Wing framework and skin welding method

By using optimized tooling fixtures and 3D printed grid structures in wing welding, combined with reasonable welding sequence and gas protection, laser welding deformation and quality problems are solved, and efficient welding process and high-quality welding results are achieved.

CN118989583AActive Publication Date: 2024-11-22BEIJING XINGHANG MECHANICAL ELECTRICAL EQUIP CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411341165.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-11-22
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

Laser welding has problems in the manufacturing of wings that are difficult to control welding deformation and difficult to ensure welding quality, especially in thin-walled parts and complex structures of thin-walled wings, which leads to accumulation of welding stress and frequent occurrence of defects.

Method used

Using a welding method of wing frame and skin, the longitudinal members and transverse ribs of grid structures are optimized by designing tool fixtures for welding and 3D printing to manufacture grid structures, combined with reasonable positioning and clamping mechanisms, and optimize welding sequence and gas protection measures. , ensure deformation control and quality improvement during welding.

Benefits of technology

Effectively control welding deformation below ±0.5%, significantly improve welding quality, reduce defects, such as oxidation, inclusion, pores, cracks, etc., and meet the requirements of lightweight, high strength and welding efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989583A_ABST
    Figure CN118989583A_ABST
Patent Text Reader

Abstract

The invention relates to a welding method for a wing framework and a skin, belongs to the technical field of welding, and solves the problems that when an existing laser welding method is applied to wing manufacturing, welding deformation is difficult to control, and welding quality is difficult to guarantee. A welding method for a wing framework and a skin comprises the steps that S1, a tool clamp used for welding the wing framework is designed; s2, all longitudinal components and transverse ribs of the wing framework are manufactured through a 3D printing method; s3, all the longitudinal components and the transverse bars are assembled on a tool clamp; and S4, front face protection and back face protection are conducted on the weld joints, welding is conducted under protection of inert gas, and the wing framework is obtained. By optimizing the joint form, the tool clamp, the assembly procedure, the welding sequence, the gas protection measures and the process parameters, the welding deformation can be controlled to be + / -0.5% or below, the defects prone to occurring in the wing laser welding process are reduced, and the welded joint can meet the requirements for light weight, high strength and high welding efficiency at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding, and in particular to a welding method for a wing frame and a skin. Background Art

[0002] Laser welding has the advantages of high energy density, small heat-affected zone, flexible spatial position conversion, and fast welding speed. It shows great potential and advantages in the manufacturing of thin-walled wings in the aerospace field.

[0003] However, the application of laser welding in wing manufacturing faces a series of challenges, especially in controlling welding deformation and ensuring welding quality. The following are the main difficulties and reasons for laser welding wings: (1) Welding deformation is difficult to control: a. The high energy input during laser welding may cause the temperature of the welding area and its surrounding areas to rise rapidly, resulting in thermal expansion and uneven thermal stress, causing deformation; b. The components of the wing are usually made of light metal materials such as titanium alloys and are all thin-walled parts. Due to the high thermal expansion coefficient of light metal materials and the low stiffness of thin-walled parts, welding deformation may be aggravated; c. The structure of the wing is relatively complex and there are many welding joints. , which makes it easier to accumulate welding stress and cause structural deformation; (2) Welding quality is difficult to ensure: a. In the welding of multiple joints in the wing, it is a challenge to achieve a back gas protection method that is both simple and easy to operate and effectively protects each weld. Poor back gas protection can lead to defects such as weld oxidation and inclusions; b. Due to the structural and material characteristics of the wing, it is highly sensitive to welding parameters. Slight changes in parameters may lead to welding defects such as pores, cracks, lack of fusion, undercuts, and dents; c. In the welding of multiple joints in the wing, it is difficult to simultaneously meet the requirements of lightweight, high strength, and high welding efficiency due to unreasonable joint design or limitations of manufacturing and assembly processes.

[0004] Based on the above analysis, there is an urgent need to provide a welding method for the wing frame and skin to effectively control and reduce welding deformation and significantly improve welding quality, which is of great significance for improving the overall performance and reliability of the aircraft. Summary of the invention

[0005] In view of the above analysis, the present invention aims to provide a method for welding a wing frame and a skin, so as to solve the problem that the existing laser welding method is difficult to control welding deformation and ensure welding quality when applied to wing manufacturing.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] The present invention provides a method for welding a wing frame and a skin, comprising the following steps:

[0008] S1. Design of fixture for welding wing frame;

[0009] The wing skeleton is a thin-walled grid structure, which is mainly formed by M longitudinal members parallel to the first direction and N transverse members parallel to the second direction through M*N nodes, and each transverse member contains M-1 transverse ribs; M≥3, N≥3; the first direction is different from the second direction;

[0010] The tooling fixture of the wing frame includes: a base plate, a positioning mechanism and a clamping mechanism arranged on the base plate;

[0011] S2. All longitudinal components and transverse ribs of the wing skeleton are manufactured by 3D printing; wherein, when establishing a 3D printed model, the M longitudinal components are designed to include 2×N×(M-1) connection ends along the second direction to accurately connect with the two end faces of each transverse rib to form 2×N×(M-1) butt joints; the inner side edges of the longitudinal components and transverse components located at the outermost side of the wing skeleton are designed to include step grooves with the same thickness as the skin; ventilation holes are reserved on the longitudinal components and transverse ribs located inside the wing skeleton to connect each grid structure;

[0012] S3. Assemble all longitudinal components and transverse ribs on the fixture, and control welding deformation and meet assembly tolerance requirements through reasonably designed positioning and clamping mechanisms;

[0013] S4. Protect the front and back sides of the weld. Under the protection of inert gas, weld 2×N×(M-1) butt joints of the wing skeleton in sequence from one end to the other end in the first direction and from one side to the other side along the second direction to obtain the wing skeleton.

[0014] Further, S3 specifically includes the following steps:

[0015] S31: cooperating and positioning the first longitudinal member with the positioning mechanism, and providing a clamping mechanism at a 1 / 5 to 4 / 5 section of the first longitudinal member between any two adjacent butt joints;

[0016] S32: assembling N transverse ribs on the base plate in sequence from one end to the other end of the first longitudinal member, and providing a clamping mechanism at a 1 / 3 to 2 / 3 section of each transverse rib;

[0017] S33: assembling the second longitudinal member on the base plate, and providing a clamping mechanism at a 1 / 5 to 4 / 5 section of the second longitudinal member between any two adjacent butt joints;

[0018] Repeat S32 and S33 alternately to assemble the third longitudinal member to the M-1 longitudinal member and the remaining transverse reinforcements;

[0019] S34: Assemble the Mth longitudinal member on the base plate; set a clamping mechanism in the 1 / 5 to 4 / 5 section of the Mth longitudinal member between any two adjacent butt joints, and set a clamping mechanism on the outside of the Mth longitudinal member and directly opposite to each butt joint.

[0020] Further, in S1, the angle between the first direction and the second direction is 85° to 95°.

[0021] Furthermore, in S1, the cross-sectional shape of the longitudinal member and the transverse rib is an I-shaped or Π-shaped or a combination thereof; and / or the wall thickness of the longitudinal member and the transverse rib is 2 mm to 10 mm.

[0022] Furthermore, the method further comprises the following steps:

[0023] S5, assembling the wing frame and the skin to be welded obtained in S4 on a fixture for welding the wing frame and the skin; controlling welding deformation and meeting assembly tolerance requirements through a reasonably designed frame side pressure mechanism and skin pressing mechanism on the fixture; specifically comprising the following steps:

[0024] S51: Assemble the wing frame on the fixture, and set two frame side pressure mechanisms between any two adjacent butt joints of the first longitudinal member and the Mth longitudinal member;

[0025] S52: overlap the upper and lower skins on the step groove described in S2, and set 2×(M+N-4) skin clamping mechanisms on the outer sides of the upper and lower skins and along the contact parts of the M-2 longitudinal members and N-2 transverse members in the wing frame with the upper and lower skins to ensure that the skins are fixed and clamped on the fixture, and that the skins are surrounded by the wing frame to form a butt joint with a flush surface; each skin clamping mechanism is provided with a groove of a size that can accommodate the contact surface of the corresponding longitudinal member or transverse member with the skin;

[0026] S6, protecting the front and back of the weld, welding under the protection of inert gas, to obtain a combination of the wing frame and the upper and lower skins; specifically comprising the following steps:

[0027] S61: Weld the contact parts of the second transverse member, the third transverse member, ... the N-1th transverse member and the skin in sequence from one end to the other end along the first direction; for each transverse member, weld in the same direction from one side to the other side along the second direction;

[0028] S62: weld the second longitudinal member, the M-1 longitudinal member, the third longitudinal member, the M-2 longitudinal member, etc. in sequence from both sides to the middle along the second direction to the contact portion between the 1 / 2*M longitudinal member or the 1 / 2*(M+1) longitudinal member and the skin; for each longitudinal member, weld symmetrically from both ends to the middle along the first direction;

[0029] S63: Perform lock bottom welding on the contact parts between the two longitudinal members and two transverse members on the outside of the wing frame and the skin.

[0030] Further, in S4, the main step of back side protection includes: on the back side of each butt joint, a sealing cover is built in situ with a flexible sealing material, and holes are opened in the sealing cover to form an inlet and an outlet for an inert gas; and / or,

[0031] In S6, the main steps of back protection include: using the wing frame with reserved ventilation holes in step S2 and the upper and lower skins to form a closed and connected air path environment, and the inert gas enters from one end of the wing frame and is discharged from the other end.

[0032] Furthermore, in S3 and S5, the assembly tolerance requirements include: the butt joint gap and step difference at each point of each joint shall not exceed 0.1 mm, and the butt joint gap and step difference with a cumulative length of no more than 30 mm within any local 100 mm shall not exceed 0.2 mm.

[0033] Furthermore, in steps S4 and S6, chord plane measurements are performed before and after welding, respectively, and shape correction is performed by comparing the chord plane measurement results.

[0034] Furthermore, in steps S3 and S5, the assembly includes trial assembly, repair trial assembly, pickling, removing oxide scale, and formal assembly.

[0035] Furthermore, it also includes: before trial assembly, pre-treating the area to be welded until the metallic luster is exposed and the surface roughness of the surface to be welded Ra≤3.2μm.

[0036] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:

[0037] The present invention provides a method for welding a wing frame and a skin, which is optimized from many aspects (such as: fixtures and assembly procedures, welding sequence, chord plane measurement and shape correction), effectively controlling and significantly reducing the deformation of the wing frame and the skin during laser welding, and the welding deformation can be controlled below ±0.5%; specifically,

[0038] (1) The present invention optimizes the jig and assembly process, including the positioning scheme and the clamping scheme (clamping mechanism type, clamping point position and number, assembly sequence), effectively controls the movement and dislocation during the welding process, and significantly reduces welding deformation; a. Positioning scheme: When assembling the parts of the wing frame, firstly, the positioning mechanism on the jig cooperates with the first longitudinal member to determine the position of the first longitudinal member relative to the base plate along the first direction and use this as the reference position when other components are installed, so as to ensure the relative position of each component during assembly; b. Clamping scheme: By selecting a suitable type of clamping mechanism (including a clamping mechanism, a side pressure mechanism, a push mechanism, a frame side pressure mechanism, and a skin clamping mechanism), and setting a suitable number of clamping mechanisms at suitable positions, and using a suitable assembly sequence to rigidly fix each part, ensure that the clamping force is evenly distributed, avoid unnecessary constraints in the welding area, and at the same time, through the suitable support points provided by the base plate for the parts to be welded, effectively control the movement and dislocation during the welding process, and significantly reduce welding deformation.

[0039] (2) The present invention reduces welding stress and welding deformation by optimizing the welding sequence; for example, when welding parts of a wing frame, a preferred welding sequence (i.e., welding is performed sequentially from one end to the other end along the first direction and from one side to the other side along the second direction) is adopted to first perform positioning welding and then perform formal welding; when welding the wing frame and the skin, a preferred welding sequence (including welding M-2 longitudinal components from both sides to the middle along the second direction, and symmetrically welding each longitudinal component from both ends to the middle along the first direction) is first adopted to perform penetration welding, and then a preferred welding sequence (including welding the outermost longitudinal component first and then welding the outermost transverse component) is adopted to perform surrounding lock bottom welding; the above welding sequence can enable the weld to shrink more freely, reduce the accumulation of welding stress, and minimize the welding deformation that may be caused by the residual stress generated during the laser welding process.

[0040] (3) The present invention further eliminates the slight deformation caused by welding through chord plane measurement and correction, thereby ensuring the geometric dimensional accuracy of the wing frame and skin after welding; specifically, the chord plane measurement is performed on the wing frame and the combination of the wing frame + upper and lower skins before and after welding, and the deformation point positions and deformation amounts are compared to correct the shape of the wing frame and the combination of the wing frame + upper and lower skins.

[0041] The present invention provides a method for welding a wing frame and a skin, which is optimized from many aspects (such as joint form, fixture and assembly process, gas protection measures, and process parameters), effectively reducing defects that are prone to occur during laser welding of wings (including oxidation, inclusions, pores, cracks, unfusion, undercuts, and depressions), and the welded joint can simultaneously meet the requirements of lightweight, high strength, and high welding efficiency, thereby improving the welding quality; specifically, it includes:

[0042] (1) By optimizing the joint form, fixtures and assembly procedures, the present invention can simultaneously meet the requirements of high strength, light weight and high welding efficiency for the welded joint; at the same time, it can effectively reduce crack defects.

[0043] a. Joint form: The parts to be welded of the wing skeleton are processed by 3D printing, and machining is used to ensure that the parts of the wing skeleton and the skeleton and the skin can be accurately aligned to form a butt joint, that is, the longitudinal member includes a connecting end along the second direction, which can be connected one by one with the two end faces of the transverse rib to form a butt joint, the inner side edges of the longitudinal member and the transverse member located at the outermost side of the wing skeleton include step grooves, and the skin is overlapped on the step grooves to form a butt joint with a flush surface. Compared with T-joints between parts of the wing skeleton and lap joints directly around the wing skeleton and the skin, the present invention uses 3D printing in combination with machining and fixtures to accurately process and align to form a butt joint, which effectively improves the welding strength of the wing skeleton and the skin. At the same time, the weld width is small and the welding operation is convenient, so that the welded joint can have the advantages of high strength, light weight, and high welding efficiency.

[0044] b. Fixtures and assembly procedures: Through the careful design of fixtures and the rational arrangement of assembly procedures, the welding stress and deformation are effectively reduced, the crack defects caused by residual stress are avoided, and the dimensional accuracy of the welded wing frame and skin is ensured.

[0045] (2) The present invention effectively reduces the defects of oxidation, inclusions and pores by optimizing gas protection measures.

[0046] Specifically, inert gas is used for front and back protection at each weld. For example, when welding parts of the wing frame, a sealing cover is built in situ with flexible sealing material on the back of each butt joint; when welding the wing frame and skin, a closed and connected air path environment is formed by the wing frame and upper and lower skins with vents; the above simple, easy-to-operate and reliable gas protection measures can effectively prevent air from contacting the molten pool, minimize the oxidation, inclusion and porosity problems that may occur during welding of light metal wings, thereby improving the intrinsic quality of the weld.

[0047] (3) The present invention optimizes the welding process parameters, that is, according to the structural characteristics of the wing frame and skin to be welded, selects appropriate process parameters, including: laser power, defocusing amount, welding speed, arc starting and extinguishing distance, and shielding gas flow rate, thereby effectively reducing the problems of oxidation, inclusions, pores, cracks, unfused, undercuts, and depressions, and significantly improving the welding quality of thin-walled wing parts.

[0048] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0049] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.

[0050] Figure 1 A schematic diagram (partial) of a wing skeleton provided by an embodiment of the present invention;

[0051] Figure 2 A schematic diagram (partial) of a wing frame on a fixture provided by an embodiment of the present invention;

[0052] Figure 3 In (a), Figure 2 The enlarged three-dimensional schematic diagram of part A in the middle, (b) Figure 2 The enlarged three-dimensional schematic diagram of part B in the middle, (c) Figure 2 The enlarged three-dimensional schematic diagram of the middle C part, (d) Figure 2 The enlarged three-dimensional schematic diagram of the D part in the middle, (e) Figure 2 The enlarged three-dimensional schematic diagram of the middle E part;

[0053] Figure 4 A schematic diagram (partial) of a wing frame and skin provided by an embodiment of the present invention;

[0054] Figure 5 A schematic diagram (partial) of a wing frame and skin on a fixture provided by an embodiment of the present invention;

[0055] Figure 6 A site map of welding deformation obtained by comparing the chord plane three-dimensional model of the wing skeleton before and after welding provided by an embodiment of the present invention;

[0056] Figure 7 A photo (partial) of the weld seam of the wing frame and skin lock bottom weld provided in an embodiment of the present invention;

[0057] Figure 8 A photograph (partial) of an X-ray nondestructive test of the weld of the wing frame and skin lock bottom weld provided in an embodiment of the present invention;

[0058] Reference numerals:

[0059] 100-wing frame; 11-first main beam; 12-second main beam; 13-third main beam; 14-first transverse rib; 15-second transverse rib; 16-third transverse rib; 17-fourth transverse rib; 18-vent; 200-fixture for wing frame; 21-locating pin; 22a-clamping mechanism; 22b-side pressure mechanism; 22c-pushing mechanism; 23a-first rotating mechanism; 23b-second rotating mechanism; 24-connecting end; 25-butt joint; 26-step groove; 300-skin; 400-fixture for wing frame and skin; 41-skin clamping mechanism; 42-frame side pressure mechanism; 43a-first fixture rotating mechanism; 43b-second fixture rotating mechanism. DETAILED DESCRIPTION

[0060] The preferred embodiments of the present invention are described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of this application and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.

[0061] The present invention provides a method for welding a wing frame and a skin, comprising the following steps:

[0062] Step S1, designing a fixture for welding a wing frame;

[0063] The wing skeleton is a thin-walled grid structure, which is mainly formed by M longitudinal members parallel to the first direction and N transverse members parallel to the second direction through M×N nodes, and each transverse member contains M-1 transverse ribs; M≥3, N≥3; the first direction is different from the second direction;

[0064] The tooling fixture of the wing frame includes: a base plate, a positioning mechanism and a clamping mechanism arranged on the base plate;

[0065] Preferably, the angle between the first direction and the second direction is 85° to 95°; illustratively, the angle between the first direction and the second direction is a right angle.

[0066] Preferably, the longitudinal members and the transverse ribs are rod-shaped members; more preferably, the longitudinal members and the transverse ribs are rod-shaped members with hollow structures.

[0067] Optionally, the cross-sectional shape of the longitudinal member and the transverse rib may be, but is not limited to, an I-shaped, a Π-shaped, or a combination thereof.

[0068] Preferably, the wall thickness of the longitudinal members and the transverse ribs is 2 mm to 10 mm; more preferably, the wall thickness of the longitudinal members and the transverse ribs is 2 mm to 3 mm.

[0069] Preferably, the longitudinal members and transverse ribs are made of titanium alloy, aluminum alloy, steel or a combination of the two.

[0070] It is understandable that the shape of the substrate depends on the shape of the wing frame and can be designed as needed, as long as it can support and support the parts to be welded of the wing frame. Figure 2 The substrate is in the shape of a grid-like thin plate, and each grid includes a hollow structure.

[0071] It should be noted that the positioning mechanism on the substrate includes W positioning pins, W ≥ 2; the W lugs included in the first longitudinal member are matched with the W positioning pins to limit the position of the first longitudinal member relative to the substrate along the first direction, and this position will serve as the reference position when other components are installed, thereby ensuring the relative position of each component during assembly.

[0072] Preferably, the positioning mechanism is arranged outside the area to be welded, avoiding the weld position and ensuring the accessibility of the welding tool; in a possible design, see Figure 2 The outer side of the first longitudinal member (i.e., the first main beam 11) includes two lugs spaced apart along the first direction, and each lug cooperates with a positioning pin 21 on the base plate, that is, the positioning pin 21 passes through the inner hole on the lug to accurately position the first longitudinal member along the first direction at the position where the positioning pin is located on the base plate.

[0073] It should be noted that the clamping mechanism on the substrate includes one or a combination of three types: a pressing mechanism, a side pressure mechanism, and a pushing mechanism, and the number and position of each type of clamping mechanism can be designed as needed.

[0074] Preferably, the clamping mechanism comprises a combination of three types: a clamping mechanism, a side pressure mechanism, and a pushing mechanism.

[0075] Preferably, each clamping mechanism includes a clamping strip, the two ends of which can be located on both sides of the same longitudinal member or transverse rib, and the longitudinal member or transverse rib is fixed and clamped on the substrate along the entire width direction to control the relative position of the parts to be welded in the wing frame and the thermal deformation during welding.

[0076] As an optional embodiment, the two ends of the compression strip are fixed to the base plate by threaded connection; for example, see Figure 2 and Figure 3 (a) The clamping mechanism 22a includes a clamping strip with inner holes at both ends for screws or bolts to pass through and be screwed into the base plate.

[0077] Preferably, each side pressure mechanism includes a clamping plate, one end of which may be located on the surface of the longitudinal member or transverse rib, and the other end of which is fixed to the base plate, and is used to fix and clamp the longitudinal member or transverse rib to the base plate along part or all of the width, so as to control the relative position of the parts to be welded in the wing frame and the thermal deformation during welding.

[0078] As an optional embodiment, the pressing sheet is fixed to the base plate by threaded connection; for example, see Figure 2 and Figure 3 (b) The side pressure mechanism 22b includes a pressure plate whose portion not in contact with the longitudinal member or the transverse rib has an inner hole for a screw or a bolt to pass through and be screwed into the base plate.

[0079] It is understandable that the number of inner holes on the clamping plate can be designed as needed; illustratively, the clamping plate includes two inner holes to achieve effective fixation while ensuring that the clamping force is evenly distributed to avoid deformation due to local over-tightening.

[0080] In a possible design, a blind groove is also provided on the clamping plate to accommodate the protrusion on the longitudinal member or the transverse rib to adapt to the non-planar shape of the parts to be welded in the wing frame and facilitate installation operations; the shape of the blind groove depends on the shape of the protrusion on the longitudinal member or the transverse rib.

[0081] Preferably, each pushing mechanism includes a pushing block and a mounting seat, the pushing block includes a push rod and an end pressure portion which are connected to each other, the mounting seat is fixed on the base plate, the push rod is fixed in the mounting seat by a rotating connection, and the end pressure portion is driven to abut against the side wall of the longitudinal member or the transverse rib by rotating the push rod, so as to control the relative position of the parts to be welded in the wing frame and the thermal deformation during welding.

[0082] Preferably, the push rod and the mounting seat are rotatably connected via threads; for example, see Figure 2 and Figure 3 (c) The push mechanism 22c cooperates with the threads of the inner hole of the mounting seat through the threads on the outer surface of the push rod.

[0083] Preferably, the tooling fixture used for welding the wing frame also includes a rotating mechanism coaxially arranged on both sides of the base plate; the two rotating mechanisms are connected to the welding workbench, and the tooling fixture is adjusted by the rotating mechanism to facilitate welding of different angles of the wing frame, thereby improving the accessibility of the welding gun.

[0084] Preferably, the two rotating mechanisms ( Figure 2 The first rotating mechanism 23a and the second rotating mechanism 23b) are coaxially arranged on both sides of the substrate and the rotation axis is perpendicular to the first direction; more preferably, the two rotating structures are coaxially arranged at the middle position of both sides of the substrate and the rotation axis is perpendicular to the first direction.

[0085] Step S2, using a 3D printing method to manufacture all longitudinal components and transverse ribs of the wing skeleton; wherein, when establishing a 3D printed model, the M longitudinal components are designed to include 2×N×(M-1) connection ends along the second direction, so as to accurately connect with the two end faces of each transverse rib to form 2×N×(M-1) butt joints; the inner side edges of the longitudinal components and transverse components located at the outermost side of the wing skeleton are designed to include step grooves with the same thickness as the skin; ventilation holes are reserved on the longitudinal components and transverse ribs located inside the wing skeleton to connect each grid structure;

[0086] Preferably, the above 3D printing method further includes: after the 3D printing is completed, all longitudinal members and transverse ribs (mainly the surfaces to be welded) are machined and finished to further improve the accuracy of the alignment of the butt joints between the longitudinal members and transverse ribs, and between the outermost longitudinal members and transverse members of the wing skeleton and the skin. The machining finishing method can be selected as needed, including but not limited to one or a combination of milling, grinding, scraping, lapping, super finishing, and polishing.

[0087] For example, see Figure 3 (d) The third main beam 13 includes a connecting end 24 along the second direction to accurately butt with the left end surface of the fourth transverse reinforcement 17 to form a butt joint 25.

[0088] It is worth noting that compared with the T-joint between the longitudinal member and the transverse rib, the longitudinal member obtained by 3D printing and machining in the present invention forms a butt joint by connecting the end head with the two ends of the transverse rib one by one, which achieves at least the following beneficial effects: (1) Due to the symmetry of the butt joint formed at both ends of the transverse rib, it can provide a more uniform stress distribution in the welding area and reduce the risk of cracks and other welding defects caused by stress concentration; (2) The heat distribution during the welding of the butt joint is relatively uniform, which helps to reduce the occurrence of welding defects such as pores and lack of fusion; (3) The welding strength of the butt joint is higher and the weld width is smaller. No additional filling material or special edge design is required, which may be more economical in material use and is conducive to achieving the requirements of both lightweight and high strength of the wing.

[0089] For example, see Figure 3 (e) The inner sides of the transverse member at the uppermost end of the wing frame and the longitudinal member at the rightmost end include a step groove 26, the height of which is the same as the thickness of the skin, so that the upper and lower skins overlap on the step groove 26 to form a butt joint with a flush surface.

[0090] It is worth noting that, compared with the case where the upper and lower skins are directly placed on the surface of the wing frame to form a lap joint, the present invention achieves at least the following beneficial effects by designing step grooves along the outermost sides of the wing frame for the skin to overlap on the step grooves to form a butt joint with a flush surface: (1) The contact area of ​​the welds around the wing frame and the skin is larger, which is beneficial to improving the welding strength of the bottom lock welds around the wing frame, and the weld width is smaller, which is beneficial to achieving a balance between light weight and high strength; (2) Since the contact area around the wing frame and the skin is larger, the heat distribution during welding is relatively uniform, which helps to reduce the occurrence of welding defects such as pores and unfused welds; (3) By utilizing the positioning function of the step groove, the positioning of the skin and the wing frame can be quickly achieved without the need for an additional positioning mechanism, and the relative position and structural stability of the skin and the wing frame can be maintained during the welding process, reducing the risk of cracks and other welding defects caused by stress concentration.

[0091] For example, see Figure 1 Ventilation holes are reserved on all longitudinal members and transverse ribs (such as the second main beam 12 and the third transverse rib 16) inside the wing frame to allow each grid structure to be connected.

[0092] Step S3, assembling all longitudinal members and transverse ribs on a fixture, controlling welding deformation and meeting assembly tolerance requirements through a reasonably designed positioning mechanism and clamping mechanism; specifically comprising the following steps:

[0093] S31: cooperating and positioning the first longitudinal member with the positioning mechanism, and providing a clamping mechanism at a 1 / 5 to 4 / 5 section of the first longitudinal member between any two adjacent butt joints;

[0094] In a possible design, W lugs included in the first longitudinal member are matched and positioned with W positioning pins on the base plate to define a relative position of the first longitudinal member relative to the base plate along a first direction; W≥2.

[0095] Preferably, a side pressure mechanism is respectively arranged in the 1 / 5 to 2 / 5 and 3 / 5 to 4 / 5 sections of the first longitudinal member between any two adjacent butt joints (based on any one of the two adjacent butt joints), and a clamping mechanism is arranged in the 2 / 5 to 3 / 5 section;

[0096] More preferably, a side pressure mechanism is provided at 1 / 4 and 3 / 4 of the first longitudinal member between any two adjacent butt joints (based on any one of the two adjacent butt joints), and a clamping mechanism is provided at 1 / 2.

[0097] S32: assembling N transverse ribs on the base plate in sequence from one end to the other end of the first longitudinal member, and providing a clamping mechanism at a 1 / 3 to 2 / 3 section of each transverse rib;

[0098] Preferably, two side pressure mechanisms are arranged at the 1 / 3 to 2 / 3 section of each transverse rib (based on either end of each transverse rib); more preferably, one side pressure mechanism is arranged at the 1 / 3 and 2 / 3 of each transverse rib (based on either end of each transverse rib).

[0099] S33: assembling the second longitudinal member on the base plate, and providing a clamping mechanism at a 1 / 5 to 4 / 5 section of the second longitudinal member between any two adjacent butt joints;

[0100] Specifically, the second longitudinal member is placed on the substrate and abutted against the ends of the N transverse ribs in step S32, and a clamping mechanism is provided in the 1 / 5 to 4 / 5 section of the second longitudinal member between any two adjacent butt joints (based on any one of the two adjacent butt joints).

[0101] Preferably, a side pressure mechanism is provided in a section of the second longitudinal member between any two adjacent butt joints (based on any one of the two adjacent butt joints) at 1 / 5 to 4 / 5;

[0102] In a possible design, a side pressure mechanism is provided in a section of the second longitudinal member between 2 / 5 and 3 / 5 of any two adjacent butt joints (based on any one of the two adjacent butt joints);

[0103] In a possible design, a side pressure mechanism is respectively provided in the 1 / 5 to 2 / 5 and 3 / 5 to 4 / 5 sections of the second longitudinal member located between any two adjacent butt joints (based on any one of the two adjacent butt joints).

[0104] Repeat S32 and S33 alternately to assemble the third longitudinal member to the M-1 longitudinal member and the remaining transverse reinforcements;

[0105] Specifically, assemble the third longitudinal member according to S33, assemble N transverse reinforcements between the third longitudinal member and the fourth longitudinal member according to S32...; assemble the M-1th longitudinal member according to S33, and assemble N transverse reinforcements between the M-1th longitudinal member and the Mth longitudinal member according to S32.

[0106] S34: assembling the Mth longitudinal member on the base plate; providing a clamping mechanism at a 1 / 5 to 4 / 5 section of the Mth longitudinal member between any two adjacent butt joints, and providing a clamping mechanism at the outside of the Mth longitudinal member and directly opposite to each butt joint;

[0107] Preferably, a side pressure mechanism is respectively arranged at the 1 / 5 to 2 / 5 and 3 / 5 to 4 / 5 sections of the Mth longitudinal member located between any two adjacent butt joints (based on any one of the two adjacent butt joints), a clamping mechanism is arranged at the 2 / 5 to 3 / 5 section, and a push mechanism is arranged outside the Mth longitudinal member and directly opposite to each butt joint;

[0108] More preferably, a side pressure mechanism is provided at 1 / 4 and 3 / 4 of the Mth longitudinal member between any two adjacent butt joints (based on any one of the two adjacent butt joints), and a clamping mechanism is provided at 1 / 2.

[0109] See also Figure 2 A push mechanism 22c is arranged on the outside of the Mth longitudinal member and directly opposite to each butt joint.

[0110] Step S4, perform front and back protection on the weld, and under the protection of inert gas, weld 2×N×(M-1) butt joints of the wing skeleton in sequence from one end to the other end in the first direction and from one side to the other side along the second direction to obtain the wing skeleton.

[0111] Step S41: using inert gas to protect the front and back of the weld;

[0112] Specifically, a fixture equipped with wing skeleton parts to be welded is placed on a laser welding platform and fixed, and an inert gas is used to protect the front and back sides of the weld. In a possible design, the fixture is assembled and fixed to the laser welding platform through rotating mechanisms on both sides. Among them, the front protection can adopt the drag hood protection method in the prior art (nozzle + drag hood, inert gas is sprayed from the drag hood).

[0113] Preferably, in step S4, the main steps of back side protection include: on the back side of each butt joint, a sealing cover is built in situ with a flexible sealing material (sealing at the weld), and holes are opened in the sealing cover to form an inlet and an outlet for the inert gas.

[0114] In one possible design, a sealing tape is bonded to the longitudinal member and / or transverse rib near the back of each weld to form a sealing cover, and holes are opened in the sealing cover to form an inlet and outlet for the inert gas. This method has easy-to-obtain materials, simple operation, good back gas protection effect, and the tape can be quickly removed after welding.

[0115] Furthermore, the positions of the gas inlet and outlet are designed according to the specific gravity of the selected inert gas and air; preferably, the inert gas is argon, the gas inlet is located at the lower part of the sealing cover, and the gas outlet is located at the upper part of the sealing cover; argon is heavier than air, and it is easy to obtain a higher concentration by filling argon from a lower position, and the argon filling protection effect is better.

[0116] Step S42: Under the protection of an inert gas, 2×N×(M-1) butt joints of the wing skeleton are welded sequentially from one end to the other end in the first direction and from one side to the other side in the second direction; comprising the following steps:

[0117] S421: Positioning welding;

[0118] Specifically, first find the welding trajectory, that is, ensure that the laser spot is located in the middle of the weld; then perform positioning welding on all welding joints of the wing frame.

[0119] Preferably, the middle part of the welding joint is selected for tack welding; since the length of the welding joints of the longitudinal members and transverse ribs of the wing frame is short, selecting the middle part of the joint for tack welding can effectively ensure uniform heat input and reduce welding deformation and stress concentration.

[0120] The tack weld length may be determined according to the length of the weld joint; preferably, the tack weld length is 1 / 5 to 1 / 3 of the length of the weld joint; illustratively, the length of the weld joint is 30 mm and the tack weld length is 10 mm.

[0121] Optionally, the process parameters of positioning welding are: laser power of 700W to 900W, defocus of -1.0mm to -3.0mm, and welding speed of 0.5m / min to 2.5m / min; preferably, the process parameters of positioning welding are: laser power of 750W to 850W, defocus of -1.5mm to -2.5mm, and welding speed of 1.0m / min to 2.0m / min; exemplarily, the laser power is 800W, the defocus is -2mm, and the welding speed is 1.5m / min.

[0122] Step S422: formal welding;

[0123] Preferably, according to the welding sequence: from one end to the other end in the first direction, and from one side to the other side along the second direction, 2×N×(M-1) butt joints of the wing frame are welded in sequence.

[0124] The above welding sequence allows the weld to shrink more freely, reducing the accumulation of welding stress, thereby minimizing the welding deformation that may be caused by the residual stress generated during the laser welding process; at the same time, it facilitates the welding operation and effectively ensures the straightness of the welding joints located in the same straight line.

[0125] For example, see Figure 1, the eight welding joints are welded in sequence (①-⑧); that is, from top to bottom, along the second cross beam (including the second cross rib 15 and the first cross rib 14) from left to right, first weld the butt joint ① between the second cross rib 15 and the third main beam 13, and the butt joint ② between the second cross rib 15 and the second main beam 12 in sequence; then weld the butt joint ③ between the first cross rib 14 and the second main beam 12, and the butt joint ④ between the first cross rib 14 and the first main beam 11 in sequence; then, along the third cross beam (including the fourth cross rib 17 and the third cross rib 16) from left to right, first weld the butt joint ⑤ between the fourth cross rib 17 and the third main beam 13, and the butt joint ⑥ between the fourth cross rib 17 and the second main beam 12 in sequence; then weld the butt joint ⑦ between the third cross rib 16 and the second main beam 12, and the butt joint ⑧ between the third cross rib 16 and the first main beam 11 in sequence.

[0126] If ① and ④ are welded first, ② and ③ may not be able to be connected in a straight line due to different directions of thermal deformation.

[0127] Preferably, the welding sequence of step S422 is the same as that of step S421. By following a consistent welding sequence for positioning welding and formal welding, it is helpful to better control the heat input and heat distribution during the welding process, thereby reducing welding deformation.

[0128] Optionally, the process parameters of formal welding are: laser power of 1700W to 2100W, defocus of -3.5mm to -6.5mm, and welding speed of 0.5m / min to 2.5m / min; preferably, the process parameters of formal welding are: laser power of 1850W to 1950W, defocus of -4.5mm to -5.5mm, and welding speed of 1.0m / min to 2.0m / min; exemplarily, the laser power is 1900W, the defocus is -5mm, and the welding speed is 1.5m / min.

[0129] As an optional implementation, step S422 further includes the following welding sequence to reduce welding deformation:

[0130] S4221: Weld the front weld of each joint of the wing frame;

[0131] S4222: Flip the fixture by rotating the mechanism to weld the reverse weld of each joint of the wing frame;

[0132] S4223: Adjust the fixture through the rotating mechanism to weld the side weld of each joint.

[0133] In one possible design, for areas that are difficult to reach or observe during the welding process, that is, processing dead corners, nonlinear programming or flexible welding equipment, such as welding robots, can be used to adjust the welding gun angle according to actual conditions to ensure the accessibility of the welding gun.

[0134] Step S5, assembling the wing frame and the skin to be welded obtained in step S4 on a fixture for welding the wing frame and the skin; controlling welding deformation and meeting assembly tolerance requirements through a reasonably designed frame side pressure mechanism and skin pressing mechanism on the fixture;

[0135] The tooling fixture for welding the wing frame and skin comprises: a base plate, a frame side pressing mechanism and a skin pressing mechanism arranged on the base plate;

[0136] Preferably, each skeleton side pressure mechanism includes a clamping plate, one end of which can be pressed on the surface of the outermost longitudinal member or transverse member of the wing skeleton, and the other end is fixed on the base plate; thereby controlling the relative position and thermal deformation of the wing skeleton and the tooling fixture.

[0137] Step S5 specifically includes the following steps:

[0138] S51: Assemble the wing frame on the fixture, and set two frame side pressure mechanisms between any two adjacent butt joints of the first longitudinal member and the Mth longitudinal member;

[0139] Specifically, the wing frame welded in S4 is disassembled from the fixture 200 for welding the wing frame, and then assembled on another set of fixtures 400 for welding the wing frame and the skin, and two frame side pressure mechanisms are arranged between any two adjacent butt joints of the first longitudinal member and the Mth longitudinal member; see Figure 5 The frame side pressing mechanism 42 is used to fix and press the wing frame onto the base plate.

[0140] Preferably, a skeleton side pressure mechanism is respectively provided in the 1 / 5 to 2 / 5 and 3 / 5 to 4 / 5 sections of the first longitudinal member and the Mth longitudinal member located between any two adjacent butt joints (taking any one of the two adjacent butt joints as a reference).

[0141] S52: Overlap the upper and lower skins on the step groove described in S2, and set 2×(M+N-4) skin clamping mechanisms on the outside of the upper and lower skins and along the contact parts of the M-2 longitudinal members and N-2 transverse members in the wing frame with the upper and lower skins to ensure that the skins are fixed and clamped on the fixture, and that the skins form a butt joint with the wing frame with a flush surface all around; each skin clamping mechanism is provided with a groove of a size that can accommodate the contact surface of the corresponding longitudinal member or transverse member with the skin.

[0142] Preferably, each skin clamping mechanism comprises a clamping strip, on which is provided a groove which is just large enough to accommodate the contact surface between the corresponding longitudinal member or transverse member and the upper skin or lower skin and which passes through the upper and lower surfaces of the clamping strip.

[0143] It can be understood that the skin clamping mechanism is used to fix and press the wing frame together with the upper skin and / or lower skin covering the surface of the wing frame on the substrate along the first direction and / or the second direction; the skin clamping mechanism can control the relative position of the wing frame and the upper and lower skins, and at the same time, for such long weld penetration welding, the skin clamping mechanism is arranged along the weld between the wing frame and the upper and lower skins, which can effectively control the thermal deformation of the wing frame and the skin during welding.

[0144] As an optional embodiment, the clamping strip is fixed to the base plate by a threaded connection; exemplarily, a plurality of holes are provided at the end of the clamping strip and / or along both sides of the groove for screws or bolts to pass through and be screwed into the base plate and / or the skin.

[0145] Preferably, the tooling fixture used for welding the wing frame and skin also includes a rotating mechanism coaxially arranged on both sides of the base plate; the two rotating mechanisms are connected to the welding workbench, and by rotating the tooling fixture, different angles of the wing frame and skin can be welded conveniently, thereby improving the accessibility of the welding gun.

[0146] Preferably, the two rotating mechanisms ( Figure 5 The first clamp rotating mechanism 43a and the second clamp rotating mechanism 43b) are coaxially arranged on both sides of the substrate and the rotation axis is perpendicular to the first direction; more preferably, the two rotating structures are coaxially arranged at the middle position of both sides of the substrate and the rotation axis is perpendicular to the first direction.

[0147] Step S6, protecting the front and back of the weld, and welding under the protection of inert gas to obtain a combination of the wing frame and the upper and lower skins;

[0148] S61: Weld the contact parts of the second transverse member, the third transverse member, ... the N-1th transverse member and the skin in sequence from one end to the other end along the first direction; for each transverse member, weld in the same direction from one side to the other side along the second direction;

[0149] S62: weld the second longitudinal member, the M-1 longitudinal member, the third longitudinal member, the M-2 longitudinal member, etc. in sequence from both sides to the middle along the second direction to the contact portion between the 1 / 2*M longitudinal member or the 1 / 2*(M+1) longitudinal member and the skin; for each longitudinal member, weld symmetrically from both ends to the middle along the first direction;

[0150] S63: Perform lock bottom welding on the contact parts between the two longitudinal members and two transverse members on the outside of the wing frame and the skin.

[0151] Preferably, in S63, the first longitudinal member and the Mth longitudinal member are welded first, and then the first transverse member and the Nth transverse member are welded. The longitudinal member with greater rigidity is welded first, and then the transverse member with less rigidity is welded, so as to ensure the stability and accuracy of the overall structure.

[0152] The above welding sequence of S61 to S63 can allow the weld to shrink more freely, reduce welding stress and deformation, improve the stability of the welding structure, and reduce defects such as cracking and decreased joint strength caused by residual stress generated during laser welding.

[0153] Preferably, in S6, the main steps of back protection include: utilizing the wing frame with reserved ventilation holes in S2 and the upper and lower skins to form a closed and connected air path environment, and the inert gas enters from one end of the wing frame and is discharged from the other end.

[0154] In S6, the front protection adopts the drag hood + nozzle method in the prior art.

[0155] It should be noted that in S61 and S62, the preferred process parameters for penetration welding that can obtain high-quality welds include: laser power of 2000W to 2200W, defocus of -4mm to -6mm, and welding speed of 0.02m / min to 0.03m / min; illustratively, the laser power is 2100W, the defocus is -5mm, and the welding speed is 0.025m / min;

[0156] In S63, the bottom lock welding includes positioning welding and formal welding; the preferred process parameters for obtaining high-quality welds include:

[0157] Positioning welding: laser power is 700W~900W, defocus is -1.0mm~-3.0mm, and welding speed is 0.5m / min~2.5m / min; more preferably, laser power is 750W~850W, defocus is -1.5mm~-2.5mm, and welding speed is 1.0m / min~2.0m / min; the length of positioning welding is 5mm~15mm, and the weld spacing is 25mm~35mm; if the positioning welding length is too long, it may cause overheating and excessive melting of the welding area, while insufficient length may cause the positioning welding point to be loosely connected.

[0158] Formal welding: laser power is 900W~1100W, defocus is -3mm~-7mm, and welding speed is 0.5m / min~2.5m / min; more preferably, laser power is 950W~1050W, defocus is -4mm~-6mm, and welding speed is 1.0m / min~2.0m / min.

[0159] Preferably, in S4 and S6, the front protection gas flow rate is 20L / min to 40L / min, and the back protection gas flow rate is 4L / min to 6L / min; more preferably, the front protection gas flow rate is 20L / min to 30L / min; illustratively, the front protection hood gas flow rate is 25L / min; and the back protection flow rate is 5L / min.

[0160] Preferably, when welding is performed in S4 and S6, the distance between arc starting and arc extinguishing is 3 mm to 7 mm; illustratively, the distance between arc starting and arc extinguishing is 5 mm.

[0161] Preferably, in S4 and S6, after welding is completed, the inert gas protection is stopped after cooling for 15 minutes to 20 minutes; after welding is completed, gas protection (mainly back gas protection) can protect the weld metal from erosion by harmful gases in the air during the cooling process, maintaining the purity and performance of the weld metal.

[0162] It is worth noting that in S4 and S6, the above-mentioned preferred arc starting and arc extinguishing distances and welding parameters (including laser power, welding speed, defocusing amount, and shielding gas flow rate) can ensure that a smooth and uniform weld surface is formed between all welded joints, reduce welding defects, and improve the quality of welded joints; specifically,

[0163] (1) Arc starting distance: In S4 and S6, the preferred arc starting distance can ensure that the starting part of the weld can be formed sequentially and maintain a stable welding process; if the arc starting distance is too short, the welding starting point will overheat, forming a weld nodule or burn-through; and if the arc starting distance is too long, it may lead to insufficient penetration of the starting point, affecting the connection strength of the weld.

[0164] (2) Arc extinction distance: In S4 and S6, the preferred arc extinction distance is used to help maintain the continuity and uniformity of the welding process and ensure the quality of the end of the weld. If the arc extinction distance is too short, the end of the weld will overheat, forming arc crater cracks or other welding defects. If the arc extinction distance is too long, the end of the weld will cool too quickly, forming cold cracks or other microscopic defects.

[0165] (3) Laser power: In S4 and S6, the above-mentioned preferred laser power can effectively ensure that there are no defects such as pores, cracks, lack of fusion, undercuts, and depressions on the weld surface. Specifically, a. Too high laser power leads to too high a temperature in the molten pool, an increase in metal vapor, and the failure of the gas to escape from the molten pool in time, thereby forming pores; b. Too high laser power leads to too high a temperature in the molten pool, an increase in the thermal stress of the material, thereby inducing the formation of cracks; c. Insufficient laser power may result in insufficient molten pool temperature, inability to fully melt the material, resulting in lack of fusion; d. Too high laser power leads to too high a temperature in the molten pool, an expansion of the melting range, and an easy occurrence of undercuts; e. Too high laser power may result in too high a temperature in the center of the molten pool, and the metal in the center of the molten pool solidifies before the edge, forming depressions.

[0166] (4) Defocus: In S4 and S6, the above-mentioned preferred defocus can effectively ensure that there are no defects such as pores, cracks, lack of fusion, undercuts, and depressions on the weld surface. Specifically, a. Too much or too little defocus will result in an irregular shape of the molten pool, poor gas discharge, and increased risk of pores. b. Too much or too little defocus will result in uneven cooling of the molten pool and stress concentration in local areas, increasing the possibility of cracks. c. Too much defocus will result in uneven distribution of laser energy, too high temperature at the center of the molten pool and insufficient temperature at the edge, which may easily cause lack of fusion. d. Too much or too little defocus will result in inconsistent cooling speed at the edge of the molten pool, which may easily cause undercuts. e. Too much or too little defocus will result in uneven cooling of the molten pool, which may easily cause depressions.

[0167] (5) Welding speed: In S4 and S6, the above-mentioned preferred welding speed can effectively ensure that there are no defects such as pores, cracks, lack of fusion, undercuts, and depressions on the weld surface. Specifically, a. Welding speed that is too fast may cause the molten pool to cool too quickly, and the gas cannot escape sufficiently, which may easily form pores. b. Welding speed that is too slow may cause the molten pool to be in a high temperature state for a long time, increasing the thermal stress of the material and thus increasing the risk of cracks. c. Welding speed that is too fast may cause the molten pool to cool too quickly, and the material cannot be fully melted, which may easily lead to lack of fusion and undercuts. d. Welding speed that is too fast may cause the metal in the center of the molten pool to fail to be fully filled, forming depressions.

[0168] (6) Shielding gas flow rate: In S4 and S6, the above-mentioned preferred gas flow rate is used to protect the front and back of each weld, which can effectively prevent oxidation and inclusions in the weld area, ensure the stability and uniformity of the molten pool, and avoid defects such as pores. Too low a gas flow rate cannot provide sufficient protection, resulting in weld oxidation; while too high a gas flow rate will interfere with the stability of the molten pool and affect the formation of the weld.

[0169] Preferably, in steps S3 and S5, the assembly includes: trial assembly, repair and trial assembly to meet the assembly tolerance requirements, and marking matching marks on each component; pickling to remove oxide scale and improve welding quality; formal assembly: after pickling, assemble the components in sequence according to the matching marks on each component, and clamp them with tooling fixtures to ensure that the assembly tolerance requirements are met.

[0170] Preferably, in steps S3 and S5, the assembly tolerance requirements include: the butt gap and step difference at each point of each joint are not greater than 0.1 mm, and the butt gap and step difference with a cumulative length of no more than 30 mm within any local 100 mm are not greater than 0.2 mm.

[0171] Preferably, before trial assembly, the area to be welded is pretreated until the metallic luster is exposed and the surface roughness of the surface to be welded is Ra≤3.2 μm.

[0172] Specifically, the pretreatment mainly includes processing the area to be welded by machining finishing; specifically, the surface to be welded is processed by mechanical processing method to ensure flatness, smoothness, burr-free, and maintain edges and corners. The surface roughness of the surface to be welded after processing is Ra≤3.2μm; the area to be welded is cleaned by mechanical processing method to remove surface oil, non-metallic impurities, etc. until the metallic luster is exposed; wherein, the area to be welded includes the surface to be welded and both sides of the weld; non-metallic impurities include oxides.

[0173] Optionally, the area to be welded includes 10 mm to 30 mm on both sides of the weld; preferably, 20 mm on both sides of the weld.

[0174] Optionally, the above-mentioned machining methods include but are not limited to milling, grinding, scraping, lapping, super finishing, and polishing.

[0175] Optionally, the mechanical treatment method includes mechanical grinding. Exemplarily, the tools for mechanical grinding include but are not limited to wire brushes, sandpaper, and files.

[0176] It can be understood that by pre-treating the area to be welded (including the surface to be welded), the quality and reliability of the welded joint can be ensured.

[0177] Preferably, in steps S4 and S6, chord plane measurement and shape correction are performed before and after welding, respectively.

[0178] It should be noted that the main steps of chord plane measurement include: selecting a suitable chord plane measuring device; using the chord plane measuring device to scan along the chord length direction of the wing frame, wing frame and skin assembly, and recording data points; inputting the collected data into computer-aided design (CAD) software for data analysis to generate a chord plane three-dimensional model of the wing frame, wing frame and skin assembly before and after welding.

[0179] Optionally, the chord plane measuring device includes at least one of a laser scanner and a laser tracker.

[0180] Furthermore, the 3D models of the chord plane before and after welding are compared to obtain the position and amount of deformation points, and the wing frame, wing frame and skin assembly are calibrated to further eliminate minor deformations during laser welding.

[0181] Optionally, the shaping method includes one or a combination of mechanical shaping, thermal shaping, cold shaping, and CNC shaping. Among them, mechanical shaping includes but is not limited to manual shaping, pressure shaping, and stretching shaping; thermal shaping includes but is not limited to local heating and overall heating; cold shaping includes but is not limited to cooling shrinkage and cold stretching; CNC shaping includes but is not limited to CNC shaping and robot shaping.

[0182] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments.

[0183] Embodiment 1:

[0184] This embodiment provides a method for welding a TA15 titanium alloy wing frame and skin, comprising the following steps:

[0185] S1: Design of fixture for welding wing frame;

[0186] See also Figure 1-Figure 5 The wing skeleton 100 includes a first main beam 11, a second main beam 12, and a third main beam 13 distributed in parallel along a first direction, and a first cross beam (not shown in the figure), a second cross beam, a third cross beam, and a fourth cross beam (not shown in the figure) distributed in parallel along a second direction; wherein the second cross beam includes a first cross rib 14 and a second cross rib 15 distributed in a straight line, and the third cross beam includes a third cross rib 16 and a fourth cross rib 17 distributed in a straight line; the angle between the first direction and the second direction is 87°.

[0187] The main beam and transverse reinforcement are made of TA15 titanium alloy, and both are hollow structure rods with a wall thickness of 3mm and an I-shaped cross-section; the skin is made of TA15 titanium alloy with a wall thickness of 2mm.

[0188] The fixture 200 for welding the wing frame includes a base plate, a positioning mechanism, a clamping mechanism, a side pressure mechanism, a pushing mechanism, and two rotating mechanisms 23a and 23b symmetrically and coaxially distributed in the middle of both sides of the base plate.

[0189] The substrate is in the shape of a grid-shaped thin plate, and each grid includes a quadrilateral or cross-shaped hollow structure;

[0190] The positioning mechanism includes two positioning pins 21 located on the base plate;

[0191] Each clamping mechanism 22a includes a long clamping strip with inner holes at both ends for screws to pass through and be screwed into the base plate;

[0192] Each side pressure mechanism 22b includes a rectangular pressing piece, and the part of the pressing piece that does not contact the main beam or the transverse rib has two inner holes for screws to pass through and be screwed into the base plate;

[0193] Each push mechanism 22c includes a push block and a mounting seat. The push block includes a push rod and an end pressure portion connected to each other. The mounting seat is fixed on the base plate. The outer surface of the push rod is provided with a thread that matches the thread of the inner hole of the mounting seat. The end pressure portion is driven to abut against the side wall of the main beam by rotating the push rod.

[0194] Step S2, using a selective laser melting (SLM) method to manufacture all the main beams and transverse ribs of the wing skeleton 100 in S1;

[0195] Among them, when establishing a 3D printed model, the first main beam 11 and the third main beam 13 each include four connecting ends on one side, and the second main beam 12 includes four connecting ends on both sides, which can be connected one by one with the two end faces of 8 transverse ribs (four transverse ribs are not shown in the figure) to form 16 butt joints; the inner sides of the first main beam 11, the third main beam 13, the first cross beam, and the fourth cross beam include step grooves with a height of 2 mm; ventilation holes 18 are reserved on the second main beam 12 and the first cross rib 14, the second cross rib 15, the third cross rib 16, and the fourth cross rib 17 to connect the six grid structures.

[0196] Step S3, assembling all the main beams and transverse ribs of the wing skeleton printed in S2 on the fixture 200;

[0197] S31: The two lugs on the right side of the first main beam 11 are matched and positioned with the two positioning pins 21 on the base plate; a side pressure mechanism 22b is respectively provided at 1 / 4 and 3 / 4 of the first main beam 11 between any two adjacent butt joints, and a clamping mechanism 22a is provided at 1 / 2;

[0198] S32: assemble four transverse ribs on the base plate in sequence from the upper end to the lower end of the first main beam 11, and set a side pressure mechanism 22b at 1 / 3 and 2 / 3 of each transverse rib respectively;

[0199] S33: assembling the second main beam 12 on the base plate, and providing two side pressure mechanisms 22b distributed face to face at a position 2 / 5 between any two adjacent butt joints of the second main beam 12;

[0200] Repeat S32 to sequentially assemble four transverse ribs between the second main beam 12 and the third main beam 13;

[0201] S34: Assemble the third main beam 13 on the base plate, and respectively set a side pressure mechanism 22b at 1 / 4 and 3 / 4 of the third main beam 13 between any two adjacent butt joints, and set a clamping mechanism 22a at 1 / 2; set a push mechanism 22c on the outside of the third main beam 13 and facing each butt joint.

[0202] Furthermore, after assembly, the wing skeleton is measured in the chord plane using a laser scanner; the collected data is input into Geomagic Control X software to generate a 3D model of the wing skeleton in the chord plane before welding.

[0203] Step S4, using 3M tape to bond the main beam and / or transverse reinforcement near the back of each butt joint to form a sealing cover in situ, punching holes in the lower part of the sealing cover and introducing argon gas, punching holes in the upper part to form an argon gas outlet, and protecting the back of the weld; the front protection adopts the method of dragging a cover + nozzle in the prior art for protection;

[0204] With argon gas protecting the front and back of the weld, a laser welding device (name: large-size three-dimensional multi-layer curved surface high-power and high-precision laser welding equipment, manufacturer: Aerospace Sanjiang Laser) was used to perform positioning welding on 16 butt joints in order from top to bottom and from left to right, and then formal welding was carried out.

[0205] The above-mentioned positioning welding includes: first finding the welding trajectory, that is, ensuring that the laser spot is located in the middle of the weld; selecting the middle part of each butt joint for positioning welding, the positioning welding length is 10mm, and the process parameters of positioning welding include: laser power is 800W, defocus is -2mm, and welding speed is 1.5m / min.

[0206] The parameters of formal welding include: laser power is 1900W, defocus is -5mm, welding speed is 1.5m / min; arc starting and arc extinguishing distance is 5mm.

[0207] After the formal welding is completed, the argon gas for back protection is stopped after cooling for 20 minutes. The chord plane of the welded wing skeleton is measured by a laser scanner. The collected data is input into Geomagic Control X software to generate a 3D model of the chord plane of the welded wing skeleton. The 3D models of the chord plane of the wing skeleton before and after welding are compared to obtain the position and amount of deformation points. Cold correction is performed by hot correction and tapping with tools such as rubber wood hammer to correct the remaining minor deformation.

[0208] Step S5, assembling the wing frame and the skin to be welded obtained in S4 on a fixture for welding the wing frame and the skin; specifically comprising the following steps:

[0209] S51: Assemble the wing frame on the base plate, and respectively set a frame side pressure mechanism 42 at the 1 / 4 position and the 3 / 4 position between any two adjacent butt joints of the first main beam 11 and the third main beam 13 of the wing frame;

[0210] S52: Overlap the upper and lower skins on the step groove of the wing frame, and set 6 skin clamping mechanisms 41 at the contact parts of the second main beam 12, the second cross beam and the third cross beam with the upper skin and the lower skin; ensure that the skin is fixed and clamped on the fixture, and the skin forms a butt joint with the wing frame with a flush surface all around.

[0211] Step S6: Before welding, a laser scanner is used to measure the chord plane of the assembled wing frame and skin; the collected data is input into Geomagic Control X software to generate a chord plane three-dimensional model of the wing frame and skin assembly before welding;

[0212] Argon is used to protect the front and back of the weld. The wing frame and the upper and lower skins with reserved vents 18 form a relatively closed and connected gas path environment. Argon enters from the fourth beam at the bottom of the wing frame and is discharged from the first beam at the top of the wing frame to protect the back of the weld. The front is protected by a drag hood + nozzle method in the prior art.

[0213] Under the protection of argon gas, welding is performed in the following order to obtain a combination of the wing frame and the upper and lower skins;

[0214] S61 and S62: Figure 4 , perform penetration welding on the contact parts between the third cross beam, the second cross beam, the second main beam 12 and the skin in the order of ①-⑤;

[0215] S63: Figure 4 , weld the third main beam 13 and the first main beam 11 in the order of ⑥-⑦, and then weld the first cross beam at the top and the fourth cross beam at the bottom (not shown in the figure).

[0216] In S61 and S62, the laser power was 2100 W, the defocus was -5 mm, and the welding speed was 0.025 m / min;

[0217] In S63, positioning welding: laser power is 800W, defocus is -2mm, welding speed is 1.5m / min, positioning welding length is 10mm, weld spacing is 30mm; formal welding: laser power is 1000W, defocus is -5mm, welding speed is 1.5m / min, arc starting and arc extinguishing distance is 5mm.

[0218] In S4 and S6, the gas flow rate of the hood for front protection is 25L / min; the gas flow rate for back protection is 5L / min.

[0219] In S6, after the formal welding is completed, the argon gas for back protection is stopped after cooling for 20 minutes; the chord plane of the welded wing frame and skin assembly is measured by a laser scanner; the collected data is input into Geomagic Control X software to generate a 3D model of the chord plane of the welded assembly; the 3D models of the chord plane of the assembly before and after welding are compared to obtain the position and amount of deformation points, and cold shaping is performed by hot shaping and tapping with tools such as rubber wood hammers to correct the remaining minor deformations.

[0220] Implementation results:

[0221] 1. Chord plane measurement shows that the welding deformation of the wing frame, wing frame and skin assembly can be controlled below ±0.5%. Figure 6 As shown; this shows that the method provided by the present invention can significantly reduce welding deformation, thereby reducing residual stress and cracking problems, and improving welding quality; and because the welding deformation is very small, little or no correction is required to meet the standard requirements, thereby achieving cost reduction and efficiency improvement.

[0222] 2. Visual inspection or inspection with a magnifying glass of 10 times or less shall be conducted on the weld appearance quality. The results shall show that the weld surface of the wing frame and the combination of the wing frame and the skin obtained by welding shall be free of defects such as oxidation, inclusions, pores, cracks, lack of fusion, undercut, depression, etc. Figure 7 shown.

[0223] 3. X-ray nondestructive testing shows that the weld quality of the wing frame, wing frame and skin assembly fully meets the requirements of Grade I welds in QJ20465-2016 (Technical requirements for laser welding of titanium and titanium alloys). Figure 8 As shown;

[0224] 4. Take room temperature tensile specimens from the welds and test the mechanical properties of the joints at room temperature. The results show that the room temperature tensile strength of the welds of the wing frame, wing frame and skin combination obtained by welding can reach more than 95% of the base material; for example, Figure 1 The tensile strength of the four joints ①-④ is 900Mpa~912Mpa, and the tensile strength of the base material is about 930Mpa.

[0225] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.

Claims

1. A method for welding a wing frame and a skin, characterized in that: The following steps are involved: S1. Design of fixture for welding wing frame; The wing skeleton is a thin-walled grid structure, which is mainly formed by M longitudinal members parallel to the first direction and N transverse members parallel to the second direction through M×N nodes, and each transverse member contains M-1 transverse ribs; M≥3, N≥3; the first direction is different from the second direction; The tooling fixture of the wing frame includes: a base plate, a positioning mechanism and a clamping mechanism arranged on the base plate; S2. All longitudinal members and transverse ribs of the wing skeleton are manufactured by 3D printing; wherein, when establishing a 3D printed model, the M longitudinal members are designed to include 2×N×(M-1) connecting ends along the second direction to precisely connect with the two end faces of each transverse rib to form 2×N×(M-1) butt joints; the inner side edges of the longitudinal members and transverse members located at the outermost side of the wing skeleton are designed to include step grooves with the same thickness as the skin; ventilation holes are reserved on the longitudinal members and transverse ribs located inside the wing skeleton to connect each grid structure; S3. Assemble all longitudinal components and transverse ribs on the fixture, and control welding deformation and meet assembly tolerance requirements through reasonably designed positioning and clamping mechanisms; S4. Protect the front and back sides of the weld. Under the protection of inert gas, weld 2×N×(M-1) butt joints of the wing skeleton in sequence from one end to the other end in the first direction and from one side to the other side along the second direction to obtain the wing skeleton.

2. The method for welding a wing frame and a wing skin according to claim 1, characterized in that: S3 specifically includes the following steps: S31: cooperating and positioning the first longitudinal member with the positioning mechanism, and providing a clamping mechanism at a 1 / 5 to 4 / 5 section of the first longitudinal member between any two adjacent butt joints; S32: assembling N transverse ribs on the base plate in sequence from one end to the other end of the first longitudinal member, and providing a clamping mechanism at a 1 / 3 to 2 / 3 section of each transverse rib; S33: assembling the second longitudinal member on the base plate, and providing a clamping mechanism at a 1 / 5 to 4 / 5 section of the second longitudinal member between any two adjacent butt joints; Repeat S32 and S33 alternately to assemble the third longitudinal member to the M-1 longitudinal member and the remaining transverse reinforcements; S34: Assemble the Mth longitudinal member on the base plate; set a clamping mechanism in the 1 / 5 to 4 / 5 section of the Mth longitudinal member between any two adjacent butt joints, and set a clamping mechanism on the outside of the Mth longitudinal member and directly opposite to each butt joint.

3. The method for welding a wing frame and a wing skin according to claim 1, characterized in that: In S1, the angle between the first direction and the second direction is 85° to 95°.

4. The method for welding a wing frame and a wing skin according to claim 1, characterized in that: In S1, the cross-sectional shape of the longitudinal member and the transverse rib is an I-shaped or Π-shaped or a combination thereof; and / or the wall thickness of the longitudinal member and the transverse rib is 2 mm to 10 mm.

5. The method for welding a wing frame and a wing skin according to claim 1, characterized in that: The following steps are also included: S5, assembling the wing frame and the skin to be welded obtained in S4 on a fixture for welding the wing frame and the skin; controlling welding deformation and meeting assembly tolerance requirements through a reasonably designed frame side pressure mechanism and skin pressing mechanism on the fixture; comprising the following steps: S51: Assemble the wing frame on the fixture, and set two frame side pressure mechanisms between any two adjacent butt joints of the first longitudinal member and the Mth longitudinal member; S52: overlap the upper and lower skins on the step groove described in S2, and set 2×(M+N-4) skin clamping mechanisms on the outer sides of the upper and lower skins and along the contact parts of the M-2 longitudinal members and N-2 transverse members in the wing frame with the upper and lower skins to ensure that the skins are fixed and clamped on the fixture, and that the skins are surrounded by the wing frame to form a butt joint with a flush surface; each skin clamping mechanism is provided with a groove of a size that can accommodate the contact surface of the corresponding longitudinal member or transverse member with the skin; S6, protecting the front and back of the weld, welding under the protection of inert gas, to obtain a combination of the wing frame and the upper and lower skins; comprising the following steps: S61: Weld the contact parts of the second transverse member, the third transverse member, ... the N-1th transverse member and the skin in sequence from one end to the other end along the first direction; for each transverse member, weld in the same direction from one side to the other side along the second direction; S62: weld the second longitudinal member, the M-1 longitudinal member, the third longitudinal member, the M-2 longitudinal member, etc. in sequence from both sides to the middle along the second direction to the contact portion between the 1 / 2*M longitudinal member or the 1 / 2*(M+1) longitudinal member and the skin; for each longitudinal member, weld symmetrically from both ends to the middle along the first direction; S63: Perform lock bottom welding on the contact parts between the two longitudinal members and two transverse members on the outside of the wing frame and the skin.

6. The method for welding a wing frame and a wing skin according to claim 1 or 5, characterized in that: In S4, the main steps of back side protection include: on the back side of each butt joint, a sealing cover is built in situ with a flexible sealing material, and holes are opened in the sealing cover to form an inlet and an outlet for an inert gas; and / or, In S6, the main steps of the back protection include: using the wing frame with reserved ventilation holes in S2 and the upper and lower skins to form a closed and connected air path environment, and the inert gas enters from one end of the wing frame and is discharged from the other end.

7. The method for welding a wing frame and a wing skin according to claim 1 or 5, characterized in that: In S3 and S5, the assembly tolerance requirements include: the butt joint gap and step difference at each point of each joint are not greater than 0.1 mm, and the butt joint gap and step difference with a cumulative length of no more than 30 mm within any local 100 mm are not greater than 0.2 mm.

8. The method for welding a wing frame and a wing skin according to claim 1 or 5, characterized in that: In steps S4 and S6, chord plane measurements are performed before and after welding, respectively, and shape correction is performed by comparing the chord plane measurement results.

9. The method for welding a wing frame and a wing skin according to claim 1 or 5, characterized in that: In steps S3 and S5, the assembly includes trial assembly, repair trial assembly, pickling, removing oxide scale, and formal assembly.

10. The method for welding a wing frame and a wing skin according to claim 9, characterized in that: Also includes: Before the trial assembly, the area to be welded is pretreated until the metallic luster is exposed and the surface roughness Ra of the surface to be welded is ≤3.2 μm.

Citation Information

Patent Citations

  • Laser welding method for large-size thin-wall weakly rigid titanium alloy rudder wing structure

    CN108672935A

  • Framework stressed-skin structure laser welding assembly tool

    CN109277756A

  • High-energy-beam welding assembly tool and method for lightweight wing rudder component

    CN112643234A

  • Laser welding tool and welding method for skin skeleton structure rudder wing product

    CN113523571A

  • Integral structural shell component for an aircraft and method of manufacturing the same