Manufacturing method of large hot forging die forging material
By adopting the manufacturing method of annular annealing furnace bottom plate in the manufacturing of large-scale hot forging die forging materials, the temperature drop and superheat of the ladle are controlled, and the air-cooled conditioning technology is adopted to solve the quality instability in the existing technology. and the problem of long production cycles have achieved the effect of reducing costs and shortening production cycles, and preventing white point defects.
Patent Information
- Application Number
- CN202411204750.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
There are problems in the manufacturing process of existing large-scale hot forging die forging materials, such as unstable quality, high production costs and long production cycles, especially the high energy consumption and long production cycles caused by hydrogenation annealing.
The manufacturing method of the annular annealing furnace furnace bottom plate includes steel ingot die injection, red heating, forging forming, after forging air cooling and rough processing, through controlling the temperature drop, overheating, two upset and two pull-out deformation system, and after forging air cooling and direct tempering process to reduce hydrogenation annealing steps, optimize process parameters to reduce hydrogen content and white point defects.
The production cycle is shortened by about 15 days, and the production cost is reduced by about 600 yuan/ton, which prevents the occurrence of white spot defects. By refining grains and online thermal cleaning, the quality stability of the forging is ensured.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of forging, and in particular to a method for manufacturing a large hot forging die forging material. Background Art
[0002] The main steel types of hot forging dies are SKT4, 5CrNiMo, 5CrNiMoV, etc. Large hot forging dies usually refer to forgings weighing more than 15 tons, using steel ingots of more than 20 tons. At present, the process adopted by most domestic manufacturers is steel ingot mold injection → hot delivery (cold delivery after annealing) heating → forging molding → normalizing + hydrogen expansion annealing → sawing both ends → quenching and tempering → rough processing. The following problems often occur when using this process: 1. Unstable quality, white spots are easy to appear during flaw detection; 2. High production cost, the production cost of normalizing and hydrogen expansion annealing is very high, and the energy consumption cost alone is as high as 600 yuan / t. 3. Long production cycle, the production cycle of a single piece of forging material is as long as 40 days. The reason for the long production cycle is that hydrogen expansion annealing takes about 10 days. Summary of the invention
[0003] The purpose of the present invention is to solve the problems existing in the above-mentioned prior art and to provide a method for manufacturing a furnace bottom plate of an annular annealing furnace.
[0004] The specific scheme of the present invention is as follows: a method for manufacturing a large hot forging die forging material, comprising the following steps: S1. Ingot casting, ensure that the ladle temperature drop is ≤1℃ / min, the superheat is controlled at 45-55℃, single tray casting is 45-50℃, double tray casting is 50-55℃; S2, hot-feed heating to ensure that the steel ingot is burned through without any yin or yang surface; S3, forging, using two upsetting and two drawing, wide and thick interchangeable deformation system; S4. After forging, air cool to 300-350℃ and then put into the furnace for tempering; S5. Rough machining.
[0005] Furthermore, in step S2, the high temperature insulation time = ingot diameter / 200, the high temperature insulation time of a 20-26t ingot is ≥10h, and the high temperature insulation time of a 26-30t ingot is ≥12h.
[0006] Furthermore, the step S3 is specifically as follows: upsetting in the first fire, the aspect ratio after upsetting is controlled between 0.5-1 and the upsetting reduction rate is ≥35%, and then drawing to a flat billet, the width-to-thickness ratio of the flat billet is controlled between 1.2-1.4, and the aspect ratio is controlled between 2.2-2.5; upsetting again in the second fire, the upsetting parameters are the same as the first time, the riser pressure clamp handle is used, the width and thickness are interchanged to draw to the forging size, the clamp handle is chopped off, and the red forging material is cleaned online with a cutter to remove defects such as folding, cracks, shrinkage holes, etc. at the head and tail.
[0007] Furthermore, the tempering process in step S4 includes the following steps: first quenching at 880°C and holding for a holding time of effective size of the forging material / 50, and then intermittent water cooling until the surface temperature returns to 200-250°C; then tempering, the tempering temperature is determined according to the hardness required by the forging material, and the tempering holding time is effective size of the forging material / 25.
[0008] Furthermore, in step S4, since there is a lot of retained austenite in the hot forging die steel after quenching and tempering, at least two temperings are required to eliminate the stress generated by the retained austenite.
[0009] The method of the present invention is obtained after repeated research, reasoning and verification by the inventor in long-term work practice. The reasons for the process and process parameters adopted in the method of the present invention are as follows: (1) Controlling the temperature drop of the ladle and the appropriate superheat can reduce the segregation and air absorption of molten steel during the pouring process, thereby reducing the hydrogen content in the steel and preventing the occurrence of white spot defects.
[0010] (2) Heat the steel ingot to 100-150℃ below the solidus temperature and keep it warm for a sufficient time to fully austenitize and ensure that the steel ingot is burned through, thereby improving the ability to weld defects during forging.
[0011] (3) The deformation system of two upsetting and two pulling, and interchange of width and thickness is adopted in the forging process, mainly to make the deformation relatively uniform, break the dendrites of the steel ingot, refine the grains, weld the defects such as looseness and bubbles, make hydrogen have nowhere to hide, and prevent the occurrence of white spot defects. After forming, chop off the pliers handle and clean up the defects at the head and tail, in order to create good conditions for direct quenching and tempering after forging, and prevent the head and tail from bursting due to defects during the quenching and tempering process.
[0012] (4) After forging, air cool to 300-350℃ to refine the grains and create good conditions for direct tempering after forging. At the same time, air cooling is also to fully expand hydrogen and release hydrogen, thereby controlling the generation of white spot defects.
[0013] (5) The present invention adopts a direct tempering process after forging, which reduces the hydrogen expansion annealing process compared to the prior art. The hydrogen expansion process takes a long time, but the white spot problem still occurs. Direct tempering after forging can prevent the generation of white spots. Because hydrogen expansion annealing produces ordinary pearlite at room temperature, pearlite has poor hydrogen solubility, only 2ppmm. When cooling from austenite to pearlite, the solubility of hydrogen decreases, and a large number of hydrogen atoms will not have time to diffuse and will gather into hydrogen molecules at the defects. A large number of hydrogen molecules will gather and eventually generate great stress, which will exceed the strength limit of steel and form hydrogen cracks. However, tempering only produces martensite and tempered troostite at low temperature, which have strong hydrogen solubility and can reach 8ppm. In martensite and troostite, there are many lattice defects, and hydrogen molecules are not easy to gather. The incubation cycle of white spots is much longer than that of pearlite, so it is difficult to produce white spots.
[0014] Compared with the prior art, the present invention has the following beneficial effects: 1. It optimizes the process flow, shortens the production cycle, and significantly reduces the production cost. The production cycle can be shortened by about 15 days, and the cost per ton of steel can be reduced by about 600 yuan.
[0015] 2. This process only produces troostite and martensite with strong hydrogen solubility at room temperature, and does not produce pearlite with poor hydrogen solubility, thereby preventing hydrogen accumulation from producing white spot defects.
[0016] 3. Through two upsetting and two drawing, width and thickness interchange, air cooling after forging, the grains are refined. At the same time, the defects at both ends of the forging material are cleaned online to create favorable conditions for direct tempering after forging and prevent direct tempering after forging. Explosion. DETAILED DESCRIPTION
[0017] In order to better explain the technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with specific embodiments. The following embodiments are merely illustrative of the technical solution of the present invention and do not limit the present invention in any form.
[0018] Implementation Case 1 This embodiment is steel grade SKT4, the forging module is 650mm×710mm×4200mm, 21t octagonal ingot is selected for forging, the diameter of the octagonal ingot is 1130mm, and the forging ratio is 6.3. The specific implementation process is as follows: S1. Double tray casting is adopted, the casting temperature is 1533-1538℃, and 21t octagonal ingot is cast. After the surface of the ingot is demoulded at 650℃, it is red-sent to the heating furnace of the forging steel plant.
[0019] S2. Heat the 21t octagonal ingot to 1260℃ and keep it warm for 10h, then start forging. The 31.5MN hydraulic press uses a wide anvil with a width of 500mm. The first fire upsetting is roughened to 1500mm, and the lengthening is to 980mm×1180mm. The second fire upsetting is roughened to 1500mm. The clamp handle is used, and the width and thickness are interchangeable. The lengthening is to the forging material size. The main deformation requires full anvil, the pressing amount is ≥20%, and it is not less than four times. After forming, the defects at both ends are cleaned online with a cutter.
[0020] S3. After forging, air cool to 300-350℃, quickly heat up to 550℃ and keep warm for 2h, heat up to 880℃ at 60℃ / h and keep warm for 14h, use intermittent water cooling until the surface temperature returns to 200-250℃. Then put it into 300 furnace and keep warm for 3h, heat up to 560℃ at 60℃ / h and keep warm for 27h for the first tempering, test the hardness after taking it out of the furnace, and then carry out the second tempering.
[0021] S4. Perform rough machining.
[0022] Implementation Case 2 This embodiment uses 5CrNiMoV steel, a forging module of 700mm×1000mm, and uses a 26t octagonal ingot for forging. The diameter of the octagonal ingot is 1250mm, and the forging ratio is 5.5. The specific implementation process is as follows: S1. Use single tray casting, casting temperature 1532-1537℃, casting 26t octagonal ingot, the ingot surface is 650℃ and then demoulded and sent to the heating furnace of forging steel plant.
[0023] S2. Heat the 26t octagonal ingot to 1270℃ and keep it warm for 12h, then start forging. The 31.5MN hydraulic press uses a wide anvil with a width of 500mm. The first fire upsetting is roughened to 1700mm, and the lengthening is to 1050mm×1260mm. The second fire upsetting is roughened to 1700mm. The clamp handle is used, and the width and thickness are interchangeable. The lengthening is to the forging size. The main deformation requires full anvil, and the pressing amount is ≥20%, and no less than four times. After forming, the defects at both ends are cleaned online with a cutter. S3. After forging, air cool to 300-350℃, quickly heat up to 550℃ and keep warm for 2h, heat up to 880℃ at 60℃ / h and keep warm for 17h, use intermittent water cooling until the surface temperature returns to 200-250℃. Then put it into 300 furnace and keep warm for 3h, heat up to 580℃ at 60℃ / h and keep warm for 33h for the first tempering, test the hardness after taking it out of the furnace, and then carry out the second tempering.
[0024] S4. Perform rough machining.
Claims
1. A method for manufacturing a large hot forging die forging material, Its characteristics are: The following steps are involved: S1. Ingot casting, ensure that the ladle temperature drop is ≤1℃ / min, the superheat is controlled at 45-55℃, single tray casting is 45-50℃, double tray casting is 50-55℃; S2, hot-feed heating to ensure that the steel ingot is burned through without any yin or yang surface; S3, forging, using two upsetting and two drawing, wide and thick interchangeable deformation system; S4. After forging, air cool to 300-350℃ and then put into the furnace for tempering; S5. Rough machining.
2. A method for manufacturing a large hot forging die forging material according to claim 1, Its characteristics are: In the step S2, the high temperature insulation time = ingot diameter / 200, the high temperature insulation time of a 20-26t ingot is ≥10h, and the high temperature insulation time of a 26-30t ingot is ≥12h.
3. The method for manufacturing a large hot forging die forging material according to claim 1, Its characteristics are: The step S3 is specifically as follows: upsetting in the first fire, the height-to-diameter ratio after upsetting is controlled between 0.5-1 and the upsetting reduction rate is ≥35%, and then drawing to a flat billet, the width-to-thickness ratio of the flat billet is controlled between 1.2-1.4, and the height-to-width ratio is controlled between 2.2-2.5; upsetting again in the second fire, the upsetting parameters are the same as the first time, the riser pressure clamp handle is used, the width and thickness are interchanged and drawn to the forging size, the clamp handle is chopped off, and the red forging material is cleaned online with a cutter to remove defects such as folding, cracks, shrinkage holes, etc. at the head and tail.
4. The method for manufacturing a large hot forging die forging material according to claim 1, Its characteristics are: The tempering process in step S4 includes the following steps: first quenching at 880°C and holding time = effective size of forging material / 50, intermittent water cooling until the surface temperature returns to 200-250°C; then tempering, the tempering temperature is determined according to the hardness required by the forging material, and the tempering holding time = effective size of forging material / 25.
5. A method for manufacturing a large hot forging die forging material according to claim 4, Its characteristics are: In step S4, since there is a lot of retained austenite in the hot forging die steel after quenching and tempering, at least two temperings are required to eliminate the stress generated by the retained austenite.
Citation Information
Patent Citations
Forging method for 55NiCrMoV7 die steel
CN104722687A
Quenching-tempering heat treatment method for large-scale module die steel
CN108866285A
High-alloy tool and die steel and preparation method thereof
CN112322868A
Production method for controlling white spots of forging material
CN116219130A
Production method of low-carbon steel forged material
CN117512427A
Cited By
SKT4 die steel forge piece and preparation method thereof
CN119710437A