Annular part multi-plate tailor-welding process with high standard form and location tolerance

By defining the reference and subsequent welding edges in the multi-plate ring-shaped component assembly welding process, laser blanking and step-by-step welding are carried out to correct welding deviations, and the ring-shaped component with high standard shape and position tolerance is achieved, and the welding stress is solved The resulting dimensional deviation and change of positioning holes improve product quality and production efficiency.

CN118989575AActive Publication Date: 2024-11-22WUHAN NINGZHIYUAN AUTO PARTS CO LTD +1

Patent Information

Application Number
CN202410799742.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-11-22
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

In the existing multi-plate ring-shaped parts welding process, the weld size deviation and positioning hole position change due to the unevenness of welding stress, affecting product quality and the accuracy and efficiency of subsequent hot stamping and 3D laser cutting.

Method used

Adopt a multi-plate welding process for ring-shaped parts with high standard position tolerance. By defining the reference welding edge and subsequent welding edge, laser blanking and step-by-step welding are carried out, and the cutting head is used to correct the dimensional deviation during the welding process to ensure that The original blanking shape of each sheet is the same as the final product shape, and is accurately processed by laser cutting to achieve a shape and position tolerance of ≤±1mm.

Benefits of technology

The ultimate consistency of product shape and position tolerance is achieved, and the risk of material flow control and positioning hole position deviation in hot stamping and 3D laser cutting is reduced, production efficiency and material utilization are improved, and costs are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989575A_ABST
    Figure CN118989575A_ABST
Patent Text Reader

Abstract

The invention provides an annular part multi-plate tailor-welding process with high standard form and location tolerance, the high standard form and location tolerance is smaller than or equal to + / -1 mm, the number of plates in multi-plate tailor-welding is larger than or equal to 3, and the annular part multi-plate tailor-welding process comprises the following steps that a reference welding edge in each plate serves as a reference, according to the appearance of a final product, the original blanking appearance is determined, and laser blanking is conducted; step-by-step tailor-welding is carried out, after the reference welding edges of the two adjacent plates are aligned, welding is carried out, and a double-spliced plate is obtained after welding is completed; then subsequent welding edges on the double-jointed board are corrected to eliminate dimensional deviation, meanwhile, welding stress is released, finally, laser cutting is conducted on the annular blank piece, and the annular piece with the high standard form and location tolerance is obtained. According to the method, various risks of an existing conventional process can be completely avoided, the complete consistency and the high comprehensive yield are achieved, the quality and cost are optimal, and the technology upgrading of subsequent 3D machining of the thermal forming part can be effectively matched and reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention provides a multi-plate welding process for annular parts with high standard form and position tolerances, and belongs to the technical field of laser processing. Background Art

[0002] Laser welding uses laser energy to automatically join and weld several steels, stainless steels, aluminum alloys, etc. of different materials, thicknesses, and coatings to form an integral plate, profile, sandwich panel, etc., to meet the different material performance requirements of parts and components, and to achieve lightweight equipment with the lightest weight, optimal structure, and best performance. At present, laser welded plates are mainly used in the car body of the automobile manufacturing industry. Door rings (commonly known as automobile door frames) have various product forms, ranging from 2 steel plates welded to 6 steel plates welded, and each piece of raw material has a different appearance.

[0003] The following process is generally used for the welding of multi-plate annular parts: First, the die blanking / laser blanking is used, and after blanking, the precise shape of each plate is obtained, including the positioning holes. Then a special fixture is used for welding (the positioning holes can be used for welding positioning, and the fixture clamps and positions each plate as a whole). During the welding process of the above process, due to the different welding processes, the influence of welding stress is very large, resulting in 3-8 or even 10mm uneven edges of the plate after the final welding (commonly known as misalignment). The welding stress after each weld will cause dimensional deviation (or cumulative unevenness of the weld). Because multiple welds are accumulated in sequence, the unwelded seams will be inconsistent. The cumulative consequence is weld failure (weld defects due to poor welding) or large accumulated tolerances leading to dimensional failure or workpiece deformation, affecting the quality of the product. The annular plate after welding needs to be hot stamped later. Due to the existence of misalignment, the consistency of the plate is affected, resulting in the risk of material fluidity control at various locations during the hot stamping process of different misaligned plates; at the same time, the stress release of the weld after welding will cause the relative position of the positioning hole to change, and the relative position change of the positioning hole will further cause the hot stamping charging deviation or even failure, affecting the continuity of stamping. After hot stamping, the contour of the workpiece needs to be cut by 3D laser. 3D laser cutting is currently the most important process in the entire production process and is expensive. When the above-mentioned plates with misalignment are 3D laser cut after hot stamping, the misalignment and the deviation of the positioning hole position will lead to inconsistent cutting amount, which may further lead to 3D cutting risks (including production pauses, cutting head operation failures, etc.). More importantly, after hot stamping, the workpieces with misalignment and positioning hole position deviation cannot support the subsequent requirements for higher production efficiency of reducing 3D cutting amount (less cutting, no cutting, partial cutting, etc.) in the 3D laser cutting link. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention provides a multi-plate welding process for annular parts with high-standard form and position tolerances. This process can achieve the ultimate form and position tolerance of the product of ≤±1mm, and can completely avoid the various risks of the aforementioned conventional processes, achieve complete consistency and a high comprehensive yield rate, achieve the best quality and cost, and can effectively cooperate with the technical upgrade to reduce the subsequent 3D processing of hot-formed parts.

[0005] The technical solution adopted to achieve the above-mentioned purpose of the present invention is:

[0006] A multi-plate tailor-welding process for an annular part with a high standard shape and position tolerance, wherein the high standard shape and position tolerance is ≤±1 mm, and the number of plates in the multi-plate tailor-welding is ≥3, comprising the following steps:

[0007] (1) The first welded edge of each sheet is defined as the reference welded edge according to the welding sequence, and the subsequently welded edge is defined as the subsequent welded edge; the reference welded edge of each sheet is used as the reference, and the original blanking shape of each sheet is determined according to the shape of each sheet in the final product of the annular part, wherein, in the original blanking shape, except for the reference welded edge, the remaining contour edges and the subsequent welded edges are set with cutting allowances based on the shape of the sheet in the final product;

[0008] (2) Laser blanking is performed according to the original blanking shape of each sheet;

[0009] (3) Perform step-by-step welding, first align the reference welding edges of the two adjacent sheets, fix them with a clamp, and then weld them. After welding, a double-jointed plate is obtained; if the total number of sheets is an odd number, the extra sheet is not welded first;

[0010] (4) Before welding the double panels together, or before welding the double panels to a single sheet, a cutting head is used to correct the subsequent welding edges on the double panels to eliminate the dimensional deviation caused by the previous welding process, and at the same time, the original welding stress is released. After correction, the double panels are fixed on a fixture and then welded. After welding, a multi-panel or annular blank is obtained; this step is repeated for the multi-panel until the final annular blank is formed;

[0011] (5) The annular blank is laser cut to precisely cut and process its inner and outer contours and positioning holes to obtain an annular part with high standard geometric tolerances.

[0012] Furthermore, the shape and position tolerance of the annular part with high standard shape and position tolerance is ≤±0.5mm, and there is no misalignment in the welding position of the annular part, which fully meets the requirements of the product design contour line.

[0013] Furthermore, the width of the cutting margin set in step (1) is greater than 1 to 10 mm.

[0014] Furthermore, in step (2), if the subsequent welding process is laser wire welding, edge gaps are prefabricated at the reference welding edge and the subsequent welding edge while laser blanking.

[0015] Furthermore, the welding in steps (3) and (4) is performed by filler wire welding or laser welding.

[0016] Furthermore, the annular part with high standard geometric tolerance obtained in step (5) can be finally manufactured into a finished product after subsequent hot stamping and three-dimensional laser cutting.

[0017] The present invention also provides a ring-shaped part with high standard shape and position tolerance, which is manufactured by adopting the above-mentioned multi-plate welding process.

[0018] Compared with the prior art, the present application has the following advantages: (1) The ring-shaped parts with high standard geometric tolerances prepared by the process of the present application are basically consistent with the design CAD drawing, and can achieve precise positioning and precise control of material flow in the subsequent hot stamping process, ensuring the process consistency between the stamping results and the design target. Compared with the stamping blanks with missing or excessive materials on the inner and outer edges produced without this special process, the uncontrollable and consistency deviation of the edge materials during the stamping process can reduce the wrinkling and material shortage caused by the unexpected flow of materials and quality hazards; (2) The geometric tolerances of each positioning hole and the blank shape can be accurately controlled, and the edge position and accuracy of the stamping parts can be accurately controlled, which can greatly reduce the trimming amount design of the stamping parts, optimize the blank shearing and blanking sample distribution in advance, greatly improve the material utilization rate, save material consumption, and realize partial trimming or even no trimming drawing; especially for the parts after hot stamping, the processing amount of the subsequent three-dimensional laser cutting part contour can be reduced, the processing bottleneck can be reduced, and the production efficiency of hot-formed parts can be greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a CAD design drawing of the annular member provided in Example 1;

[0020] Figure 2 The final shape of sheet A in Example 1 and the original blanking shape diagram;

[0021] Figure 3 The final shape of sheet B in Example 1 and the original blanking shape diagram;

[0022] Figure 4 The final shape of sheet C in Example 1 and the original blanking shape diagram;

[0023] Figure 5 The final shape of sheet D in Example 1 and the original blanking shape diagram;

[0024] Figure 6 This is the appearance diagram of the double-jointed board AD in Example 1;

[0025] Figure 7 This is the appearance diagram of the double-jointed board BC in Example 1;

[0026] Figure 8 The figure is an outline diagram and a cutting diagram of the annular blank in Example 1;

[0027] Fig. 9 This is the CAD design drawing of the annular part provided in Example 2. DETAILED DESCRIPTION

[0028] The present application is described in detail below with reference to the accompanying drawings and specific embodiments.

[0029] Example 1

[0030] The CAD design drawing of the automobile body annular part to be prepared in this embodiment is as follows: Figure 1 As shown, it is required to be welded from 4 different sheets, namely sheets A / B / C / D.

[0031] According to the welding sequence, the first welded edge in each sheet is defined as the reference welded edge, and the subsequent welded edge is defined as the subsequent welded edge; each sheet A / B / C / D has a reference welded edge. Taking the reference welded edge in each sheet as the reference, the original blanking shape of each sheet is determined according to the shape of each sheet in the final product of the annular part. In the original blanking shape, except for the reference welded edge, the remaining contour edges and subsequent welded edges are set with cutting allowances based on the shape of the sheet in the final product; the original blanking shape drawings of sheets A / B / C / D are as follows: Figure 2-5 As shown in the above figure, the single solid line edge represents the reference welding edge, and the double solid line represents the cutting allowance. Generally speaking, the width of the cutting allowance is greater than 1 to 10 mm.

[0032] Laser blanking is performed according to the original blanking shape of each sheet; if the subsequent welding process is laser wire welding, the edge gap is prefabricated at the reference welding edge and the subsequent welding edge while laser blanking.

[0033] Then, the step-by-step welding is performed. First, the reference welding edges of the two adjacent plates are aligned, fixed with a clamp, and then welding is performed. The welding is specifically performed by wire welding or laser welding. After welding, a double-jointed plate is obtained; after welding, the double-jointed plate AD and the double-jointed plate BC are as follows Figure 6 and Figure 7 As shown, the double panels AD and BC are pre-jointed, and the subsequent welding edges on the double panels are corrected using a cutting head to eliminate the dimensional deviation caused by the previous welding process. Figure 6and Figure 7 The double solid lines in the figure indicate the subsequent welding edges that need to be corrected. After the correction is completed, it is fixed on the fixture and then welded. After the welding is completed, a ring-shaped blank is obtained, such as Figure 8 As shown in the figure, the annular blank is laser cut to precisely cut its inner and outer contours and positioning holes. Figure 8 The thick solid line in the figure is the outer contour of the annular blank, and the thin solid line is the cutting line and the cutting line of the positioning hole. After cutting, a ring part with high standard shape and position tolerance is obtained, and its shape and position tolerance is ≤±0.5mm.

[0034] Example 2

[0035] The CAD design drawing of the automobile body annular part to be prepared in this embodiment is as follows: Fig. 9 As shown, it is required to be welded from 5 different sheets, namely sheets A / B / C / D / E.

[0036] According to the welding sequence, the first welded edge in each sheet is defined as the reference welded edge, and the subsequent welded edge is defined as the subsequent welded edge; each sheet A / B / C / D / E has a reference welded edge. Taking the reference welded edge in each sheet as the reference, the original blanking shape of each sheet is determined according to the shape of each sheet in the final product of the annular part. In the original blanking shape, except for the reference welded edge, the remaining contour edges and subsequent welded edges are set with cutting allowances based on the shape of the sheet in the final product. Generally speaking, the width of the cutting allowance is greater than 1 to 10 mm.

[0037] Laser blanking is performed according to the original blanking shape of each sheet; if the subsequent welding process is laser wire welding, the edge gap is prefabricated at the reference welding edge and the subsequent welding edge while laser blanking.

[0038] Then, step-by-step welding is performed. First, the reference welding edges of the two adjacent plates are aligned, fixed with a fixture, and then welding is performed. The welding is specifically performed by wire welding or laser welding. After welding, a double panel is obtained; in this embodiment, the double panel CD and the double panel AB are welded first, and the plate E is not welded first; then the double panel AB and the plate E are pre-jointed, and the subsequent welding edges on the double panel AB are corrected by a cutting head to eliminate the dimensional deviation caused by the previous welding process. After the correction is completed, it is fixed on the fixture and then welded. After welding, a multi-panel ABE is obtained.

[0039] Finally, the double panel CD and the multi-panel ABE are pre-jointed, and the cutting head is used to correct the subsequent welding edges on the double panel CD and the multi-panel ABE to eliminate the dimensional deviation caused by the previous welding process. After the correction is completed, they are fixed on the fixture and then welded. After the welding is completed, an annular blank is obtained. The annular blank is laser cut, and its inner and outer contours and positioning holes are accurately cut and processed. After cutting, the following is obtained Fig. 9 The ring parts with high standard geometric tolerance shown have a geometric tolerance of ≤±0.5mm.

[0040] The ring-shaped parts with high standard geometric tolerances obtained in Examples 1 and 2 of the present invention can be made into final products after subsequent hot stamping and three-dimensional laser cutting. This process can adapt to the continuous improvement of subsequent product designs, partially reduce or even completely eliminate the subsequent 3D laser contour cutting process after hot stamping, greatly improve production efficiency, reduce investment in 3D cutting equipment, and reduce manufacturing costs.

Claims

1. A process for welding multiple plates of annular parts with high standard shape and position tolerance, wherein the high standard shape and position tolerance is ≤±1mm, and the number of plates in the welding multiple plates is ≥3, characterized in that The following steps are involved: (1) The first welded edge of each sheet is defined as the reference welded edge according to the welding sequence, and the subsequently welded edge is defined as the subsequent welded edge; the reference welded edge of each sheet is used as the reference, and the original blanking shape of each sheet is determined according to the shape of each sheet in the final product of the annular part, wherein, in the original blanking shape, except for the reference welded edge, the remaining contour edges and the subsequent welded edges are set with cutting allowances based on the shape of the sheet in the final product; (2) Laser blanking is performed according to the original blanking shape of each sheet; (3) Perform step-by-step welding, first align the reference welding edges of the two adjacent sheets, fix them with a clamp, and then weld them. After welding, a double-jointed plate is obtained; if the total number of sheets is an odd number, the extra sheet is not welded first; (4) Before welding the double panels together, or before welding the double panels to a single sheet, a cutting head is used to correct the subsequent welding edges on the double panels to eliminate the dimensional deviation caused by the previous welding process, and at the same time, the original welding stress is released. After correction, the double panels are fixed on a fixture and then welded. After welding, a multi-panel or annular blank is obtained; this step is repeated for the multi-panel until the final annular blank is formed; (5) The annular blank is laser cut to precisely cut and process its inner and outer contours and positioning holes to obtain an annular part with high standard geometric tolerances.

2. The multi-plate tailor-made welding process for annular parts with high standard geometric tolerances according to claim 1 is characterized in that: The shape and position tolerance of the annular part with high standard shape and position tolerance is ≤±0.5mm, and there is no misalignment in the welding position of the annular part, which fully meets the requirements of the product design contour line.

3. The multi-plate tailor-made welding process for annular parts with high standard geometric tolerances according to claim 1 is characterized in that: The width of the cutting margin set in step (1) is greater than 1 to 10 mm.

4. The multi-plate tailor-made welding process for annular parts with high standard geometric tolerances according to claim 1 is characterized in that: In step (2), if the subsequent welding process is laser wire welding, edge gaps are prefabricated at the reference welding edge and the subsequent welding edge while laser blanking is taking place.

5. The multi-plate tailor-made welding process for annular parts with high standard geometric tolerances according to claim 1 is characterized in that: The welding in steps (3) and (4) is specifically performed by filler wire welding or laser welding.

6. The multi-plate tailor-made welding process for annular parts with high standard geometric tolerances according to claim 1 is characterized in that: The annular part with high standard geometric tolerance obtained in step (5) can be finally manufactured into a finished product after subsequent hot stamping and three-dimensional laser cutting.

7. An annular part with high standard geometric tolerances, manufactured by the multi-plate welding process described in claim 1.

Citation Information

Patent Citations

  • Method for controlling tailor welding deformation of large metal pipe plate

    CN104148773A

  • Multi-plate splicing welding tooling

    CN106541240A

  • System and method for processing automobile door-ring tailor-welded plate blanks

    CN110102888A

  • Tailor welding process of light conduction box

    CN115805372A

  • Flexible displacement clamp and tailor-welding process based on same

    CN116787053A

Cited By

  • Blank manufacturing method

    JP7808758B1