Supporting core device of bimetal composite pipe and preparation process

By using support core devices in the manufacturing process of bimetal composite pipes, using the cooperation of outer sleeves and propulsion rods, the shrinkage deformation problem caused by alloy rods is solved, and efficient welding composites and easy removal of support cores is achieved, improving the yield and applicability.

CN118989548APending Publication Date: 2024-11-22XIAN RES INST OF CHINA COAL TECH & ENG GRP CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411118237.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

During the manufacturing process of bimetal composite pipes, when the mechanical strength of the base pipe is low and the mechanical strength of the cover pipe is high, the use of alloy rods as support cores can easily lead to the overall shrinkage deformation, resulting in the inability to remove the support rods and base pipes, which will affect welding Effect.

Method used

Using a support core device including an outer sleeve, a movable left push rod, a right push rod and a limit screw, the appropriate support for the bimetal composite tube is achieved by adjusting the moving distance of the push rod and the change of the outer radius of the outer sleeve. , resists high temperature and high pressure shock waves of explosive welding, and facilitates removal of the support core after welding.

Benefits of technology

It effectively resists the shock wave of explosive welding, ensures the successful welding composite, and can easily remove the support core after welding, improves the yield rate, and is suitable for pipe processing of different specifications. It has high support strength and can be reused, with good economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989548A_ABST
    Figure CN118989548A_ABST
Patent Text Reader

Abstract

The invention provides a supporting core device of a bimetal composite pipe and a preparation technology, the technology adopts the supporting core device to realize explosive welding compounding of the bimetal composite pipe, the supporting core device comprises an outer sleeve, a pair of left pushing rod and right pushing rod is movably arranged in the outer sleeve, and the left pushing rod and the right pushing rod are arranged in the outer sleeve. Limiting screws are arranged in the left pushing rod and the right pushing rod, the two axial ends of each limiting screw extend out of the two axial ends of the outer sleeve correspondingly, and the two axial ends of each limiting screw are each detachably provided with a driving nut. Through cooperation of the pair of pushing rods and the outer sleeve, change of the overall outer diameter of the supporting core device is achieved, the supporting core device is adopted for explosive welding, high-temperature, high-pressure and high-speed shock waves of explosive welding can be resisted, welding compounding of the bimetal composite pipe is effectively guaranteed, and the welding quality of the bimetal composite pipe is improved. And meanwhile, the supporting core device can be conveniently taken out after welding is finished, the yield of the bimetal composite pipe is increased, and the explosive cladding process requirement is fully met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pipe preparation, relates to a bimetallic composite pipe, and specifically relates to a supporting core device and a preparation process of the bimetallic composite pipe. Background Art

[0002] Bimetallic composite pipe has the performance advantages of both base pipe and cladding pipe due to its special structure, and has broad application prospects in the industrial field. Bimetallic composite pipe includes an inner base pipe and an outer cladding pipe. The base pipe and cladding pipe are generally made of two metal materials with large differences in physical and chemical properties. The explosive welding composite technology can achieve metallurgical bonding between the material interfaces of the double base pipe and the cladding pipe, so as to maintain the advantages of the performance of each component material, thereby obtaining comprehensive performance that cannot be achieved by a single component material.

[0003] When bimetallic pipes are composited by explosive welding, especially when the strength of the covering pipe is higher than that of the base pipe, the inner pipe often shrinks and deforms due to the explosion shock wave. To address the above problem, the commonly used solution is to place an alloy rod as a support core in the bimetallic composite pipe to be processed. The defects of the above prior art are: the overall strength of the alloy rod is insufficient, which easily leads to the overall shrinkage and deformation of the bimetallic composite pipe, resulting in interference fit between the support rod and the base pipe and inability to remove it, which in turn leads to the inability to put the welded bimetallic composite pipe into use. Summary of the invention

[0004] In view of the defects and shortcomings of the prior art, the purpose of the present invention is to provide a supporting core device and a preparation process for a bimetallic composite pipe, so as to solve the technical problem in the prior art that when the mechanical strength of the base pipe of the bimetallic composite pipe is low and the mechanical strength of the covering pipe is high, the use of alloy rods easily leads to overall shrinkage and deformation of the bimetallic composite pipe.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions to achieve the above problems:

[0006] The invention discloses a preparation process of a bimetallic composite pipe, wherein the process adopts a supporting core device of the bimetallic composite pipe to realize the explosive welding composite of the bimetallic composite pipe.

[0007] The supporting core device of the bimetallic composite tube includes an outer sleeve, in which a pair of left propulsion rods and a right propulsion rod are movably arranged, and a limiting screw is arranged in the left propulsion rod and the right propulsion rod, and the axial ends of the limiting screw extend out of the axial ends of the outer sleeve respectively, and a driving nut is detachably installed on the axial ends of the limiting screw.

[0008] The left propulsion rod and the right propulsion rod have the same shape and are arranged opposite to each other; the left propulsion rod comprises, from left to right, a left propulsion rod outer section, a left propulsion rod middle section and a left propulsion rod inner section; the right propulsion rod comprises, from right to left, a right propulsion rod outer section, a right propulsion rod middle section and a right propulsion rod inner section.

[0009] The left propulsion rod, the right propulsion rod and the two driving nuts can move along the axial direction on the limiting screw, and the moving distances of the left propulsion rod and the right propulsion rod in the axial direction are equal; as the left propulsion rod and the right propulsion rod move in the axial direction, the outer radius of the outer sleeve also changes accordingly.

[0010] The process specifically includes the following steps:

[0011] Step 1: According to the change in the outer radius of the outer sleeve, the taper of the inner section of the left propulsion rod, and the propulsion distance, the moving distance of the left propulsion rod and the right propulsion rod in the axial direction is calculated and obtained using Formula I; the Formula I is:

[0012]

[0013] Where:

[0014] ΔY represents the change in the outer radius of the outer sleeve, in mm; ΔY is equal to the difference between the inner diameter of the bimetallic composite tube and the minimum outer diameter of the outer sleeve.

[0015] α represents the taper of the inner section of the left propulsion rod, in degrees.

[0016] l represents the propulsion distance, which means that the initial distance between the axial right end face of the left propulsion rod and the midpoint of the outer sleeve is the propulsion distance or the initial distance between the axial left end face of the right propulsion rod and the midpoint of the outer sleeve, and the unit is mm.

[0017] x represents the moving distance of the left propulsion rod in the axial direction, and the moving distance of the right propulsion rod in the axial direction is equal to it, and the unit is mm.

[0018] Step 2, device installation: prepare the bimetallic composite tube to be processed, insert the supporting core device of the bimetallic composite tube into the bimetallic composite tube, and push the left push rod and the right push rod into the outer sleeve by tightening the drive nut. When the moving distance of the left push rod and the right push rod in the axial direction reaches x, the outer diameter of the outer sleeve is equal to the inner diameter of the bimetallic composite tube, and the advancement is stopped.

[0019] Step three: perform explosion welding.

[0020] Step 4, take out the device: After the explosion welding is completed, wait until the temperature of the bimetallic composite pipe drops, loosen the drive nut, and then pull the left and right push rods out of the outer sleeve. After the outer diameter of the outer sleeve becomes smaller, take out the support core device of the bimetallic composite pipe.

[0021] The present invention also has the following technical features:

[0022] Specifically, the cavities in the outer sleeve are, from left to right, a left outer conical cavity, a left main body cavity, a left inner conical cavity, a middle transition cavity, a right inner conical cavity, a right main body cavity and a right outer conical cavity; the shapes of the left inner conical cavity and the right inner conical cavity are exactly the same and are symmetrically arranged, the shapes of the left main body cavity and the right main body cavity are exactly the same and are symmetrically arranged, and the shapes of the left outer conical cavity and the right outer conical cavity are exactly the same and are symmetrically arranged.

[0023] Specifically, the inner diameter of the bimetallic composite pipe to be processed is 92 mm, and the length of the bimetallic composite pipe to be processed is 600 mm.

[0024] Specifically and preferably, the taper α of the inner section of the left propulsion rod is 9°; the propulsion distance l is 45 mm; and the minimum outer diameter of the outer sleeve is 89 mm.

[0025] Specifically and preferably, the distance L0 between the axial outer ends of the left propulsion rod and the right propulsion rod is 1100 mm; the length L of the outer sleeve is 1000 mm; and the length of the limit screw is 1200 mm.

[0026] Specifically and preferably, the length L1 of the left propulsion rod and the right propulsion rod is 468 mm, and the outer diameter D1 of the middle section of the left propulsion rod and the middle section of the right propulsion rod is 50 mm.

[0027] Specifically and preferably, the thinnest wall thickness h of the outer sleeve is 20 mm.

[0028] Specifically, a thickened washer is installed on each of the axial ends of the limiting screw, and the thickened washer is located on the inner side of the driving nut.

[0029] Specifically and preferably, in step three, the instantaneous pressure of the explosion welding is greater than or equal to 700 MPa, the instantaneous temperature is greater than or equal to 3000° C., and the speed of the shock wave generated by the explosion welding is 500-1000 m / s.

[0030] The present invention also protects the supporting core device of the bimetallic composite pipe as described above.

[0031] Compared with the prior art, the present invention has the following beneficial technical effects:

[0032] (I) The supporting core device of the bimetallic composite pipe of the present invention realizes the change of the overall outer diameter of the supporting core device by cooperating with a pair of push rods and an outer sleeve. The supporting core device is used for explosive welding, which can not only resist the high temperature, high pressure and high-speed shock wave of explosive welding, but also effectively ensure the welding and bonding of the bimetallic composite pipe. At the same time, the supporting core device can be easily removed after the welding is completed, thereby improving the yield of the bimetallic composite pipe and fully meeting the requirements of the explosive bonding process.

[0033] (II) The outer diameter of the supporting core device of the bimetallic composite tube of the present invention can be changed, so it can adapt to the processing requirements of tubes of different specifications and has wide applicability.

[0034] (III) The supporting core device of the bimetallic composite pipe of the present invention has high supporting strength, can meet the requirements of explosive welding composite pipes under various process conditions, and the supporting core device can be repeatedly used, with high economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic diagram of the overall structure of the supporting core device of the bimetallic composite tube.

[0036] Figure 2 It is a schematic diagram of the structure of the limit screw, drive nut and thickened washer.

[0037] Figure 3 It is a schematic diagram of the structure of the left propulsion rod and the right propulsion rod.

[0038] Figure 4 Schematic diagram of the supporting process of the supporting core device of the bimetallic composite tube.

[0039] Figure 5 It is a schematic diagram of the structure of the outer sleeve.

[0040] Figure 6 This is a physical picture of the bimetallic composite pipe and the supporting core device before welding. Figure 6 Middle: A is a physical picture of the support core device of the bimetallic composite pipe, and B is a physical picture of the bimetallic composite pipe equipped with the support core device.

[0041] Figure 7 This is a physical picture of the bimetallic composite pipe after welding. Figure 7 Middle: A and B are the appearance pictures of the bimetallic composite pipe with the support core device after welding, and C is the internal picture of the bimetallic composite pipe with the support core device removed after welding.

[0042] Figure 8 This is a physical picture of the bimetallic composite pipe after welding without using a supporting core.

[0043] Fig. 9 This is a physical picture of the bimetallic composite pipe after welding using alloy rods as the supporting core.

[0044] The meanings of the numbers in the figure are: 1-outer sleeve, 2-left propulsion rod, 3-right propulsion rod, 4-limiting screw, 5-driving nut, 6-thickened washer.

[0045] 101 - left outer conical cavity, 102 - left main body cavity, 103 - left inner conical cavity, 104 - middle transition cavity, 105 - right inner conical cavity, 106 - right main body cavity, 107 - right outer conical cavity.

[0046] 201 - outer section of the left propulsion rod, 202 - middle section of the left propulsion rod, 203 - inner section of the left propulsion rod.

[0047] 301 - outer section of the right propulsion rod, 302 - middle section of the right propulsion rod, 303 - inner section of the right propulsion rod.

[0048] The technical solution of the present invention is further described below in conjunction with embodiments. DETAILED DESCRIPTION

[0049] The working principle of the present invention is as follows Figure 5 As shown in the figure: when point B on the end face of the push rod is pushed axially to point B', the moving distance of the push rod in the axial direction is x, and after point A on the inner wall cone inclined surface of the corresponding outer sleeve 1 rises to point A', the support radius of the support core increases by an increment of △Y. When the two push rods continue to be tightened axially, the outer sleeve 1 can continue to increase in diameter as needed, and △Y is numerically equal to the distance from a fixed point A on the inclined surface to A' when the inclined surface moves.

[0050] It should be noted that all components used in the present invention, unless otherwise specified, are components known in the art.

[0051] In accordance with the above technical scheme, specific embodiments of the present invention are given below. It should be noted that the present invention is not limited to the following specific embodiments, and all equivalent changes made on the basis of the technical scheme of this application fall within the protection scope of the present invention.

[0052] Embodiment 1:

[0053] This embodiment provides a support core device for a bimetallic composite tube, such as Figure 1 and Figure 2 As shown, it includes an outer sleeve 1, in which a pair of left propulsion rods 2 and right propulsion rods 3 are movably arranged, and a limiting screw 4 is arranged in the left propulsion rod 2 and the right propulsion rod 3. The axial ends of the limiting screw 4 respectively extend out of the axial ends of the outer sleeve 1, and a driving nut 5 is detachably installed on the axial ends of the limiting screw 4.

[0054] like Figure 3As shown, the left propulsion rod 2 and the right propulsion rod 3 have the same shape and are arranged relatively to each other; the left propulsion rod 2 comprises, from left to right, a left propulsion rod outer section 201, a left propulsion rod middle section 202 and a left propulsion rod inner section 203; the right propulsion rod 3 comprises, from right to left, a right propulsion rod outer section 301, a right propulsion rod middle section 302 and a right propulsion rod inner section 303.

[0055] As a specific solution of this embodiment, the left thrust rod 2, the right thrust rod 3 and the two drive nuts 5 can move along the axial direction on the limit screw 4, and the moving distances of the left thrust rod 2 and the right thrust rod 3 in the axial direction are equal; as the left thrust rod 2 and the right thrust rod 3 move in the axial direction, the outer radius of the outer sleeve 1 also changes accordingly.

[0056] like Figure 4 As shown, the relationship between the moving distance of the left propulsion rod 2 in the axial direction and the change in the outer radius of the outer sleeve is shown in the following formula I:

[0057]

[0058] Where:

[0059] ΔY represents the change in the outer radius of the outer sleeve, in mm.

[0060] α represents the taper of the inner section of the left propulsion rod, and the unit is °; the taper of the inner section of the left propulsion rod is equal to the taper of the inner section of the right propulsion rod, the taper of the left inner conical cavity, and the taper of the right inner conical cavity.

[0061] l represents the advancement distance in mm.

[0062] x represents the moving distance of the left propulsion rod in the axial direction (equal to the moving distance of the right propulsion rod in the axial direction), in mm.

[0063] In this embodiment, before the device is used, the drive nut 5 is located in an outer position, and the left propulsion rod 2 and the right propulsion rod 3 are also located in an outer position. When the device is in use, by tightening the drive nut 5, the drive nut 5 can move along the axial direction on the limit screw 4. When the drive nut 5 contacts the left propulsion rod 2 and the right propulsion rod 3, the drive nut 5 can push the left propulsion rod 2 and the right propulsion rod 3 to move from the outside to the inside in the outer sleeve 1, and the function of pushing the propulsion rod is realized by the drive nut 5.

[0064] In this embodiment, the outer sleeve 1, the left propulsion rod 2 and the right propulsion rod 3 are all made of 45# steel. 45# steel has high yield strength and tensile strength, which can fully meet the needs. In addition, it is easy to process and has high cost performance.

[0065] In this embodiment, the limiting screw 4 and the driving nut 5 are both made of alloy steel with a strength of 12.9 grade, so as to effectively improve the strength of the overall supporting core device.

[0066] As a specific solution of this embodiment, Figure 1 and Figure 2 As shown, a thickened washer 6 is respectively installed on both axial ends of the limiting screw 4 , and the thickened washer 6 is located on the inner side of the driving nut 5 .

[0067] As a specific solution of this embodiment, Figure 5 As shown, the outer sleeve 1 is a hollow cylindrical structure, and the cavities in the outer sleeve 1 are, from left to right, a left outer conical cavity 101, a left main body cavity 102, a left inner conical cavity 103, an intermediate transition cavity 104, a right inner conical cavity 105, a right main body cavity 106 and a right outer conical cavity 107; the left inner conical cavity 103 and the right inner conical cavity 105 are exactly the same in shape and are symmetrically arranged, the left main body cavity 102 and the right main body cavity 106 are exactly the same in shape and are symmetrically arranged, and the left outer conical cavity 101 and the right outer conical cavity 107 are exactly the same in shape and are symmetrically arranged.

[0068] In this embodiment, Figure 1 , Figure 2 and Figure 5 As shown, the outer surface of the outer sleeve 1 is a cylindrical structure, and the inner surface is a stepped concave structure. The cavity inside the outer sleeve 1 matches the shape of the push rod.

[0069] In this embodiment, the bimetallic composite pipe to be processed is a steel-aluminum composite pipe, the inner diameter of the bimetallic composite pipe is 92 mm, the outer diameter of the bimetallic composite pipe is 108 mm, the length of the bimetallic composite pipe is 600 mm, the wall thickness of the inner aluminum alloy layer of the bimetallic composite pipe is 5 mm, and the wall thickness of the outer steel cladding of the bimetallic composite pipe is 3 mm.

[0070] As a specific solution of this embodiment, Figure 1 As shown, the distance L0 between the axial outer ends of the left propulsion rod 2 and the right propulsion rod 3 needs to be greater than the length of the bimetallic composite tube, and L0 is 1100 mm; the length L of the outer sleeve needs to be greater than the length of the bimetallic composite tube and less than the distance L0 between the axial outer ends of the left propulsion rod 2 and the right propulsion rod 3, and L is 1000 mm.

[0071] As a specific solution of this embodiment, Figure 1 As shown, the length of the limiting screw 4 needs to be greater than the distance L0 between the axial outer ends of the left propulsion rod 2 and the right propulsion rod 3, which is 1200 mm. The outer diameter of the limiting screw 4 and the inner diameter of the driving nut 5 are 22 mm.

[0072] As a specific solution of this embodiment, Figure 1 and Figure 3 As shown, the length L1 of the left propulsion rod 2 and the right propulsion rod 3 is 468 mm, and the outer diameter D1 of the left propulsion rod middle section 202 and the right propulsion rod middle section 302 is 50 mm. The above design can effectively ensure the strength of the supporting core device.

[0073] As a specific solution of this embodiment, Figure 5 As shown, the thinnest wall thickness h of the outer sleeve 1 is 20 mm to ensure an effective movement gap between the left propulsion rod 2 and the right propulsion rod 3 and the outer sleeve 1.

[0074] As a specific solution of this embodiment, Figure 4 As shown, the taper α of the inner section of the left propulsion rod is 9°. In this embodiment, the value of the taper α of the inner section of the left propulsion rod needs to be determined based on experiments. After experimental verification, when the taper of the inner section of the propulsion rod and the taper of the inner conical cavity are 9°, the change in the outer diameter of the outer sleeve 1 with the axial movement of the propulsion rod is the largest, and at this inclination, the cone propulsion rod will not adhere to the conical surface of the outer sleeve 1 due to the explosion shock wave, and at the same time, the maximum support force of the propulsion rod on the outer sleeve 1 can be guaranteed.

[0075] As a specific solution of this embodiment, Figure 4 As shown, the initial distance between the axial right end face of the left propulsion rod 2 and the midpoint of the outer sleeve 1 is the propulsion distance l, and the initial distance between the axial left end face of the right propulsion rod 3 and the midpoint of the outer sleeve 1 is the propulsion distance l. In this embodiment, after machining according to the taper α of 9°, the propulsion distance l is machined to 45mm. 45mm is determined according to the effective distance designed based on the intermediate reserved size of the taper α of 9°.

[0076] As a specific solution of this embodiment, the minimum outer diameter of the outer sleeve is 89 mm, the maximum supporting outer diameter of the outer sleeve is equal to the inner diameter of the bimetallic composite tube, that is, 92 mm, and the change ΔY of the outer radius of the outer sleeve is equal to 1.5 mm.

[0077] Embodiment 2:

[0078] This embodiment provides a preparation process of a bimetallic composite tube based on an external explosion method, and the process adopts the support core device of the bimetallic composite tube in Example 1. The process specifically includes the following steps:

[0079] Step 1: According to the change in the outer radius of the outer sleeve 1, the taper of the inner section 203 of the left propulsion rod, and the propulsion distance, the moving distance of the left propulsion rod 2 and the right propulsion rod 3 in the axial direction is calculated and obtained using Formula I; Formula I is:

[0080]

[0081] Where:

[0082] ΔY represents the change in the outer radius of the outer sleeve, in mm; ΔY is equal to the difference between the inner diameter of the bimetallic composite tube and the minimum outer diameter of the outer sleeve.

[0083] α represents the taper of the inner section of the left propulsion rod, in degrees.

[0084] l represents the advancement distance in mm.

[0085] x represents the moving distance of the left propulsion rod in the axial direction, and the moving distance of the right propulsion rod in the axial direction is equal to it, and the unit is mm.

[0086] In this embodiment, the taper α (9°) of the inner section of the left push rod, the change in the outer radius of the outer sleeve ΔY (1.5 mm) and the push distance l (45 mm) of the embodiment 1 are substituted into formula I, and the moving distance x of the push rod in the axial direction is calculated and obtained to be 16 mm. That is, starting from 45 mm, after the left push rod 2 and the right push rod 3 are moved 16 mm in the axial direction, the outer diameter of the outer sleeve 1 is expanded from 89 mm to 92 mm, which can effectively meet the support size requirements of the bimetallic composite pipe.

[0087] Step 2: Device installation: Figure 6 As shown, prepare the bimetallic composite tube to be processed, insert the supporting core device into the bimetallic composite tube, and push the left propulsion rod 2 and the right propulsion rod 3 into the outer sleeve 1 by tightening the driving nut 5. When the moving distance of the left propulsion rod 2 and the right propulsion rod 3 in the axial direction reaches 16 mm, the outer diameter of the outer sleeve 1 increases from 89 mm to 92 mm, and the advancement is stopped.

[0088] Step three, perform explosion welding: During explosion welding, the explosives instantly generate high pressure of more than 700MPa, high temperature of more than 3000℃ and high-speed shock wave of 500-1000m / s.

[0089] Step 4, taking out the device: After the explosion welding is completed, wait until the temperature of the bimetallic composite pipe drops, loosen the drive nut 5, and then pull the left push rod 2 and the right push rod 3 out of the outer sleeve 1. After the outer diameter of the outer sleeve 1 becomes smaller, take out the support core device.

[0090] In this embodiment, the final welding result is as follows: Figure 7 As shown. Figure 7 It can be seen that the use of the support core device of the present invention for explosive welding can effectively resist the explosive impact force generated during explosive welding and composite bonding, while also ensuring that the support core device can be removed after welding is completed, fully meeting the requirements of the explosive composite process.

[0091] Comparative Example 1:

[0092] This comparative example provides a preparation process of a bimetallic composite pipe based on an external explosion method. The process does not use any supporting device and directly performs explosion welding on the bimetallic composite pipe to be processed. The temperature, pressure and shock wave velocity of the explosion welding are exactly the same as those in step three of Example 2.

[0093] In this comparative example, the final welding result is as follows Figure 8 As shown. Figure 8 It can be seen that in the explosive welding composite process without a supporting core device, the impact force of the explosion wave causes severe deformation and serious damage to the covering pipe and the base pipe.

[0094] Comparative Example 2:

[0095] This comparative example provides a preparation process of a bimetallic composite tube based on an external explosion method, which includes: preparing a bimetallic composite tube to be processed, inserting an alloy rod into the bimetallic composite tube as a support core, and then performing explosion welding. The temperature, pressure and shock wave velocity of the explosion welding are exactly the same as those in step three of Example 2.

[0096] In this comparative example, the final welding result is as follows Fig. 9 As shown. Fig. 9 It can be seen that when alloy rods are used for support, the overall shrinkage and deformation of the composite tube causes interference fit between the support rods and the base tube and makes them unable to be removed, so the bimetallic composite tube cannot be used.

Claims

1. A preparation process of a bimetallic composite pipe, It is characterized in that This process uses a supporting core device for the bimetallic composite pipe to realize the explosive welding composite of the bimetallic composite pipe; The supporting core device of the bimetallic composite pipe comprises an outer sleeve (1), a pair of left propulsion rods (2) and right propulsion rods (3) are movably arranged in the outer sleeve (1), a limiting screw (4) is arranged in the left propulsion rod (2) and the right propulsion rod (3), the axial ends of the limiting screw (4) respectively extend out of the axial ends of the outer sleeve (1), and a driving nut (5) is detachably mounted on the axial ends of the limiting screw (4); The left propulsion rod (2) and the right propulsion rod (3) have the same shape and are arranged opposite to each other; the left propulsion rod (2) comprises, from left to right, a left propulsion rod outer section (201), a left propulsion rod middle section (202) and a left propulsion rod inner section (203); the right propulsion rod (3) comprises, from right to left, a right propulsion rod outer section (301), a right propulsion rod middle section (302) and a right propulsion rod inner section (303); The left propulsion rod (2), the right propulsion rod (3) and the two driving nuts (5) can move along the axial direction on the limiting screw (4), and the moving distances of the left propulsion rod (2) and the right propulsion rod (3) in the axial direction are equal; as the left propulsion rod (2) and the right propulsion rod (3) move in the axial direction, the outer radius of the outer sleeve (1) also changes accordingly; The process specifically includes the following steps: Step 1: Based on the change in the outer radius of the outer sleeve (1), the taper of the inner section (203) of the left propulsion rod, and the propulsion distance, the movement distance x of the left propulsion rod (2) and the right propulsion rod (3) in the axial direction is calculated and obtained using Formula I; the Formula I is: Where: ΔY represents the change in the outer radius of the outer sleeve, in mm; ΔY is equal to the difference between the inner diameter of the bimetallic composite tube and the minimum outer diameter of the outer sleeve; α represents the taper of the inner section of the left propulsion rod, in degrees; l represents the propulsion distance, which means that the initial distance between the axial right end surface of the left propulsion rod (2) and the midpoint of the outer sleeve (1) is the propulsion distance or the initial distance between the axial left end surface of the right propulsion rod (3) and the midpoint of the outer sleeve (1), in mm; x represents the moving distance of the left propulsion rod in the axial direction, and the moving distance of the right propulsion rod in the axial direction is equal to it, in mm; Step 2, device installation: prepare the bimetallic composite tube to be processed, insert the support core device of the bimetallic composite tube into the bimetallic composite tube, and push the left push rod (2) and the right push rod (3) into the outer sleeve (1) by tightening the driving nut (5). When the moving distance of the left push rod (2) and the right push rod (3) in the axial direction reaches x, the outer diameter of the outer sleeve (1) is equal to the inner diameter of the bimetallic composite tube, and the pushing is stopped; Step three, performing explosion welding; Step 4, removing the device: After the explosion welding is completed, when the temperature of the bimetallic composite pipe drops, loosen the drive nut (5), and then pull the left push rod (2) and the right push rod (3) out of the outer sleeve (1). After the outer diameter of the outer sleeve (1) becomes smaller, remove the support core device of the bimetallic composite pipe.

2. The preparation process of the bimetallic composite pipe according to claim 1, It is characterized in that The cavities in the outer sleeve (1) are, from left to right, a left outer conical cavity (101), a left main body cavity (102), a left inner conical cavity (103), an intermediate transition cavity (104), a right inner conical cavity (105), a right main body cavity (106) and a right outer conical cavity (107); the shapes of the left inner conical cavity (103) and the right inner conical cavity (105) are completely identical and symmetrically arranged, the shapes of the left main body cavity (102) and the right main body cavity (106) are completely identical and symmetrically arranged, and the shapes of the left outer conical cavity (101) and the right outer conical cavity (107) are completely identical and symmetrically arranged.

3. The preparation process of the bimetallic composite pipe according to claim 1, It is characterized in that The inner diameter of the bimetallic composite pipe to be processed is 92 mm, and the length of the bimetallic composite pipe to be processed is 600 mm.

4. The process for preparing the bimetallic composite pipe according to claim 3, It is characterized in that The taper α of the inner section of the left propulsion rod is 9°; the propulsion distance l is 45 mm; and the minimum outer diameter of the outer sleeve is 89 mm.

5. The preparation process of the bimetallic composite pipe according to claim 3, It is characterized in that The distance L between the axial outer ends of the left propulsion rod (2) and the right propulsion rod (3) is 0 is 1100mm; the length L of the outer sleeve (1) is 1000mm; the length of the limiting screw (4) is 1200mm.

6. The process for preparing the bimetallic composite pipe according to claim 3, It is characterized in that The length L of the left propulsion rod (2) and the right propulsion rod (3) is 1 The outer diameter D of the left propulsion rod middle section (202) and the right propulsion rod middle section (302) is 468 mm. 1 is 50mm.

7. The process for preparing the bimetallic composite pipe according to claim 3, It is characterized in that The thinnest wall thickness h of the outer sleeve (1) is 20 mm.

8. The process for preparing the bimetallic composite pipe according to claim 1, It is characterized in that A thickened washer (6) is respectively installed on both axial ends of the limiting screw (4), and the thickened washer (6) is located on the inner side of the driving nut (5).

9. The process for preparing the bimetallic composite pipe according to claim 1, It is characterized in that In step three, the instantaneous pressure of the explosion welding is greater than or equal to 700 MPa, the instantaneous temperature is greater than or equal to 3000° C., and the speed of the shock wave generated by the explosion welding is 500-1000 m / s.

10. A bimetallic composite pipe support core device, the device is used to support the bimetallic composite pipe to be processed, It is characterized in that The invention comprises an outer sleeve (1), wherein a pair of left propulsion rods (2) and right propulsion rods (3) are movably arranged in the outer sleeve (1), and a limiting screw rod (4) is arranged in the left propulsion rod (2) and the right propulsion rod (3), and the axial ends of the limiting screw rod (4) respectively extend out of the axial ends of the outer sleeve (1), and a driving nut (5) is detachably mounted on the axial ends of the limiting screw rod (4); The left propulsion rod (2) and the right propulsion rod (3) have the same shape and are arranged opposite to each other; the left propulsion rod (2) comprises, from left to right, a left propulsion rod outer section (201), a left propulsion rod middle section (202) and a left propulsion rod inner section (203); the right propulsion rod (3) comprises, from right to left, a right propulsion rod outer section (301), a right propulsion rod middle section (302) and a right propulsion rod inner section (303); The left propulsion rod (2), the right propulsion rod (3) and the two driving nuts (5) can move along the axial direction on the limiting screw (4), and the moving distances of the left propulsion rod (2) and the right propulsion rod (3) in the axial direction are equal; as the left propulsion rod (2) and the right propulsion rod (3) move in the axial direction, the outer radius of the outer sleeve (1) also changes accordingly; The cavities in the outer sleeve (1) are, from left to right, a left outer conical cavity (101), a left main cavity (102), a left inner conical cavity (103), an intermediate transition cavity (104), a right inner conical cavity (105), a right main cavity (106) and a right outer conical cavity (107); the shapes of the left inner conical cavity (103) and the right inner conical cavity (105) are completely identical and symmetrically arranged, the shapes of the left main cavity (102) and the right main cavity (106) are completely identical and symmetrically arranged, and the shapes of the left outer conical cavity (101) and the right outer conical cavity (107) are completely identical and symmetrically arranged; The inner diameter of the bimetallic composite pipe to be processed is 92 mm, and the length of the bimetallic composite pipe to be processed is 600 mm; The taper α of the inner section of the left propulsion rod is 9°; the propulsion distance l is 45 mm; the minimum outer diameter of the outer sleeve is 89 mm; The distance L between the axial outer ends of the left propulsion rod (2) and the right propulsion rod (3) is 0 1100mm; The length L of the outer sleeve (1) is 1000 mm; the length of the limiting screw (4) is 1200 mm; The length L of the left propulsion rod (2) and the right propulsion rod (3) is 1 The outer diameter D of the left propulsion rod middle section (202) and the right propulsion rod middle section (302) is 468 mm. 1 50mm; The thinnest wall thickness h of the outer sleeve (1) is 20 mm; A thickened washer (6) is respectively installed on both axial ends of the limiting screw (4), and the thickened washer (6) is located on the inner side of the driving nut (5).