Method for rapidly sintering superfine iron-copper-nickel pre-alloy powder in electric heating power multi-physical field

Through electric and thermal multi-physics coupled sintering technology, the problems of complex sintering process, long time and high energy consumption of pre-alloy powder are solved, and the ultra-fine iron-copper-nickel pre-alloy powder products with low temperature fast burning, dense and high performance are realized, and the process is simplified. , reduce costs and reduce environmental pollution.

CN118989323APending Publication Date: 2024-11-22SICHUAN UNIV
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411133915.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing pre-alloy powder sintering technology has problems such as complex process, long sintering time and high energy consumption, which affects production efficiency and cost.

Method used

The method of rapid sintering ultrafine iron-copper-nickel prealloy powder by electric thermal multi-physics field is adopted to achieve a lower sintering temperature and a shorter time through the coupling of alternating electric field, thermodynamic temperature field and force field, and no need to add sintering aids , improve product density and performance.

Benefits of technology

It has achieved the reduction of sintering temperature, shortening of time, and improved product density and performance, simple process, high efficiency, low energy consumption, and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989323A_ABST
    Figure CN118989323A_ABST
Patent Text Reader

Abstract

The invention discloses a method for rapidly sintering superfine iron-copper-nickel pre-alloyed powder in an electric heating power multi-physical field, and belongs to the technical field of pre-alloyed powder sintering, and the method comprises the steps that the mass of the superfine iron-copper-nickel pre-alloyed powder is calculated; the weighed superfine iron-copper-nickel pre-alloy powder is filled into a graphite mold; fixing the graphite mold in an electric heating power multi-physical field sintering experiment machine; the superfine iron-copper-nickel pre-alloy powder is subjected to pre-sintering treatment and sintering treatment; after sintering treatment is completed, when the sintered target part is cooled to 50 DEG C or below, the target part is taken out of the graphite mold; and testing the performance of the target part. A plurality of physical fields such as an alternating electric field, a thermodynamic temperature field and a force field are coupled to act on the sintering process of the superfine iron-copper-nickel pre-alloy powder, so that the temperature required by sintering is lower, the sintering time is shorter, and meanwhile, the sintering can be completed without adding a sintering aid in the sintering process; and the sintered product has higher density and better performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pre-alloy powder sintering, and in particular relates to a method for rapidly sintering ultrafine iron-copper-nickel pre-alloy powder using an electric, thermal and force multi-physical field. Background Art

[0002] In the diamond tool industry, the matrix powder used in traditional diamond metal tools is obtained by mechanically mixing various single powders through equipment such as ball mills. This method has some disadvantages: in the process of mixing various powders in the ball mill, due to the different particle sizes and densities among the various powders, there is uneven mixing, resulting in component segregation and aggregation; since diamond is prone to graphitization at high temperatures, too high a temperature is often not used to make diamond tools, but the sintering temperature of metal powder is relatively high, and a lower temperature will result in insufficient alloying of the metal powder, resulting in reduced holding force and service life of the diamond tool; the production process of traditional diamond tools is complicated, the sintering time is long, and the energy consumption is high.

[0003] Pre-alloyed powder is a technology developed in the 1980s. It is a matrix powder prepared by atomization, hydrometallurgy and other methods according to a certain composition ratio. Compared with traditional matrix powder, pre-alloyed powder matrix powder has higher hardness, toughness, strength and wear resistance, more uniform components, and alloyed powder has a lower melting point and lower sintering temperature.

[0004] At present, the pre-alloyed powder industry has been perfected and the production of related products has been standardized. However, existing sintering technologies such as hot pressing sintering, microwave sintering, laser sintering, etc. still have shortcomings such as complex process, long sintering time, and high energy consumption, which seriously affect production efficiency and increase production costs. Summary of the invention

[0005] The purpose of the present invention is to provide a method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder by electro-thermal multi-physical fields in view of the above-mentioned deficiencies in the prior art, so as to solve the problems of the existing pre-alloyed powder sintering technology such as complex process, long sintering time and high energy consumption.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for rapidly sintering ultrafine iron-copper-nickel pre-alloyed powder by using multiple physical fields of electricity, heat and force, comprising the following steps:

[0008] S1. Calculate the mass of the ultrafine iron-copper-nickel pre-alloyed powder according to the volume of the target part to be sintered;

[0009] S2, filling the weighed ultrafine iron-copper-nickel pre-alloyed powder into a graphite mold;

[0010] S3, fixing the graphite mold in an electric, thermal and mechanical multi-physics field sintering test machine;

[0011] S4, setting the loading parameters of the electric, thermal and mechanical multi-physics field sintering test machine, and pre-sintering the ultrafine iron, copper and nickel pre-alloyed powder in the graphite mold according to the loading parameters;

[0012] S5. After the pre-sintering process is completed, the loading parameters of the electric, thermal and mechanical multi-physics field sintering test machine are set again, and the ultrafine iron-copper-nickel pre-alloyed powder in the graphite mold is sintered according to the re-set loading parameters;

[0013] S6. After the sintering process is completed, when the temperature of the sintered target part drops below 50° C., the target part is taken out from the graphite mold;

[0014] S7. Perform performance test on the target parts based on the density and Rockwell hardness of the target parts.

[0015] Furthermore, the density of the ultrafine Fe-Cu-Ni pre-alloyed powder in S1 is 8.15 g / cm 3 , the median particle size D50 is 5 μm, and the mass ratio of iron, copper and nickel is 7:2:1.

[0016] Furthermore, the graphite mold in S2 includes a left punch, a right punch and a die; the left punch and the right punch each include a pressure push rod and an end cover, respectively; the pressure push rod includes a conical part and a cylindrical part; the tip of the conical part is fixedly connected to one end of the cylindrical part; the bottom end of the conical part is fixedly connected to the end cover; a 45° chamfer is provided between the conical part and the end cover of the pressure push rod; the die is a hollow columnar structure, and both ends of the hollow columnar structure are provided with a 45° chamfer; the two pressure push rods are respectively embedded in the two ends of the die, and a cavity for filling ultrafine iron-copper-nickel pre-alloyed powder is formed between the two pressure push rods and the die.

[0017] Furthermore, in S3, the end caps at both ends of the graphite mold are fixed by a fixture on the electric, thermal and mechanical multi-physics field sintering experimental machine, and the electric field, force field and temperature field are applied to the ultrafine iron-copper-nickel pre-alloyed powder through the end caps at both ends.

[0018] Further, in S4, the ultrafine iron-copper-nickel pre-alloyed powder in the graphite mold is pre-sintered, including:

[0019] The vacuum degree was set to less than 0.01 Pa, and a pressure of 3 MPa was applied to the end caps at both ends of the graphite mold. At the same time, an alternating electric field of 50 Hz and 2 V was applied. The temperature was raised to 600 °C and kept warm for 20 seconds.

[0020] Further, in S5, the ultrafine iron-copper-nickel pre-alloyed powder in the graphite mold is sintered, including:

[0021] Increase the pressure of the end caps at both ends of the graphite mold to 5-9 MPa, set the heating rate to 20°C / s, and when the temperature is increased from 600°C to 800-900°C, apply a 5V alternating electric field at both ends of the graphite mold and keep it warm for 360-600s.

[0022] Further, the pressure of the end caps at both ends of the graphite mold in S5 is 5Mpa, 7Mpa or 9Mpa;

[0023] The temperature is increased to 800°C, 850°C or 900°C;

[0024] The holding time is 360s, 480s or 600s.

[0025] Furthermore, S6 specifically includes:

[0026] After the sintered target parts are kept warm, they are cooled to room temperature at a rate of 5°C / s, and then taken out of the graphite mold.

[0027] Furthermore, S7 performs performance tests on the target parts, including:

[0028] Calculate the density of the target part, compare the calculated density of the target part with the theoretical density, and then perform a performance test on the target part;

[0029] The Rockwell hardness of the target part surface was measured using a microhardness tester, and a load of 0.2 kgf was applied to the target part; the surface state of the target part was observed using a JEOL L-type scanning electron microscope.

[0030] Furthermore, the density of the target part is calculated in S7, including:

[0031]

[0032] Among them, ρ 样品 is the density of the target part in the air, m 空气中质量 is the mass of the target part in the air, m 蒸馏水中质量 is the mass of the target part in distilled water, ρ 蒸馏水 is the density of the target part in distilled water.

[0033] The method for rapidly sintering ultrafine iron-copper-nickel pre-alloyed powder by using electric, thermal and mechanical multi-physical fields provided by the present invention has the following beneficial effects:

[0034] 1. The technology of the present invention couples multiple physical fields such as alternating electric field, thermodynamic temperature field and force field to act on the sintering process of ultrafine iron-copper-nickel pre-alloyed powder, so that the sintering temperature required is lower and the sintering time is shorter. At the same time, sintering can be completed without adding sintering aids during the sintering process, and the sintered products have higher density and better performance.

[0035] 2. When the alternating current of the present invention flows through the mold and the powder, the Joule heating effect of the current generated causes the temperature of the mold and the pre-alloyed powder to rise, and the originally loose powder particles are affected by thermal expansion and contraction, and the gaps between the powders become smaller; under the action of pressure, the pre-alloyed powder particles undergo plastic deformation and produce relative slip, further filling the pores; under the action of the alternating current, electrothermal aggregation occurs between the powder particles, accelerating the densification of the powder; when the temperature rises to a certain level, the surface area of ​​the powder particles melts to form a micro-liquid phase, thereby causing the powder particles to produce metallurgical bonding.

[0036] 3. Excellent product performance: The ultrafine iron-copper-nickel pre-alloyed powder prepared by the electric-thermal-mechanical multi-physical field coupled sintering process has high density, high hardness, dense surface state and few pores.

[0037] 4. Simple working conditions: The electric-thermal-mechanical multi-physical field coupled sintering process proposed in the present invention only requires equipment that can provide a stable vacuum degree, alternating electric field, pressure and heating rate. No other processes and special equipment are required. This method has simple processes, high efficiency, low energy consumption and low cost, and has great advantages over traditional powder metallurgy.

[0038] 5. Short sintering time and low sintering temperature: Compared with traditional powder metallurgy, the present invention adds an electric field to assist the sintering process. Under the action of Joule heat effect and electrothermal focusing effect, the heating time is significantly shortened, the axial shrinkage of the powder during the sintering process is accelerated, the powders are denser, the sintering time is greatly shortened, and the sintering temperature is reduced.

[0039] 6. Environmentally friendly: The sintering process does not produce waste gas, waste water, or waste residue, and will not pollute the environment. It is a green, clean and efficient sintering process.

[0040] 7. The present invention first pre-sinters the ultrafine iron-copper-nickel pre-alloyed powder, and then performs a formal sintering process based on the process parameters of the pre-sintering process. The purpose is to reduce the sintering time, reduce energy consumption, and improve the density of the sintered sample; the pre-sintering creates certain initial temperature conditions and powder surface states for the formal sintering, so that the sintering can proceed more smoothly. In the pre-sintering stage, the gaps between the powders are large, and the resistance between the powders is also large. A large amount of Joule heat is generated under the action of the electric field, and the heating time is significantly reduced. The higher heating rate helps to quickly reach the sintering temperature and improve the forming efficiency; under the action of pressure, the powder undergoes elastic-plastic deformation, and the contact between the powders changes from point contact to surface contact. The gaps between the powders are rapidly reduced, and the density is rapidly increased. In the formal sintering stage, the high temperature conditions in the pre-sintering stage cause the powder to soften, undergo plastic deformation and local liquefaction, and the contact area is further increased. Under the action of pressure field, electrothermal focusing effect, particle surface tension, etc., the liquid metal quickly fills into the pores of the powders that are in contact with each other. After the liquid metal solidifies, the contact surface between the powder particles disappears, forming a sintering neck, achieving metallurgical bonding, and further improving the density of the sintered sample. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 The present invention is a flow chart of the method for rapidly sintering ultrafine iron-copper-nickel pre-alloyed powder using electric, thermal and mechanical multi-physical fields.

[0042] Figure 2 It is a structural schematic diagram of the graphite mold of the present invention.

[0043] Figure 3 This is a SEM picture of the sintering of the ultrafine iron-copper-nickel pre-alloyed powder of the present invention, wherein: Figure 3 (a) and (c) are SEM images of the target part surface under the sintering conditions of 850°C, 9MPa pressure, and 360s; Figure 3 (b) and (d) are SEM images of the target part surface under the sintering conditions of 850°C, 9MPa pressure and 600s. DETAILED DESCRIPTION

[0044] The specific implementation modes of the present invention are described below so that those skilled in the art can understand the present invention. However, it should be clear that the present invention is not limited to the scope of the specific implementation modes. For those of ordinary skill in the art, as long as various changes are within the spirit and scope of the present invention as defined and determined by the attached claims, these changes are obvious, and all inventions and creations utilizing the concept of the present invention are protected.

[0045] Example 1

[0046] This embodiment provides a method for rapidly sintering ultrafine iron-copper-nickel pre-alloyed powder by electrothermal-mechanical multi-physical fields. Figure 1, which specifically includes the following:

[0047] Step S1, calculating the mass of the ultrafine iron-copper-nickel pre-alloyed powder according to the volume of the target part to be sintered;

[0048] The density of the ultrafine iron-copper-nickel pre-alloyed powder in this embodiment is 8.15 g / cm 3 , the median particle size D50 is 5 μm, and the mass ratio of iron, copper and nickel is 7:2:1.

[0049] Step S2, filling the weighed ultrafine iron-copper-nickel pre-alloyed powder into a graphite mold;

[0050] refer to Figure 2 The graphite mold of this embodiment includes a left punch, a right punch and a die. The left punch and the right punch respectively include a pressure push rod and an end cover. The pressure push rod includes a conical part and a cylindrical part. The tip of the conical part is fixedly connected to one end of the cylindrical part, and the bottom end of the conical part is fixedly connected to the end cover. A 45° chamfer is arranged between the conical part and the end cover of the pressure push rod. The die is a hollow columnar structure, and both ends of the hollow columnar structure are provided with a 45° chamfer; two pressure push rods are respectively embedded in the two ends of the die, and a cavity for filling ultrafine iron-copper-nickel pre-alloyed powder is formed between the two pressure push rods and the die.

[0051] Step S3, fixing the graphite mold in an electric, thermal and mechanical multi-physics field sintering test machine;

[0052] The end caps at both ends of the graphite mold are fixed by fixtures on an electric, thermal and mechanical multi-physics field sintering experimental machine, and electric field, force field and temperature field are applied to the ultrafine iron-copper-nickel pre-alloyed powder through the end caps at both ends.

[0053] Step S4, setting the loading parameters of the electric, thermal and mechanical multi-physics field sintering test machine, and pre-sintering the ultrafine iron, copper and nickel pre-alloyed powder in the graphite mold according to the loading parameters;

[0054] The vacuum degree was set to less than 0.01 Pa, and a pressure of 3 MPa was applied to the end caps at both ends of the graphite mold. At the same time, an alternating electric field of 50 Hz and 2 V was applied. The temperature was raised to 600 °C and kept warm for 20 seconds.

[0055] In this embodiment, the pre-alloyed powder is first pre-sintered, so that the powder in a loose state can be displaced, rearranged and filled under the action of external pressure, the pores between the powders are reduced, elastic-plastic deformation occurs, and the powders are fully in contact; under the action of the Joule heating effect of the alternating electric field, the powder temperature rises rapidly.

[0056] Step S5, after the pre-sintering process is completed, the loading parameters of the electric, thermal and mechanical multi-physics field sintering test machine are set again, and the ultrafine iron-copper-nickel pre-alloyed powder in the graphite mold is sintered according to the re-set loading parameters;

[0057] Increase the pressure of the end caps at both ends of the graphite mold to 5-9 MPa, set the heating rate to 20°C / s, and when the temperature is increased from 600°C to 800-900°C, apply a 5V alternating electric field at both ends of the graphite mold and keep it warm for 360-600s.

[0058] In this embodiment, the electric field, temperature field and force field work together and influence each other. Under the action of external pressure, the powder undergoes plastic deformation to make the powder more dense; under the action of temperature, the powder surface is partially liquefied, and multiple liquefied powder surfaces are connected to form a sintering neck; in the insulation stage, under the action of the electric field force of the alternating electric field, the powder distribution is more uniform, and under the action of the electrothermal focusing effect, the pores between the powders are further reduced, and the sintered sample is more uniform and dense.

[0059] Step S6: After the sintering process is completed, when the temperature of the sintered target part drops below 50° C., the target part is taken out from the graphite mold;

[0060] After the sintered target parts are kept warm, they are cooled to room temperature at a rate of 5°C / s and then taken out of the graphite mold.

[0061] Step S7: Based on the density and Rockwell hardness of the target part, a performance test is performed on the target part.

[0062] Calculate the density of the target part, compare the calculated density of the target part with the theoretical density, and then perform performance tests on the target part:

[0063]

[0064] Among them, ρ 样品 is the density of the target part in the air, m 空气中质量 is the mass of the target part in the air, m 蒸馏水中质量 is the mass of the target part in distilled water, ρ 蒸馏水 is the density of the target part in distilled water.

[0065] The Rockwell hardness of the target part surface was measured using a microhardness tester, and a load of 0.2 kgf was applied to the target part; the surface state of the target part was observed using a JEOL L-type scanning electron microscope.

[0066] Example 2

[0067] Based on the method in Example 1, this embodiment provides a method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder using multiple physical fields of electricity, heat and force, which specifically includes the following contents:

[0068] A1. Select pre-alloyed powder with a density of 8.15 g / cm3, a median particle size D50 of 5 μm, and an iron-copper-nickel mass ratio of 7:2:1 as the material to be sintered.

[0069] A2. Calculate the mass of the required ultrafine iron-copper-nickel pre-alloy powder according to the volume of the target parts to be sintered, and weigh it with an electronic balance for later use.

[0070] A3. Pour the weighed ultrafine iron-copper-nickel pre-alloyed powder into the graphite die and cover it with the left and right punches.

[0071] A4. Carry out pre-sintering, set the vacuum degree to less than 0.01Pa, apply a pressure of 3MPa to both ends of the graphite mold, and apply an alternating electric field of 50Hz and 2V at the same time, raise the temperature to 600℃, and keep it warm for 20s.

[0072] A5. Increase the pressure at both ends of the mold to 5MPa, set the heating rate to 20℃ / s, and when the temperature rises to 800℃, apply a 5V alternating electric field at both ends of the graphite mold and keep it warm for 360s.

[0073] A6. After the insulation is completed, the temperature is lowered to room temperature at a rate of 5℃ / s, and finally the sintered target parts are taken out of the graphite mold.

[0074] A7. The target parts were tested for performance. The density of the prepared target parts was 7.915 g / cm3, the density was 97.12%, and the Rockwell hardness HRB was 105.48.

[0075] Example 3

[0076] Based on the method in Example 1, this embodiment provides a method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder using multiple physical fields of electricity, heat and force, which specifically includes the following contents:

[0077] B1, select density as 8.15g / cm 3 The pre-alloyed powder with a median particle size D50 of 5 μm and an iron-copper-nickel mass ratio of 7:2:1 was used as the material to be sintered.

[0078] B2. Calculate the mass of the required ultrafine iron-copper-nickel pre-alloy powder according to the volume of the target parts to be sintered, and weigh it with an electronic balance for later use.

[0079] B3. Pour the weighed ultrafine iron-copper-nickel pre-alloyed powder into the graphite die and cover it with the left and right punches.

[0080] B4. Perform pre-sintering, set the vacuum degree to less than 0.01Pa, apply a pressure of 3MPa to both ends of the graphite mold, and apply an alternating electric field of 50Hz and 2V at the same time, raise the temperature to 600℃, and keep it warm for 20s.

[0081] B5. Increase the pressure at both ends of the mold to 5MPa, set the heating rate to 20℃ / s, and when the temperature rises to 850℃, apply a 5V alternating electric field at both ends of the graphite mold and keep it warm for 360s.

[0082] B6. After the insulation is completed, the temperature is lowered to room temperature at a rate of 5℃ / s, and finally the sintered target parts are taken out of the graphite mold.

[0083] B7. Perform performance test on target parts. The density of the prepared parts is 7.966g / cm 3 , density is 97.74%, and Rockwell hardness HRB is 108.17.

[0084] Example 4

[0085] Based on the method in Example 1, this embodiment provides a method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder using multiple physical fields of electricity, heat and force, which specifically includes the following contents:

[0086] C1, select density as 8.15g / cm 3 The pre-alloyed powder with a median particle size D50 of 5 μm and an iron-copper-nickel mass ratio of 7:2:1 was used as the material to be sintered.

[0087] C2. Calculate the mass of the required ultrafine iron-copper-nickel pre-alloy powder according to the volume of the target parts to be sintered, and weigh it with an electronic balance for later use.

[0088] C3. Pour the weighed ultrafine iron-copper-nickel pre-alloyed powder into the graphite die and cover it with the left and right punches.

[0089] C4. Pre-sintering was performed, the vacuum degree was set to be less than 0.01Pa, a pressure of 3MPa was applied to both ends of the graphite mold, and an alternating electric field of 50Hz and 2V was applied at the same time, the temperature was raised to 600℃, and the temperature was kept for 20s.

[0090] C5. Increase the pressure at both ends of the mold to 5 MPa, set the heating rate to 20 °C / s, and when the temperature rises to 900 °C, apply a 5V alternating electric field to both ends of the graphite mold and keep warm for 360 seconds.

[0091] C6. After the insulation is completed, the temperature is lowered to room temperature at a rate of 5℃ / s, and finally the sintered target parts are taken out of the graphite mold.

[0092] C7. The target parts were tested for performance. The density of the prepared target parts was 7.953 g / cm 3 , density is 97.58%, and Rockwell hardness HRB is 107.95.

[0093] Example 5

[0094] Based on the method in Example 1, this embodiment provides a method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder using multiple physical fields of electricity, heat and force, which specifically includes the following contents:

[0095] D1, select density as 8.15g / cm 3 The pre-alloyed powder with a median particle size D50 of 5 μm and an iron-copper-nickel mass ratio of 7:2:1 was used as the material to be sintered.

[0096] D2. Calculate the mass of the required ultrafine iron-copper-nickel pre-alloy powder according to the volume of the target parts to be sintered, and weigh it with an electronic balance for later use.

[0097] D3. Pour the weighed ultrafine iron-copper-nickel pre-alloyed powder into the graphite die and cover it with the left and right punches.

[0098] D4. Perform pre-sintering, set the vacuum degree to less than 0.01Pa, apply a pressure of 3MPa to both ends of the graphite mold, and apply an alternating electric field of 50Hz and 2V at the same time, raise the temperature to 600℃, and keep it warm for 20s.

[0099] D5. Increase the pressure at both ends of the mold to 7MPa, set the heating rate to 20℃ / s, and when the temperature rises to 850℃, apply a 5V alternating electric field to both ends of the graphite mold and keep it warm for 360s.

[0100] D6. After the insulation is completed, the temperature is lowered to room temperature at a rate of 5℃ / s, and finally the sintered target parts are taken out of the graphite mold.

[0101] D7. Perform performance test on target parts. The density of the prepared parts is 7.982g / cm 3 , density is 97.94%, and Rockwell hardness HRB is 109.15.

[0102] Example 6

[0103] Based on the method in Example 1, this embodiment provides a method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder using multiple physical fields of electricity, heat and force, which specifically includes the following contents:

[0104] E1, select density as 8.15g / cm 3 The pre-alloyed powder with a median particle size D50 of 5 μm and an iron-copper-nickel mass ratio of 7:2:1 was used as the material to be sintered.

[0105] E2. Calculate the mass of the required ultrafine iron-copper-nickel pre-alloy powder according to the volume of the target parts to be sintered, and weigh it with an electronic balance for later use.

[0106] E3. Pour the weighed ultrafine iron-copper-nickel pre-alloyed powder into the graphite die and cover it with the left and right punches.

[0107] E4. Perform pre-sintering, set the vacuum degree to less than 0.01Pa, apply a pressure of 3MPa to both ends of the graphite mold, and apply an alternating electric field of 50Hz and 2V at the same time, raise the temperature to 600℃, and keep it warm for 20s.

[0108] E5. Increase the pressure at both ends of the mold to 9 MPa, set the heating rate to 20 °C / s, and when the temperature rises to 850 °C, apply a 5V alternating electric field to both ends of the graphite mold and keep warm for 360 seconds.

[0109] E6. After the insulation is completed, the temperature is lowered to room temperature at a rate of 5℃ / s, and finally the sintered target parts are taken out of the graphite mold.

[0110] E7. Perform performance test on target parts. The density of the target parts is 8.002g / cm 3 , density is 98.18%, and Rockwell hardness HRB is 110.72.

[0111] Based on Examples 2 to 6, it can be seen that the parts obtained by sintering the iron-copper-nickel pre-alloyed powder using the method proposed in the present invention have high density, which is comparable to the powder density of 8.15 g / cm 3 In contrast, the density of the sintered bodies is above 97%;

[0112] Depend on Figure 3 From (a), (c) and (b), (d) in the figure, it can be seen that under the same conditions, temperature, pressure and holding time have a certain influence on the density of the parts, and the parts obtained at 850℃, 9MPa pressure and 600s holding time have the highest density.

[0113] Although the specific implementation of the invention is described in detail in conjunction with the drawings, it should not be understood as limiting the scope of protection of this patent. Within the scope described in the claims, various modifications and variations that can be made by those skilled in the art without creative work still fall within the scope of protection of this patent.

Claims

1. A method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder by electrothermal-mechanical multi-physical fields, characterized in that: The following steps are involved: S1. Calculate the mass of the ultrafine iron-copper-nickel pre-alloyed powder according to the volume of the target part to be sintered; S2, filling the weighed ultrafine iron-copper-nickel pre-alloyed powder into a graphite mold; S3, fixing the graphite mold in an electric, thermal and mechanical multi-physics field sintering test machine; S4, setting the loading parameters of the electric, thermal and mechanical multi-physics field sintering test machine, and pre-sintering the ultrafine iron, copper and nickel pre-alloyed powder in the graphite mold according to the loading parameters; S5. After the pre-sintering process is completed, the loading parameters of the electric, thermal and mechanical multi-physics field sintering test machine are set again, and the ultrafine iron-copper-nickel pre-alloyed powder in the graphite mold is sintered according to the re-set loading parameters; S6. After the sintering process is completed, when the temperature of the sintered target part drops below 50° C., the target part is taken out from the graphite mold; S7. Perform performance test on the target parts based on the density and Rockwell hardness of the target parts.

2. The method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder by electric-thermal-mechanical multi-physical fields according to claim 1, characterized in that: The density of the ultrafine iron-copper-nickel pre-alloyed powder in S1 is 8.15 g / cm 3 , the median particle size D50 is 5 μm, and the mass ratio of iron, copper and nickel is 7:2:

1.

3. The method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder by electric-thermal-mechanical multi-physical fields according to claim 1, characterized in that: The graphite mold in S2 includes a left punch, a right punch and a die; the left punch and the right punch each include a pressure push rod and an end cover; the pressure push rod includes a conical part and a cylindrical part; the tip of the conical part is fixedly connected to one end of the cylindrical part; the bottom end of the conical part is fixedly connected to the end cover; a 45° chamfer is provided between the conical part and the end cover of the pressure push rod; the die is a hollow columnar structure, and both ends of the hollow columnar structure are provided with a 45° chamfer; two pressure push rods are respectively embedded in the two ends of the die, and a cavity for filling ultrafine iron-copper-nickel pre-alloyed powder is formed between the two pressure push rods and the die.

4. The method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder by electric-thermal-mechanical multi-physical fields according to claim 1, characterized in that: In S3, the end caps at both ends of the graphite mold are fixed by a fixture on the electric, thermal and mechanical multi-physical field sintering experimental machine, and an electric field, a force field and a temperature field are applied to the ultrafine iron-copper-nickel pre-alloyed powder through the end caps at both ends.

5. The method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder by electric-thermal-mechanical multi-physical fields according to claim 1, characterized in that: The step S4 is to pre-sinter the ultrafine iron-copper-nickel pre-alloyed powder in the graphite mold, comprising: The vacuum degree was set to less than 0.01 Pa, and a pressure of 3 MPa was applied to the end caps at both ends of the graphite mold. At the same time, an alternating electric field of 50 Hz and 2 V was applied. The temperature was raised to 600 °C and kept warm for 20 seconds.

6. The method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder by electric-thermal-mechanical multi-physical fields according to claim 1, characterized in that: The step S5 is to sinter the ultrafine iron-copper-nickel pre-alloyed powder in the graphite mold, comprising: Increase the pressure of the end caps at both ends of the graphite mold to 5-9 MPa, set the heating rate to 20°C / s, and when the temperature is increased from 600°C to 800-900°C, apply a 5V alternating electric field at both ends of the graphite mold and keep it warm for 360-600s.

7. The method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder by electric-thermal-mechanical multi-physical fields according to claim 6, characterized in that: The pressure of the end caps at both ends of the graphite mold in S5 is 5Mpa, 7Mpa or 9Mpa; The temperature is increased to 800°C, 850°C or 900°C; The holding time is 360s, 480s or 600s.

8. The method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder by electric-thermal-mechanical multi-physical fields according to claim 1, characterized in that: The S6 specifically includes: After the sintered target parts are kept warm, they are cooled to room temperature at a rate of 5°C / s and then taken out of the graphite mold.

9. The method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder by electric-thermal-mechanical multi-physical fields according to claim 1, characterized in that: The performance test of the target part in S7 includes: Calculate the density of the target part, compare the calculated density of the target part with the theoretical density, and then perform a performance test on the target part; The Rockwell hardness of the target part surface was measured using a microhardness tester, and a load of 0.2 kgf was applied to the target part; the surface state of the target part was observed using a JEOL L-type scanning electron microscope.

10. The method for rapid sintering of ultrafine iron-copper-nickel pre-alloyed powder by electric-thermal-mechanical multi-physical fields according to claim 9, characterized in that: The density of the target part is calculated in S7, including: Among them, ρ 样品 is the density of the target part in the air, m 空气中质量 is the mass of the target part in the air, m 蒸馏水中质量 is the mass of the target part in distilled water, ρ 蒸馏水 is the density of the target part in distilled water.

Citation Information

Patent Citations

  • Method for preparing WC-Co hard alloy by rapid sintering under multi-physics coupling action

    CN102994852A

  • Ni-Ti porous material mini-sized part and sintering method thereof

    CN103862049A

  • WC-Ni mini-type component prepared based on multi-physics field activated sintering and preparing method of WC-Ni mini-type component

    CN104874796A

  • Method for preparing miniature ultrasonic motor stator based on multi-physical-field activated sintering

    CN109079135A

  • Method of preparing Mo-Cu alloy through field-assisted activated sintering

    CN112620631A