%; S3, cold continuous annealing and pickling of the intermediate rolling hardened stainless steel, the annealing temperature is 1130°C; S4, the 304 stainless steel after recrystallization annealing and pickling is subjected to final hardness rolling on a 20-roller reversible cold rolling mill, and the final hardness reduction rate is controlled to be 30%; S5. Degrease the 304 stainless steel hard coil at a degreasing temperature of 39°C; S6. The degreased steel coil is placed in a bell-type annealing furnace filled with argon protection, annealed at 450°C, kept warm for 45 hours, and finally a stainless steel hard product with a hardness increased by 56HV is obtained.
[0014] Example 5 A production method for improving the surface hardness of 300 series austenitic stainless steel, comprising the following steps: S1. Perform hot continuous annealing and pickling on 1600 mm wide 300 series hot-rolled black coil stainless steel at an annealing temperature of 1200°C to obtain a solid solution stainless steel coil; S2, rolling the solid solution stainless steel coil through a 20-roller reversible cold rolling mill with a total reduction rate of 20% to obtain intermediate rolling hardened stainless steel; S3, performing recrystallization annealing and pickling on the intermediate rolling hardened stainless steel, the annealing temperature is 1200° C., and 300 series stainless steel after recrystallization annealing and pickling is obtained; S4, the 300 series stainless steel after recrystallization annealing and pickling is subjected to final hardness rolling on a 20-roller reversible cold rolling mill, and the final hardness reduction rate is controlled to be 40%, so as to obtain a 300 series stainless steel final rolling process hardened steel coil; S5. Degrease the 300 series stainless steel hard coils at a degreasing temperature of 45°C; S6. The degreased steel coil is subjected to cold continuous annealing, and then pickled by neutral salt electrolysis + nitric acid electrolysis, or the degreased steel coil is placed in a bell-type annealing furnace filled with argon protection for annealing, and finally a stainless steel hard product with a hardness increased by 100HV is obtained.
[0015] Wherein, in the step S6, specifically, the degreased steel coil is subjected to cold continuous annealing at 750°C, the annealing speed is 30m / min, and then subjected to neutral salt electrolysis + nitric acid electrolysis pickling, the neutral salt current is 8000A, the concentration is 300g / L, the nitric acid current is 6000A, the concentration is 300g / L, and the temperature is 60°C, or the degreased steel coil is placed in a bell-type annealing furnace filled with argon protection, annealed at 750°C, and kept warm for 48h before being taken out of the furnace.
[0016] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A production method for improving the surface hardness of 300 series austenitic stainless steel, characterized in that: The following steps are involved: S1. 300 series hot-rolled black coil stainless steel is subjected to hot continuous annealing and pickling at an annealing temperature of 1050°C-1200°C to obtain a solid solution stainless steel coil; S2. Rolling the solid solution stainless steel coil by a 20-roller reversible cold rolling mill, with a total reduction ratio of ≥10%, to obtain intermediate rolling hardened stainless steel; S3, performing recrystallization annealing and pickling on the intermediate rolling hardened stainless steel, the annealing temperature is 1050°C-1200°C, and 300 series stainless steel after recrystallization annealing and pickling is obtained; S4. The 300 series stainless steel after recrystallization annealing and pickling is subjected to final hardness rolling on a 20-roller reversible cold rolling mill, and the final hardness reduction rate is controlled to be 6%-60%, so as to obtain a 300 series stainless steel final rolling process hardened steel coil; S5. Degrease the 300 series stainless steel hard coils at a degreasing temperature of 38°C-45°C; S6. The degreased steel coil is subjected to cold continuous annealing, and then pickled by neutral salt electrolysis + nitric acid electrolysis, or the degreased steel coil is placed in a bell-type annealing furnace filled with argon protection for annealing, and finally a stainless steel hard product with a hardness increased by 10HV-100HV is obtained.
2. A production method for improving the surface hardness of 300 series austenitic stainless steel according to claim 1, characterized in that: In the step S6, specifically, the degreased steel coil is subjected to cold continuous annealing at 300°C-750°C, the annealing speed is 10m / min-100m / min, and then subjected to neutral salt electrolysis + nitric acid electrolysis pickling, the neutral salt current is 1000A-8000A, the concentration is 100g / L-300g / L, the nitric acid current is 1000A-6000A, the concentration is 100g / L-300g / L, and the temperature is 40-60°C, or the degreased steel coil is placed in a bell-type annealing furnace filled with argon protection, annealed at 300°C-750°C, and kept warm for 2h-48h before being taken out of the furnace, and finally a stainless steel hard product with a hardness increased by 10HV-100HV is obtained.
Citation Information
Patent Citations
Cold rolling hot-dip steel with thickness greater than 1.5 mm for folding forming and production method thereof
CN103451519A
Process method for improving mechanical property of cold-rolled 304 austenitic stainless steel
CN113234908A
Rolling method for 300-series wide stainless steel hard product
CN113578964A
2D surface control method conforming to ink test for SUS410L stainless steel for refrigerated container
CN117380771A
Preparation method of austenitic stainless steel hard rough surface product
CN117960781A