Method for processing silicon carbide positioning edge, silicon carbide crystal with positioning edge and application of silicon carbide crystal
Through XRD orientation and micro jet water-conducting laser processing, the problems of inaccurate and low efficiency of silicon carbide crystal positioning edge processing caused by mechanical grinding are solved, and efficient and accurate positioning edge processing is achieved, improving product quality and production efficiency.
Patent Information
- Application Number
- CN202411072332.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
AI Technical Summary
The existing silicon carbide crystal processing methods rely on mechanical grinding, resulting in inaccurate positioning edge processing, low production efficiency, large material loss, poor product quality, and defects caused by mechanical stress reduce the product yield and aesthetics.
XRD is used to orient the silicon carbide crystals, and the positioning edge processing is carried out through micro jet water-conducting laser to avoid material waste and defect introduction, improve processing accuracy and efficiency, and detect the orientation accuracy in real time to ensure the smooth processing of the positioning edges.
It improves the processing accuracy and efficiency of positioning edges, reduces material losses and production costs, improves the surface quality and yield of products, and is suitable for industrial production.
Smart Images

Figure CN118989629A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a method for processing a silicon carbide positioning edge, a silicon carbide crystal with a positioning edge and an application thereof, and belongs to the technical field of silicon carbide processing. Background Art
[0002] Silicon carbide is a semiconductor material with excellent performance, which is widely used in the field of high-power, high-frequency and high-temperature electronic devices. With the development of silicon carbide technology, its application in power electronics, optoelectronic devices and high-temperature devices has been continuously expanded, and higher requirements have been put forward for the quality and processing technology of silicon carbide crystal materials. However, the current silicon carbide crystal processing methods have many shortcomings, which restrict the improvement of its production efficiency and product quality.
[0003] The existing silicon carbide crystal processing method mainly relies on mechanical grinding technology, and the specific steps include rough rolling, orientation, flat grinding, fine rolling, positioning edge processing, etc. Each of these steps requires precise operation and repeated adjustments, especially the positioning edge as the last processing step, which will directly affect the factory quality of the crystal. If the positioning edge is deviated, the production quality of the epitaxial wafer will be significantly reduced.
[0004] However, in the above mechanical grinding process, due to the "hard-on-hard" grinding method, even if the initial orientation position is accurate, the crystal will be offset during the processing of the positioning edge, so orientation deviation will inevitably occur, thereby reducing the accuracy of the positioning edge processing. If the orientation method is repeated at a certain interval during the processing of the positioning edge, the overall processing time will be too long, which will seriously affect the production efficiency, and repeated rest of the positioning edge will lead to poor surface quality and reduce the aesthetics of the product.
[0005] Mechanical grinding will inevitably introduce mechanical stress, which not only easily damages the internal structure of the silicon carbide crystal, but also may cause defects such as cracks and edge collapse. These defects significantly reduce the yield of silicon carbide crystals, thereby affecting the performance and stability of subsequent applications. In addition, a large amount of silicon carbide debris is generated during mechanical grinding, which not only increases material loss and production costs, but also has a negative impact on the environment. Summary of the invention
[0006] In order to solve the above problems, a method for processing a silicon carbide positioning edge is provided. The method uses XRD to orient the silicon carbide crystal and then processes the positioning edge through a micro-jet water-guided laser. This processing method can firstly avoid material waste and the introduction of new defects into the crystal. Second, it can improve the processing accuracy, avoid crystal deviation during processing, and improve the processing efficiency and processing accuracy of the positioning edge. Third, the accuracy of the orientation can be detected in real time during the processing, thereby ensuring the smooth processing of the positioning edge.
[0007] According to one aspect of the present application, a method for machining a silicon carbide positioning edge is provided, comprising the following steps:
[0008] (1) Fixing the silicon carbide crystal;
[0009] (2) Use XRD to orient the (0004) or (11-28) crystal plane of the silicon carbide crystal. First, adjust the incident angle θ1 and the exit angle θ2 of the X-ray, and then rotate and align the silicon carbide crystal around the vertical center line. Scanning, until the position of maximum diffraction intensity is stopped, then the silicon carbide crystal is rotated with the horizontal center line as the axis and χ scanning is performed until the position of maximum diffraction intensity is rotated, and finally the silicon carbide crystal is continued to be rotated with the horizontal center line as the axis, and the χ value is adjusted according to the required crystal deflection angle;
[0010] (3) A microjet water-guided laser is used to mark the positioning edge on the (1-100) crystal plane of the crystal to form a positioning edge.
[0011] In step (2), the silicon carbide crystal is rotated and rotated about the vertical center line. Scan until it rotates to the position with the maximum diffraction intensity and stops, adjust the crystal rod to the initial deflection direction, then rotate the silicon carbide crystal around the horizontal center line and perform χ scanning until it rotates to the position with the maximum diffraction intensity, in order to adjust the upper surface of the silicon carbide crystal to the initial reference plane, at which time the crystal deflection is 0°, then continue to rotate around the horizontal center line, adjusting the χ value while adjusting the crystal deflection until it is adjusted to the desired deflection.
[0012] Optionally, when orienting the (0004) plane of the crystal in step (2), the incident angle θ1 and the exit angle θ2 of the X-ray are both 17.85°±0.1°.
[0013] Optionally, when the (0004) crystal plane is used for orientation in step (2), the process further includes the following steps between rotating to the position where the diffraction intensity is maximum and finally continuing to rotate the silicon carbide crystal around the horizontal center line:
[0014] Stop the rotation about the horizontal center line, then rotate the silicon carbide crystal 90° or 270° about the vertical center line, continue to rotate about the horizontal center line and perform χ scanning until it rotates to the position of the maximum diffraction intensity at this time.
[0015] Due to the orthogonal orientation deviation after crystal growth, rotating the silicon carbide crystal around the horizontal center line and performing a χ scan until the position with the maximum diffraction intensity is not the actual signal strongest position. Therefore, rotating the silicon carbide crystal 90° or 270° around the vertical center line, and then rotating and χ scanning around the horizontal center line can correct the error of the previous χ scan and obtain the true signal strongest position.
[0016] Optionally, when orienting the crystal (11-28) plane in step (2), the incident angle θ1 and the exit angle θ2 of the X-ray are adjusted to 9°±0.1° and 96°±0.1°, respectively.
[0017] Optionally, in step (2), the rotation angle of the silicon carbide crystal around the horizontal center line is -10° to 10°.
[0018] Optionally, the required crystal deflection angle ranges from 1° to 8°, for example, 1°, 2°, 3°, 4°, 5°, 6°, 7°, 8° and any angle therebetween.
[0019] Optionally, the power of the micro-jet water-guided laser is 15 to 200 W, and the frequency is 6 to 10 kHz.
[0020] The power and frequency of the micro-jet water-guided laser directly affect the cutting ability of the silicon carbide crystal, thereby affecting the processing efficiency and processing quality of the positioning edge. If the power and frequency are too small, the processing efficiency of the positioning edge will decrease, which is not conducive to large-scale production; if the power and frequency are too large, although the processing efficiency is improved, it will cause edge collapse or crystal cracking during the processing of the positioning edge, reducing the product yield.
[0021] Optionally, the microjet water-guided laser is emitted through a beam coupler, the water pressure of the beam coupler is 150 to 500 bar, and the gas flow rate is 0.2 to 1 L / min.
[0022] Optionally, the water is ultrapure water, and the gas is nitrogen or helium.
[0023] The water pressure is related to the effective cutting length of the microjet water-guided laser. The water pressure is adapted to the power of the microjet laser, and improves the processing efficiency, the surface quality and yield of the processed crystal. The higher the water pressure, the longer the effective cutting length, and the higher the processing efficiency. However, too high water pressure can also cause damage to the silicon carbide crystal, reducing the surface quality and yield of the product.
[0024] As the gas flow rate increases, the processing efficiency will also increase. However, too large a gas flow rate will cause gas waste and also deteriorate the surface quality of the crystal.
[0025] Preferably, the water pressure is P1, the unit is bar, the gas flow rate is P2, the unit is L / min, and P1 and P2 satisfy the following relationship:
[0026] P1 / 1000≤P2≤P1 / 500.
[0027] The water jet is surrounded by coaxial protective gas, and the water-gas interface is maintained by controlling the gas flow rate, which can reduce the interference of the surrounding atmosphere and increase the coherence length of the water jet.
[0028] Optionally, the inner diameter of the nozzle of the beam coupler is 30-120 μm.
[0029] Optionally, the relative cutting speed of the micro-jet water-guided laser is 100-1000 mm / min.
[0030] Optionally, in step (1), the silicon carbide crystal is fixed on a base, and the base is used to realize the rotation of the silicon carbide crystal around the vertical center line and the horizontal center line.
[0031] According to another aspect of the present application, there is provided a silicon carbide crystal with a positioning edge obtained by processing according to any one of the methods described above.
[0032] According to another aspect of the present application, there is provided application of any of the methods described above in silicon carbide processing.
[0033] The beneficial effects of this application include but are not limited to:
[0034] 1. The method for processing silicon carbide positioning edges of the present application adopts micro-jet water-guided laser for positioning edge processing, which can improve the surface quality of the positioning edge while improving the processing efficiency, reduce the silicon carbide debris generated during the processing, thereby reducing material loss, production costs and environmental impact.
[0035] 2. The method of processing silicon carbide positioning edges of the present application adopts XRD and micro-jet water-guided laser to process the positioning edges, which can improve the processing accuracy and precision of the positioning edges, and detect the orientation accuracy during the processing, achieving the effect of instant processing and instant feedback.
[0036] 3. In the method of processing silicon carbide positioning edges of the present application, the processing parameters of the micro-jet water-guided laser cooperate with each other to achieve a coordinated improvement in processing efficiency, surface quality after processing and product yield.
[0037] 4. The method for processing silicon carbide positioning edges of the present application obtains positioning edges with clear boundaries and no fractures or interfaces, thereby improving the aesthetics of the product and being suitable for industrial production and processing. The positioning edges of silicon carbide crystals obtained by batch production have good consistency. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0039] Figure 1 It is a schematic diagram of a processing device for silicon carbide positioning edge involved in the present application.
[0040] Figure 2 It is a side cross-sectional schematic diagram of a beam coupler involved in an embodiment of the present application.
[0041] Figure 3 This is a morphology diagram of the Notch positioning edge of the silicon carbide crystal prepared in Example 1 of the present application.
[0042] List of parts and reference numerals:
[0043] 1. Base; 2. X-ray emitting unit; 3. X-ray receiving unit; 4. Beam coupler; 41. Laser emitting unit; 42. Protective window; 43. Water inlet; 44. Nozzle; 45. Air inlet; 46. Microjet water-guided laser; 5. Silicon carbide crystal. DETAILED DESCRIPTION
[0044] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0045] Unless otherwise specified, the raw materials in the examples and comparative examples of the present application were purchased through commercial channels.
[0046] Unless otherwise specified, the methods used in the examples and comparative examples of the present application are conventional methods in the prior art.
[0047] The processing device used in the following embodiments and comparative examples for processing the silicon carbide positioning edge is as follows: Figure 1 and Figure 2 , which includes:
[0048] A base 1, the base 1 is used to place a silicon carbide crystal 5;
[0049] The XRD orientation mechanism comprises an X-ray emitting unit 2, an X-ray receiving unit 3 and a signal intensity monitoring unit;
[0050] The beam coupler 4 includes a laser emitting part 41, a protective window 42, a water inlet 43, a nozzle 44 and an air inlet 45 from top to bottom. The laser emitting part 42 is used to emit laser light. The water inlet 43 and the air inlet 45 are both arranged on the side of the beam coupler 4. Water and gas enter through the water inlet 43 and the air inlet 45 to realize the emission of the micro-jet water-guided laser 46.
[0051] The driving mechanism is used to drive the silicon carbide crystal and the beam coupler to move relative to each other.
[0052] In the following embodiments and comparative examples, specific components in the above-mentioned processing device are no longer numbered. During the orientation process, the silicon carbide crystal is driven by the base to rotate about the vertical center line and the horizontal center line. The specific rotation method can be manually operated or controlled by a control structure already available in the prior art, and the details will not be repeated.
[0053] Example 1
[0054] This embodiment relates to a method for processing a silicon carbide positioning edge, comprising the following steps:
[0055] (1) Fixing the silicon carbide crystal on a base;
[0056] (2) XRD was used to orient the (11-28) crystal plane of the silicon carbide crystal. The incident angle θ1 and the exit angle θ2 of the X-ray were adjusted to 9°±0.1° and 96°±0.1°, respectively. The silicon carbide crystal was then rotated and oriented about the vertical center line. Scan until the position with the maximum diffraction intensity value is stopped, marked as the strongest signal point 1, then the silicon carbide crystal is rotated with the horizontal center line as the axis and χ scan is performed, the rotation angle is -10°~10°, until it is rotated to the position with the maximum diffraction intensity, marked as the strongest signal point 2, and finally the silicon carbide crystal is continued to be rotated with the horizontal center line as the axis, and the χ value is adjusted according to the crystal deflection angle 1°;
[0057] (3) A micro-jet water-guided laser is used to mark the positioning edge in the form of Notch on the (1-100) crystal plane of the crystal to form a positioning edge. The inner diameter of the nozzle of the beam coupler is 30 μm, the water pressure is 150 bar, the gas flow rate is 0.2 L / min, the power of the micro-jet water-guided laser is 15 W, the frequency is 6 kHz, and the relative cutting speed is 1000 mm / min.
[0058] The morphology of the Notch positioning edge of the prepared silicon carbide crystal is shown in Figure 3 It can be seen that the positioning edge has a clear boundary without fractures or interfaces, and does not damage the silicon carbide crystal, and no edge collapse or cracks occur.
[0059] Example 2
[0060] This embodiment relates to a method for processing a silicon carbide positioning edge, comprising the following steps:
[0061] (1) Fixing the silicon carbide crystal on a base;
[0062] (2) XRD was used to orient the (0004) crystal plane of the silicon carbide crystal. The incident angle θ1 and the exit angle θ2 of the X-ray were first adjusted to 17.85°±0.1°. The silicon carbide crystal was then rotated and oriented about the vertical center line. Scan until it rotates to The position of the maximum value is stopped, marked as the strongest signal point 1, and then the silicon carbide crystal is rotated and χ scanned with the horizontal center line as the axis, and the rotation angle is -10° to 10°, until it is rotated to the position of the maximum diffraction intensity, marked as the strongest signal point 2, and finally the silicon carbide crystal is continued to be rotated with the horizontal center line as the axis, and the χ value is adjusted according to the crystal deflection angle of 8°;
[0063] (3) A micro-jet water-guided laser is used to mark the (1-100) crystal plane of the crystal in the form of a Notch to form a positioning edge. The inner diameter of the nozzle of the beam coupler is 120 μm, the water pressure is 500 bar, the gas flow rate is 1 L / min, the power of the micro-jet water-guided laser is 200 W, the frequency is 10 kHz, and the relative cutting speed is 100 mm / min.
[0064] Example 3
[0065] This embodiment relates to a method for processing a silicon carbide positioning edge, comprising the following steps:
[0066] (1) Fixing the silicon carbide crystal on a base;
[0067] (2) XRD was used to orient the (0004) crystal plane of the silicon carbide crystal. The incident angle θ1 and the exit angle θ2 of the X-ray were first adjusted to 17.85°±0.1°. The silicon carbide crystal was then rotated and oriented about the vertical center line. Scan until it rotates to the position of the maximum diffraction intensity and stops, marking it as the strongest signal point 1, then rotate the silicon carbide crystal with the horizontal center line as the axis and perform χ scanning, the rotation angle is -10°~10°, until it rotates to the position of the maximum diffraction intensity, marked as the strongest signal point 2, then rotate the silicon carbide crystal with the vertical center line as the axis 90° or 270°, continue to rotate with the horizontal center line as the axis and perform χ scanning, until it rotates to the position of the maximum diffraction intensity at this time, marked as the strongest signal point 3, finally continue to rotate the silicon carbide crystal with the horizontal center line as the axis, and adjust the χ value according to the crystal deflection angle of 8°;
[0068] (3) A micro-jet water-guided laser is used to mark the (1-100) crystal plane of the crystal in the form of a Notch to form a positioning edge. The inner diameter of the nozzle of the beam coupler is 60 μm, the water pressure is 300 bar, the gas flow rate is 0.4 L / min, the power of the micro-jet water-guided laser is 120 W, the frequency is 8 kHz, and the relative cutting speed is 400 mm / min.
[0069] Example 4
[0070] The difference between this embodiment and embodiment 3 is that the power of the micro jet water-guided laser is 220 W, and the rest is the same as embodiment 3.
[0071] Example 5
[0072] The difference between this embodiment and embodiment 3 is that the frequency of the micro-jet water-guided laser is 12 kHz, and the rest is the same as embodiment 3.
[0073] Example 6
[0074] The difference between this embodiment and embodiment 3 is that the water pressure is 80 bar, and the rest is the same as embodiment 3.
[0075] Example 7
[0076] The difference between this embodiment and embodiment 3 is that the water pressure is 400 bar, and the rest is the same as embodiment 3.
[0077] Example 8
[0078] The difference between this embodiment and embodiment 3 is that the gas flow rate is 0.1 L / min, and the rest is the same as embodiment 3.
[0079] Example 9
[0080] The difference between this embodiment and embodiment 3 is that the gas flow rate is 0.6 L / min, and the rest is the same as embodiment 3.
[0081] Example 10
[0082] The difference between this embodiment and embodiment 3 is that the relative cutting speed of the micro jet water-guided laser is 200 mm / min, and the rest is the same as embodiment 3.
[0083] Embodiment 11
[0084] The difference between this embodiment and embodiment 3 is that the relative cutting speed of the micro jet water-guided laser is 200 mm / min, and the rest is the same as embodiment 3.
[0085] Comparative Example 1
[0086] This comparative example is the same as steps (1) and (2) of Example 3, and step (3) adopts mechanical grinding to mark the positioning edge, and the operating parameters are: grinding wheel 500 mesh, rotation speed 500 rpm, single feed 5 μm, speed 50 mm / min.
[0087] Test Example 1
[0088] The silicon carbide crystals produced in the same batch were processed into Notch-shaped positioning edges by the above-mentioned embodiments and comparative examples. The diameter of the silicon carbide crystals was 200 mm, the thickness was 20 mm, and the size of the positioning edges was standard size. Ten parallel experiments were conducted for each embodiment or comparative example to test the processing time, product yield, and positioning edge processing accuracy. The test results are shown in Table 1. The calculation formula for the product yield is: (total number of products - number of defective products / total number of products) × 100, and the definition of defective products is that the product has a collapse edge size of > 100 μm or cracks; the calculation formula for the positioning edge processing accuracy is: (total thickness of the crystal rod - thickness of the unqualified Notch edge size / total thickness of the crystal rod) × 100.
[0089] Table 1
[0090]
[0091]
[0092] According to the data in Table 1, laser processing assisted by XRD positioning can achieve efficient and accurate positioning edge processing. According to Examples 1-3, after adjusting parameters such as gas flow, water pressure, nozzle inner diameter, relative cutting rate, power, frequency, etc., efficient cutting can be achieved. Since there is a balance between cutting efficiency and surface quality, at the extreme efficiency, surface quality and product yield are affected by the comprehensive influence of various parameters.
[0093] After the power is increased in Example 4, the laser effect is enhanced, and the processing efficiency is improved, but it may cause edge collapse and other phenomena, which reduces the yield, reduces the processing accuracy of the positioning edge, and increases the surface roughness of the positioning edge. After the frequency is increased in Example 5, under the current process, the efficiency is not greatly affected, but the edge collapse phenomenon may occur, resulting in a reduction in yield.
[0094] After the water pressure and gas flow rate of Examples 7-9 were adjusted, the water pressure and gas flow rate of Examples 7 and 9 were still within the beam action relationship, except that the effective processing distance was shortened, resulting in a longer cutting action time and worse surface quality. When the water pressure and gas flow rate of Examples 6 and 8 deviated from the action relationship, the water column would become unstable, and not only the quality would deteriorate, but the yield would also be significantly reduced.
[0095] In Example 11, increasing the relative cutting speed will reduce the cutting efficiency, and the surface quality and positioning edge processing accuracy will deteriorate; in Example 10, reducing the relative cutting speed can improve the cutting efficiency, but the surface quality will be significantly deteriorated. The laser processing method used in this application is overall more efficient than the grinding wheel mechanical grinding processing in Comparative Example 1.
[0096] The above are only embodiments of the present application. The protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for machining a silicon carbide positioning edge, characterized in that: The steps include: (1) Fixing the silicon carbide crystal; (2) Orient the (0004) crystal plane or (11-28) crystal plane of the silicon carbide crystal using XRD, first adjust the incident angle θ1 and the exit angle θ2 of the X-ray, then rotate the silicon carbide crystal with the vertical center line as the axis and perform φ scanning until it rotates to the position of the maximum diffraction intensity and stops, then rotate the silicon carbide crystal with the horizontal center line as the axis and perform χ scanning until it rotates to the position of the maximum diffraction intensity, finally continue to rotate the silicon carbide crystal with the horizontal center line as the axis, and adjust the χ value according to the required crystal deflection angle; (3) A microjet water-guided laser is used to mark the positioning edge on the (1-100) crystal plane of the crystal to form a positioning edge.
2. The method according to claim 1, characterized in that When the (0004) plane of the crystal is oriented in step (2), the incident angle θ1 and the exit angle θ2 of the X-ray are both 17.85°±0.1°; and / or When the (0004) crystal plane is used for orientation in step (2), the method further includes the following steps: Stop the rotation about the horizontal center line, then rotate the silicon carbide crystal 90° or 270° about the vertical center line, continue to rotate about the horizontal center line and perform χ scanning until it rotates to the position of the maximum diffraction intensity at this time.
3. The method according to claim 1, characterized in that When orienting the crystal (11-28) surface in step (2), the incident angle θ1 and the exit angle θ2 of the X-ray are adjusted to 9°±0.1° and 96°±0.1° respectively.
4. The method according to claim 1, characterized in that: In step (2), the rotation angle of the silicon carbide crystal around the horizontal center line is -10° to 10°.
5. The method according to any one of claims 1 to 4, characterized in that: The power of the micro jet water-guided laser is 15-200W, and the frequency is 6-10kHz.
6. The method according to any one of claims 1 to 4, characterized in that: The micro-jet water-guided laser is emitted through a beam coupler, the water pressure of the beam coupler is 150-500 bar, and the gas flow rate is 0.2-1 L / min; Preferably, the water pressure is P1, the unit is bar, the gas flow rate is P2, the unit is L / min, and P1 and P2 satisfy the following relationship: P1 / 1000≤P2≤P1 / 500.
7. The method according to claim 6, characterized in that The micro jet water-guided laser is emitted through a beam coupler, and the inner diameter of the nozzle of the beam coupler is 30-120 μm.
8. The method according to any one of claims 1 to 4, characterized in that: The relative cutting speed of the micro-jet water-guided laser is 100-1000 mm / min.
9. A silicon carbide crystal with a positioning edge obtained by processing according to any one of claims 1 to 8.
10. Use of the method according to any one of claims 1 to 8 in silicon carbide processing.
Citation Information
Cited By
Compensation method for crystal face orientation of single crystal material
CN121428673A
Method for compensating the orientation of a crystal face of a single crystal material
CN121428673B