Polishing pad, method for producing same, and polishing method

By designing the center part and the cladding part of the inspection window in the grinding pad and controlling its area ratio, the problem of insufficient bonding strength between the inspection window and the grinding layer is solved, and the service life and grinding quality of the grinding pad are improved.

CN118990328APending Publication Date: 2024-11-22IV TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410585943.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-19
Filing Date
2024-05-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The bonding strength between the detection window of the existing abrasive pad and the abrasive layer is insufficient, resulting in the problems of leakage of the abrasive liquid and short service life.

Method used

A grinding pad is designed, and its detection window includes a central part and a covering part surrounding the central part. The covering part is joined to the grinding layer. The area ratio of the center part and the covering part is between 0.03 and 5.00. By selecting a suitable material and Process conditions improve bonding strength.

Benefits of technology

It effectively improves the bonding strength between the inspection window and the grinding layer, extends the service life of the grinding pad, and improves the grinding quality and the efficiency of the inspection window.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118990328A_ABST
    Figure CN118990328A_ABST
Patent Text Reader

Abstract

A polishing pad, a manufacturing method thereof and a polishing method, the polishing pad comprising a polishing layer and at least one detection window located in the polishing layer, the at least one detection window comprising a central portion and a cladding portion surrounding the central portion, the cladding portion being bonded to the polishing layer, the cladding portion being bonded to the polishing layer, the cladding portion being bonded to the polishing layer. And the ratio of the area of the central part to the area of the coating part is between about 0.03 and about 5.00.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polishing pad, a manufacturing method thereof and a polishing method, and in particular to a polishing pad with a detection window, a manufacturing method of the polishing pad and a polishing method using the polishing pad. Background Art

[0002] In the component manufacturing process of the industry, the grinding process is a technology that is commonly used to flatten the surface of the object to be ground. In the grinding process, the object is ground by the relative motion between itself and the grinding pad, and a grinding liquid is provided between the surface of the object and the grinding pad.

[0003] For polishing equipment with an optical detection system, a detection window is usually set in a certain area of ​​the polishing layer of the polishing pad. Its function is that when using this polishing pad to polish an object, the user can use the optical detection system of the polishing equipment to detect the polishing condition of the object through the detection window, so as to serve as the end-point detection (End-Point Detection) of the polishing process and ensure the polishing quality.

[0004] In some embodiments, the polishing pad with a detection window has a structure in which the detection window material is directly combined with the polishing layer material, such as Figure 1 As shown, during the polishing process, the polishing head H carrying the object S will perform relative motion on the polishing surface of the polishing pad P in a rotating manner B or in a rotating manner B plus a left-right swinging manner C. The shear force and normal force generated in the aforementioned process will easily damage the interface between the polishing layer and the detection window, thereby causing the polishing liquid to leak through the interface between the polishing layer and the detection window during the polishing process, thereby affecting the polishing quality and the performance of the detection window.

[0005] Furthermore, the bonding strength between the detection window and the polishing layer is also limited by the material, and as the number of times the polishing pad polishes the object increases, the polishing pad wears more and more, and the bonding area between the detection window and the polishing layer becomes smaller and smaller, making it difficult for the interface between the detection window and the polishing layer to withstand the stress of the polishing process. Therefore, the current polishing pad has the problem of insufficient interface bonding strength between the detection window and the polishing layer, which leads to leakage of the polishing liquid, thereby affecting the service life of the polishing pad. In view of this, how to improve the bonding strength between the detection window and the polishing layer so that the polishing pad has a good service life is one of the topics that technicians in this field are actively studying. Summary of the invention

[0006] The invention provides a polishing pad, wherein the detection window and the polishing layer have improved bonding strength.

[0007] The polishing pad of the present invention includes a polishing layer and at least one detection window, wherein the at least one detection window is located in the polishing layer, wherein the at least one detection window includes a central portion and a covering portion surrounding the central portion, the covering portion is joined to the polishing layer, and the ratio of the area of ​​the central portion to the area of ​​the covering portion is between about 0.03 and about 5.00.

[0008] The manufacturing method of the polishing pad of the present invention comprises the following steps. Forming a detection window comprises: pre-setting a central portion in a first mold; and filling a coating material in the first mold and performing a first curing process to form a coating portion covering the central portion. Pre-setting the detection window in a second mold. Pouring a polishing layer material in the second mold and performing a second curing process to form a polishing layer bonded to the coating portion.

[0009] The polishing method of the present invention comprises the following steps: providing a polishing pad, wherein the polishing pad is any of the polishing pads described above; applying pressure to an object to press it onto the polishing pad; providing relative motion between the object and the polishing pad to perform a polishing process.

[0010] Based on the above, the polishing pad of the present invention includes a central portion and a covering portion surrounding the central portion through a detection window, the covering portion is connected to the polishing layer, and the ratio of the area of ​​the central portion to the area of ​​the covering portion is between about 0.03 and about 5.00, thereby improving the bonding strength between the detection window and the polishing layer. In addition, the covering portion of the detection window of the polishing pad of the present invention can overcome the stress problem during the polishing process by selecting a material with a high bonding degree with the polishing layer and the central portion of the detection window, and can also make the selection and matching of the polishing layer material and the central portion of the detection window material more free, so as to achieve the polishing quality required by the object.

[0011] In order to make the above features and advantages of the present invention more obvious and easy to understand, the following embodiments are specifically cited and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 is a schematic cross-sectional view of a known grinding system;

[0013] Figure 2A is a schematic top view of a polishing pad according to one embodiment of the present invention;

[0014] Figure 2B yes Figure 2A Schematic diagram of the cross section along line A-A';

[0015] Figure 3 is a cross-sectional schematic diagram of a polishing pad according to another embodiment of the present invention;

[0016] FIG. 4A to FIG. 4Cis a schematic cross-sectional view of a side surface of a central portion, a cladding portion or a polishing layer according to some embodiments of the present invention;

[0017] FIG. 5A to FIG. 5D is a schematic top view of a detection window according to another embodiment of the present invention;

[0018] 6A to 6F is a cross-sectional schematic diagram of a manufacturing process of a polishing pad according to one embodiment of the present invention;

[0019] Figure 7 is a cross-sectional schematic diagram of a manufacturing process of a polishing pad according to another embodiment of the present invention;

[0020] Figure 8 is a flow chart of a polishing method according to one embodiment of the present invention.

[0021] Description of Figure Numbers

[0022] 10, 20, 30: mold;

[0023] 12, 22, 32: mold cavity;

[0024] 100, 100', P: polishing pad;

[0025] 102: grinding layer;

[0026] 104: detection window;

[0027] 104a: center;

[0028] 104b: covering portion;

[0029] 106: basal layer;

[0030] B: Rotation mode;

[0031] BS: back side;

[0032] C: Swinging back and forth;

[0033] H: grinding head;

[0034] S: object;

[0035] S1: lateral surface;

[0036] S2, S4, S5: medial surface;

[0037] S3: lateral surface;

[0038] PS: grinding surface;

[0039] S10, S12, S14: steps;

[0040] TSa, TSb: top surface;

[0041] USa, USb: bottom surface. DETAILED DESCRIPTION

[0042] In this article, the range expressed by "a value to another value" is a summary expression method to avoid listing all the values ​​in the range one by one in the specification. Therefore, the description of a specific numerical range covers any value in the numerical range and a smaller numerical range defined by any value in the numerical range, just as if the arbitrary value and the smaller numerical range were explicitly written in the specification.

[0043] As used herein, "about" includes the stated value and the average value within an acceptable deviation range of the particular value determined by one of ordinary skill in the art, taking into account the measurement in question and the particular amount of error associated with the measurement (i.e., the limitations of the measurement system). For example, "about" can mean within one or more standard deviations of the stated value, or within, for example, ±30%, ±20%, ±15%, ±10%, ±5%. Furthermore, as used herein, "about" or "substantially" can select a more acceptable deviation range or standard deviation depending on the measured property or other property, and can apply to all properties without a single standard deviation.

[0044] It should be understood that when a component such as a layer, film, region, or trench is referred to as being "on," "connected to," or "contacting" another component, it may be directly on or connected / contacting the other component, or intermediate components may also exist. In contrast, when a component is referred to as being "directly on," "directly connected to," or "directly contacting" another component, there are no intermediate components.

[0045] In the drawings, the sizes and thicknesses of layers, regions and parts are exaggerated for clarity, that is, they are not drawn according to the actual scale.

[0046] Figure 2A FIG. 1 is a schematic top view of a polishing pad according to an embodiment of the present invention. Figure 2B yes Figure 2A Schematic diagram of the cross section along line A-A'.

[0047] Please also refer to Figure 2A and Figure 2B The polishing pad 100 includes a polishing layer 102 and a detection window 104. In another embodiment, the polishing pad further includes a base layer, which is disposed below the polishing layer 102. Figure 3 As shown (the following will be based on Figure 3 Detailed description).

[0048] In the present embodiment, the polishing layer 102 is, for example, made of a polymer substrate, wherein the polymer substrate may be polyester, polyether, polyurethane, polycarbonate, polyacrylate, polybutadiene, or other polymer substrates synthesized by suitable thermosetting resins or thermoplastic resins, but the present invention is not limited thereto. In addition to the polymer substrate, the polishing layer 102 may further include conductive materials, abrasive particles, microspheres, or soluble additives in the polymer substrate.

[0049] In this embodiment, the polishing layer 102 has a polishing surface PS and a back surface BS opposite to the polishing surface PS. In this document, the polishing surface PS of the polishing layer 102 is also referred to as the top surface; the back surface BS of the polishing layer 102 is also referred to as the bottom surface. When the polishing pad 100 is used to polish an object, the object will contact the polishing surface PS of the polishing layer 102. It is worth mentioning that although Figure 2A and Figure 2B Although not shown in the figure, any technician in the relevant technical field should know that the grinding surface PS includes a groove pattern, and the groove pattern can have a pattern distribution of various different embodiments, such as concentric rings, non-concentric rings, elliptical rings, wavy rings, irregular rings, multiple straight lines, parallel straight lines, radial straight lines, radial arcs, spirals, polygonal grids, or combinations thereof, but the present invention is not limited thereto.

[0050] The detection window 104 is located in the grinding layer 102. Figure 2A and Figure 2B As shown in FIG. 1 , the detection window 104 includes a central portion 104a and a covering portion 104b surrounding the central portion 104a. In other words, the detection window 104 includes two parts. Figure 2A and Figure 2B As shown, the central portion 104a is in direct contact with the covering portion 104b.

[0051] In addition, if Figure 2A and Figure 2B As shown, the covering portion 104b is bonded to the grinding layer 102. That is, the detection window 104 is fixed to the grinding layer 102 through the covering portion 104b. In other words, the covering portion 104b is bonded between the central portion 104a and the grinding layer 102. From another point of view, Figure 2BAs shown, the bonding interface between the central portion 104a and the covering portion 104b and the bonding interface between the covering portion 104b and the grinding layer 102 are all smooth surfaces. That is, in this embodiment, the side surface S1 of the central portion 104a, the inner surface S2 and the outer surface S3 of the covering portion 104b, and the inner surface S4 of the grinding layer 102 are all smooth surfaces. However, the present invention is not limited to this. In other embodiments, each of the side surface S1 of the central portion 104a, the inner surface S2 and the outer surface S3 of the covering portion 104b, and the inner surface S4 of the grinding layer 102 can be a rough surface, and the rough surface is, for example, a spiral surface (such as Figure 4A As shown), corrugated surface (as Figure 4B as shown) or particle surface (as Figure 4C That is, in the aforementioned embodiment, the bonding interface between the central portion 104a and the covering portion 104b and the bonding interface between the covering portion 104b and the grinding layer 102 may be rough surfaces. It is worth mentioning that by designing each of the side surface S1 of the central portion 104a, the inner surface S2 and the outer surface S3 of the covering portion 104b, and the inner surface S4 of the grinding layer 102 as a rough surface, the contact area between the central portion 104a, the covering portion 104b and the grinding layer 102 can be increased, thereby increasing the tightness between the three. In another embodiment, the side surface S1 of the central portion 104a and the inner surface S2 of the covering portion 104b may be designed as rough surfaces, and the outer surface S3 of the covering portion 104b and the inner surface S4 of the grinding layer 102 may be designed as smooth surfaces, thereby increasing the contact area between the central portion 104a and the covering portion 104b and further increasing the bonding strength between the central portion 104a and the covering portion 104b of the detection window 104.

[0052] In the present embodiment, the ratio of the area of ​​the central portion 104a to the area of ​​the covering portion 104b is between about 0.03 and about 5.00. Specifically, if the ratio of the area of ​​the central portion 104a to the area of ​​the covering portion 104b is less than about 0.03, it means that the area of ​​the covering portion 104b is much larger than the area of ​​the central portion 104a. In this way, due to the excessively large area of ​​the covering portion 104b, the polishing area on the polishing surface PS will be reduced, which may easily cause the object (object to be polished) to be polished to the polishing area on the polishing surface PS and the area on the top surface TSb of the covering portion 104b during the polishing process, or even worse, the object is mainly polished to the area on the top surface TSb of the covering portion 104 instead of the polishing area on the polishing surface PS that is mainly used to polish the object, which will affect the polishing performance, such as the object's planarity is not as expected, the object has surface concavity (dishing), or the object is prone to defects. If the ratio of the area of ​​the central portion 104a to the area of ​​the covering portion 104b is greater than about 5.00, it means that the area of ​​the covering portion 104b is less than 1 / 5 of the area of ​​the central portion 104a. In this way, because the area of ​​the covering portion 104b is too small, that is, the width d of the covering portion 104b is very small, the interface bonding force between the central portion 104a and the covering portion 104b and the covering portion 104b and the grinding layer 102 will be difficult to resist the lateral shear force and the positive (gravity direction) pressure applied by the grinding head of the object during the grinding process, thereby causing the interface to be disengaged or broken. It is worth mentioning that by designing the area ratio of the central portion 104a to the covering portion 104b in the range of about 0.03 to about 5.00, the interface bonding force between the detection window 104 and the grinding layer 102 is improved.

[0053] In this embodiment, if Figure 2B As shown, the center portion 104a has a top surface TSa and a bottom surface USa opposite to each other, wherein the top surface TSa of the center portion 104a is adjacent to the grinding surface PS of the grinding layer 102, and the bottom surface USa of the center portion 104a is also adjacent to the back surface BS of the grinding layer 102. In other words, the top surface TSa and the bottom surface USa of the center portion 104a are coplanar with the top surface (i.e., the grinding surface PS) and the bottom surface (i.e., the back surface BS) of the grinding layer 102, respectively. On the other hand, as Figure 2BAs shown in FIG. 1 , the covering portion 104b has a top surface TSb and a bottom surface USb opposite to each other, wherein the top surface TSb of the covering portion 104b is adjacent to the grinding surface PS of the grinding layer 102, and the bottom surface USb of the covering portion 104b is also adjacent to the back surface BS of the grinding layer 102. In other words, the top surface TSb and the bottom surface USb of the covering portion 104b are coplanar with the top surface (i.e., the grinding surface PS) and the bottom surface (i.e., the back surface BS) of the grinding layer 102, respectively. From another point of view, in the case of Figure 2B In the illustrated embodiment, the top surface TSa of the central portion 104a, the top surface TSb of the covering portion 104b, and the top surface of the polishing layer 102 (i.e., the polishing surface PS) are all coplanar; and the bottom surface USa of the central portion 104a, the bottom surface USb of the covering portion 104b, and the bottom surface of the polishing layer 102 (i.e., the back side BS) are all coplanar.

[0054] In this embodiment, the central portion 104a can be made of any material known to a person skilled in the art that can be used in a detection window of a polishing pad. For example, the material of the central portion 104a of the detection window 104 can be a transparent polymer, such as a thermosetting plastic or a thermoplastic. From another point of view, in this embodiment, the material of the central portion 104a is translucent under visible light. In detail, for light with a wavelength between 380nm and 780nm, the transmittance of the central portion 104a is at least 40%. In this way, when the polishing pad 100 is used to grind an object, the user can use an optical detection system to detect the grinding condition of the object through the central portion 104a of the detection window 104, so as to detect the end point of the grinding process and ensure the grinding quality.

[0055] In the present embodiment, the coating 104b may include polyester, polyether, polyurethane, polycarbonate, polyacrylate, polybutadiene, or other polymer substrates synthesized by suitable thermosetting resins or thermoplastic resins. In the present embodiment, the material of the coating 104b is different from the material of the central portion 104a. In detail, in one embodiment, the material of the central portion 104a is translucent under visible light, while the material of the coating 104b is not translucent under visible light. In another embodiment, the hardness of the coating 104b and the central portion 104a is different, and the ratio of the hardness of the central portion 104a to the hardness of the coating 104b is not greater than about 1.8. Specifically, if the ratio of the hardness of the central portion 104a to the hardness of the covering portion 104b is greater than about 1.8, the difference in hardness between the central portion 104a and the covering portion 104b is too large, which causes the covering portion 104b to be easily squeezed by the central portion 104a during the grinding process, thereby damaging the interface between the central portion 104a and the covering portion 104b, thereby affecting the service life of the grinding pad. It is worth mentioning that by designing the ratio of the hardness of the central portion 104a to the hardness of the covering portion 104b to be within a range of not more than about 1.8, in addition to improving the interface bonding force between the detection window 104 and the grinding layer 102, the wear amount of the central portion 104a and the covering portion 104b during the grinding process will not differ too much, thereby affecting the grinding quality of the object, the detection quality of the detection window 104, or the service life of the grinding pad.

[0056] From another point of view, in one embodiment, the material of the coating 104b is the same as the material of the polishing layer 102, that is, the coating 104b and the polishing layer 102 include the same polymer substrate, which may include polyester, polyether, polyurethane, polycarbonate, polyacrylate, polybutadiene, or other polymer substrates synthesized by suitable thermosetting resins or thermoplastic resins. It should be particularly noted that although the coating 104b and the polishing layer 102 are made of the same polymer substrate, the coating 104b and the polishing layer 102 can be selectively made to have the same or different physical properties (such as hardness, density or compressibility) by adjusting process conditions (such as injection volume, gas pressure, reaction temperature, mold design and other process conditions but not limited thereto). In detail, in one embodiment, polyurethane is selected as the polymer substrate of the coating portion 104b and the grinding layer 102, and the coating portion 104b and the grinding layer 102 are manufactured by the injection molding method, wherein by making the coating portion 104b and the grinding layer 102 have different process conditions (such as injection amount, gas pressure, reaction temperature, mold design and other process conditions but not limited thereto), the obtained coating portion 104b and the grinding layer 102 can have different hardness, density or compression rate. In other words, by adjusting the process conditions of the coating portion 104b and the grinding layer 102 (such as injection amount, gas pressure, reaction temperature, mold design and other process conditions but not limited thereto), the coating portion 104b and the grinding layer 102 can have predetermined physical properties (such as hardness, density or compression rate). It is worth mentioning that the coating 104 b and the grinding layer 102 are made of the same material, so that the material properties of the coating 104 b and the grinding layer 102 have better material compatibility, thereby effectively improving the interface bonding strength between the coating 104 b and the grinding layer 102 .

[0057] In another embodiment, the material of the coating 104b is different from the material of the grinding layer 102. It should be particularly noted that, although the coating 104b and the grinding layer 102 are made of different polymer substrates, in addition to selecting different polymer substrates to make the coating 104b and the grinding layer 102 have better material compatibility, the coating 104b and the grinding layer 102 can also be selectively made to have similar physical properties (such as hardness, density or compression rate) by adjusting process conditions (such as injection volume, gas pressure, reaction temperature, mold design and other process conditions but not limited thereto) so that the coating 104b and the grinding layer 102 have better material compatibility, thereby effectively improving the interface bonding force between the coating 104b and the grinding layer 102. It is worth mentioning that by adjusting the process conditions (such as injection volume, gas pressure, reaction temperature, mold design and other process conditions but not limited to these), the coating 104b and the grinding layer 102 made of different materials can have similar physical properties (such as hardness, density or compression rate), which has greater freedom in the material selection of the coating 104b and the grinding layer 102.

[0058] In this embodiment, the outer contours of the central portion 104a and the covering portion 104b can be designed into various shapes according to actual needs, such as a circle, an ellipse, a shuttle shape, or a raindrop shape. In other words, the outer contours of the central portion 104a and the covering portion 104b can be irregular shapes or regular geometric shapes. Figure 2A As shown, the outer contours of the central portion 104a and the covering portion 104b are both fusiform. That is, in this embodiment, the outer contour of the central portion 104a is the same as the outer contour of the covering portion 104b and both are irregular shapes. However, the present invention is not limited to this. In another embodiment, the outer contour of the central portion 104a is the same as the outer contour of the covering portion 104b and both are regular geometric shapes. For example, Figure 5A As shown, the outer contours of the central portion 104a and the covering portion 104b are both circular. In another embodiment, the outer contour of the central portion 104a is different from the outer contour of the covering portion 104b. Figure 5B As shown, the outer contour of the central portion 104a is circular, while the outer contour of the covering portion 104b is shuttle-shaped; Figure 5C As shown, the outer contour of the central portion 104a is in the shape of a raindrop, while the outer contour of the covering portion 104b is in the shape of a circle; and Figure 5D As shown, the outer contour of the central portion 104a is in a raindrop shape, and the outer contour of the covering portion 104b is in a shuttle shape, but the present invention is not limited thereto.

[0059] In addition, although Figure 2A and Figure 2B The number of the detection window 104 is shown as one, but the present invention is not limited thereto. In other embodiments, the number of the detection windows 104 may be two, three or more according to actual needs. In other words, as long as at least one detection window 104 is provided in the polishing layer 102, it falls within the scope of the present invention.

[0060] In another embodiment, the polishing pad may further include a base layer disposed below the polishing layer. Figure 3 As shown, the polishing pad 100' includes a polishing layer 102 and a base layer 106, wherein the base layer 106 is located below the polishing layer 102. In detail, the base layer 106 mainly functions to cushion the polishing layer 102 and is fixed on a polishing platform (not shown). Figure 3 As shown in FIG. 1 , the base layer 106 is also located below the covering portion 104 b of the detection window 104. Figure 3 As shown, the inner surface S5 of the base layer 106 is substantially aligned with the inner surface S2 of the coating 104b. That is, the coating 104b completely overlaps with the base layer 106. However, the present invention is not limited to this. In another embodiment, when the bonding interface between the coating 104b and the grinding layer 102 overlaps with the base layer 106, the inner surface S5 of the base layer 106 is not aligned with the inner surface S2 of the coating 104b (for example, there may be a spacing between the inner surface S2 and the inner surface S5). In addition, in this embodiment, the base layer 106 can be bonded to the coating 104b and the grinding layer 102 through an adhesive layer (not shown). In addition, in this embodiment, the main material of the base layer 106 is, for example, polyurethane, polyethylene, polypropylene, a copolymer of polyethylene and ethylene vinyl acetate, or a copolymer of polypropylene and ethylene vinyl acetate, or any currently known material for the base layer of the grinding pad.

[0061] It is worth mentioning that in this embodiment, by designing the ratio of the area of ​​the central portion 104a to the area of ​​the covering portion 104b to be between about 0.03 and about 5.00, and making the bonding interface between the covering portion 104b and the central portion 104a overlap with the base layer 106, the interface bonding force between the detection window 104 and the grinding layer 102 can be effectively improved, so that when the grinding pad 100' is used to grind an object, the bonding interface between the covering portion 104b and the grinding layer 102 will not cause delamination due to the applied downward pressure, thereby causing grinding leakage to the delamination position of the grinding pad and affecting the service life of the grinding pad. In this way, in the grinding pad 100', the interface bonding force between the detection window 104 and the grinding layer 102 is improved.

[0062] In order to verify that the detection window 104 and the polishing layer 102 have improved interface bonding strength, an interface bonding strength test was actually conducted. In the experimental test, the test method and sample settings used are as follows, and the test results are listed in Table 1-1 and Table 1-2.

[0063] Bonding force test method: ASTM D412 standard test method is used to measure the bonding force between the detection window and the grinding layer.

[0064] Samples 1 to 4: Samples 1 to 4 are all single-layer polishing pads with detection windows (i.e., polishing pads that do not include a base layer), wherein Sample 1 is configured with a known detection window, while Samples 2 to 4 are configured with the detection window of the present invention including a central portion and a covering portion, and the difference between the detection windows configured in Samples 2 to 4 lies in the ratio of the area of ​​the central portion to the area of ​​the covering portion.

[0065] Samples 5 to 8: Samples 5 to 8 are all double-layer polishing pads with detection windows (i.e., polishing pads including a polishing layer and a base layer), wherein Sample 5 is configured with a known detection window, while Samples 6 to 8 are configured with the detection window of the present invention including a central portion and a covering portion, and the difference between the detection windows configured in Samples 6 to 8 lies in the ratio of the area of ​​the central portion to the area of ​​the covering portion.

[0066] Table 1-1.

[0067]

[0068] Table 1-2

[0069]

[0070] From the content of Table 1-1 above, it can be seen that the bonding force between the known detection window and the grinding layer of sample 1 is 93.6 kgf / mm 2 The bonding forces between the detection window and the grinding layer of samples 2 to 4 of the present invention are 130.6 kgf / mm 2 、128.2kgf / mm 2 and 101.5kgf / mm 2 , where Samples 2 to 4 have different bonding forces because they have different area ratios of the center portion to the covering portion. It can be seen that compared with the polishing pad of Sample 1, the polishing pads of Samples 2 to 4 have better bonding forces between the detection window and the polishing layer. The same experimental results can also be seen from Table 1-2 above. In detail, the known bonding force between the detection window and the polishing layer of Sample 5 is 79.9kgf / mm 2 The bonding forces between the detection window and the grinding layer of samples 6 to 8 of the present invention are 136.7 kgf / mm 2、118.0kgf / mm 2 and 84.9kgf / mm 2 , where Samples 6 to 8 have different binding forces because they have different area ratios of the center portion to the covering portion. It can be seen that, compared with the polishing pad of Sample 5, the polishing pads of Samples 6 to 8 have better binding forces between the detection window and the polishing layer. The results of Tables 1-1 and 1-2 above show that, regardless of whether the polishing pad is a single-layer polishing pad or a double-layer polishing pad consisting of a polishing layer and a base layer, the interface binding force between the detection window and the polishing layer can be improved by replacing the known detection window with the detection window of the present invention. In other words, by including a detection window structure consisting of a center portion and a covering portion, and the ratio of the area of ​​the center portion to the area of ​​the covering portion is designed to be between about 0.03 and about 5.00, the interface binding force between the detection window and the polishing layer in the polishing pad can indeed be improved.

[0071] Table 2 below records the bonding force between the center portion and the covering portion of the inspection window measured using polishing pad samples having different ratios of the hardness of the center portion to the hardness of the covering portion according to the ASTM D412 standard test method.

[0072] Samples 9 to 13 in Table 2 are all single-layer polishing pads having the detection window of the present invention, and samples 9 to 13 are formed with different ratios of the hardness of the central portion to the hardness of the covering portion.

[0073] Table 2

[0074]

[0075] From the content of Table 2 above, it can be seen that the ratio of the hardness of the central part of the detection window of sample 9 to the hardness of the covering part is 0.85, and the measured bonding force between the central part of the detection window and the covering part can be as high as 217.7 kgf / mm 2 As the ratio of the hardness of the central part of the detection window to the hardness of the covering part is changed to 0.88, 1.00, 1.81 and 2.01 for samples 10 to 13, the measured bonding force between the central part of the detection window and the covering part is reduced to 207.3 kgf / mm 2 、93.6kgf / mm 2 、87.6kgf / mm 2 and 87.8kgf / mm 2. It can be seen that as the ratio of the hardness of the central part of the detection window to the hardness of the coating increases, the bonding force between the central part of the detection window and the coating decreases accordingly. From another point of view, when a trend graph is drawn with the horizontal axis as the ratio of the hardness of the central part of the detection window to the hardness of the coating, and the vertical axis as the bonding force between the central part of the detection window and the coating, it can be found that when the ratio of the hardness of the central part to the hardness of the coating exceeds 1.8, the value of the bonding force presents a convergence state and approaches a constant value. This result shows that by designing the ratio of the hardness of the central part to the hardness of the coating to be within a range of no more than about 1.8, the bonding force between the central part and the coating can be effectively improved. Further, when the ratio of the hardness of the central part to the hardness of the coating is designed to be within a range of no more than about 1.8, when the ratio of the area of ​​the central part to the area of ​​the coating is designed to be within a range of about 0.03 to about 5.00, the interface bonding force between the detection window and the grinding layer can be improved together (as shown in the aforementioned Tables 1-1 and 1-2).

[0076] In addition, the following will refer to 6A to 6F It should be noted that, although the manufacturing method of the polishing pad 100 in the above-mentioned embodiments is described as an example, the manufacturing method of the polishing pad 100 of the present invention is not limited thereto, and the materials, thicknesses or functions of the same or similar components in the polishing pad 100 are described in detail above, and will not be repeated here. 6A to 6F It is a schematic cross-sectional view of a manufacturing process of a polishing pad according to one embodiment of the present invention.

[0077] First, the central portion 104a of the detection window 104 is formed. The central portion 104a has a predetermined outer contour shape. The outer contour shape may be an irregular shape or a regular geometric shape. The outer contour shape may be, for example, FIG. 5A to FIG. 5D As shown. There are two methods for forming the center portion 104a having a predetermined outer contour shape. The first method is to make the predetermined outer contour shape (e.g., a shuttle shape) on the mold in advance, and after the curing process, the center portion 104a having the predetermined outer contour shape (e.g., a shuttle shape) can be obtained. The second method is not to make the predetermined outer contour shape (e.g., a shuttle shape) on the mold, but to first obtain a light-transmitting material layer having a conventional outer contour shape (e.g., a rectangle) after the curing process, and then process the light-transmitting material layer (e.g., mechanical processing) to form the center portion 104a having the predetermined outer contour shape (e.g., a shuttle shape). In this embodiment, the first manufacturing method is used for illustration. As Fig. 6AAs shown, the center portion 104a having a predetermined outer contour shape is directly formed by using the mold 10. The detailed steps are as follows: Provide a mold 10. The mold 10 has a mold cavity 12, which is used to accommodate the molding material. In this embodiment, the shape and size of the mold cavity 12 are related to the shape and size of the outer contour of the center portion 104a to be formed later. That is, Figure 2A As shown, the shape of the mold cavity 12 is shuttle-shaped. In addition, in order to enable technicians in this field to clearly understand the present invention, in the following figures, only a partial mold 10 is shown, that is, the upper cover structure of the mold 10 is omitted. Next, the light-transmitting material is filled into the mold cavity 12 of the mold 10, and a curing process is performed to form a central portion 104a in the mold 10. In this embodiment, the method of filling the light-transmitting material into the mold cavity 12 of the mold 10 includes a perfusion method. In this embodiment, the curing process for curing the light-transmitting material includes a lighting process, a heating process, a pressurizing process or a static process. In detail, the curing process includes, for example, irradiating or heating the light-transmitting material to cause a polymerization reaction to achieve curing; or, for example, including a natural polymerization reaction of the reactants in the light-transmitting material to achieve curing; or, for example, including pressurizing the light-transmitting material to cause the light-transmitting material to cause a polymerization reaction to achieve curing. Finally, the mold 10 is removed to obtain a central portion 104a with a predetermined outer contour shape. In this embodiment, the light-transmitting material used to form the central portion 104 a is light-transmitting under visible light.

[0078] Next, after forming the central portion 104a having a predetermined outer contour shape, a covering portion 104b having a predetermined outer contour shape is formed to obtain the detection window 104. The outer contour shape of the covering portion 104b may be as follows: FIG. 5A to FIG. 5D Please also refer to Figure 6B and Figure 6C , a method of directly forming the covering portion 104b having a predetermined outer contour shape by using the mold 20 is described. The detailed steps are as follows: Figure 6B As shown, a mold 20 is provided. The mold 20 has a mold cavity 22 for containing a molding material. In this embodiment, the shape and size of the mold cavity 22 are related to the shape and size of the outer contour of the covering portion 104b to be formed later. Figure 2A As shown in FIG. 1 , the shape of the mold cavity 22 is a shuttle shape. Figure 2AAs shown, the outer contour of the center portion 104a is the same as the outer contour of the covering portion 104b, so the outer contour of the mold 20 can be the same as the outer contour of the mold 10. However, as mentioned above, the outer contour of the center portion 104a and the outer contour of the covering portion 104b can be different from each other, so in this case, the outer contour of the mold 20 can be different from the outer contour of the mold 10. In addition, in order to enable technicians in this field to clearly understand the present invention, only a part of the mold 20 is shown in the following drawings, that is, the upper cover structure of the mold 20 is omitted. After that, please continue to refer to Figure 6B , the center portion 104a is arranged at a specific position in the cavity 22 of the mold 20. In detail, as Figure 6B As shown, the center portion 104a is spaced a distance from the inner edge of the mold 20. In this embodiment, as shown in FIG. Figure 6B As shown, the thickness of the central portion 104a is equivalent to the depth of the mold cavity 22. In addition, the central portion 104a can be fixed to a specific position of the mold 20 by pressing the mold 20 and the upper cover structure or by gluing.

[0079] Then, please also refer to Figure 6B and Figure 6C, fill the coating material into the cavity 22 of the mold 20 to surround the central portion 104a in the mold 20. In the present embodiment, the method of filling the coating material into the cavity 22 of the mold 20 includes a perfusion method. Next, a curing procedure is performed to cure the coating material to form a coating portion 104b that covers the central portion 104a in the mold 20. In the present embodiment, the side surface S1 of the central portion 104a is connected to the inner surface S2 of the coating portion 104b. In the present embodiment, the curing procedure for curing the coating material includes a lighting procedure, a heating procedure, a pressurizing procedure, or a standing procedure. In detail, the curing procedure includes, for example, irradiating or heating the coating material to cause a polymerization reaction to achieve curing; or, for example, including a natural polymerization reaction of the reactants in the coating material to achieve curing; or, for example, including pressurizing the coating material to cause a polymerization reaction of the light-transmitting material to achieve curing. Finally, the mold 20 is removed to obtain the central portion 104a and the coating portion 104b having a predetermined outer contour shape. However, the present invention is not limited thereto. In another embodiment, the method of forming the coating portion 104b having a predetermined outer contour shape can be divided into two steps: the first step is to first use a mold to obtain a coating material layer having a conventional shape (e.g., a rectangle), and the shape and size of the mold cavity 22 of the mold 20 used in this step are independent of the predetermined shape and size of the outer contour of the coating portion 104b to be formed subsequently. In this embodiment, after the curing process of the coating material is performed to form the coating material layer, the second step is then performed to process the coating material layer (e.g., by mechanical process) to remove part of the coating material layer to form a coating portion 104b with a predetermined shape (e.g., a shuttle shape). In this embodiment, the coating material used to form the coating portion 104b is different from the light-transmitting material used to form the central portion 104a. In this embodiment, as described above, the predetermined shape is an irregular shape or a regular geometric shape.

[0080] Next, after forming the detection window 104, the polishing layer 102 is formed to be bonded to the covering portion 104b of the detection window 104. Fig.6D and Fig. 6E , the grinding layer 102 is formed by using the mold 30. The detailed steps are as follows: Fig.6D As shown, a mold 30 is provided. The mold 30 has a mold cavity 32 for containing a molding material. In this embodiment, the shape and size of the mold cavity 32 are related to the shape and size of the polishing layer 102 to be formed later. Figure 2A As shown, the shape of the mold cavity 32 is circular. In addition, in order to enable the technicians in this field to clearly understand the present invention, only a part of the mold 30 is shown in the following drawings, that is, the upper cover structure of the mold 30 is omitted. Fig.6D, a detection window 104 is arranged at a specific position in the mold cavity 32 of the mold 30, and the specific position corresponds to the position of the optical detection system. Fig.6D As shown, the thickness of the detection window 104 is equivalent to the depth of the mold cavity 32. In addition, the detection window 104 can be fixed to a specific position of the mold 30 by pressing the mold 30 and the upper cover structure, or by gluing.

[0081] Then, please also refer to Fig.6D and Fig. 6E , the grinding layer material is filled into the mold cavity 32 of the mold 30 to surround the detection window 104 in the mold 30. In the present embodiment, the method of filling the grinding layer material into the mold cavity 32 of the mold 30 includes a perfusion method. Next, a curing process is performed to cure the grinding layer material to form the grinding layer 102 in the mold 30. In the present embodiment, the outer surface S3 of the coating 104b is connected to the inner surface S4 of the grinding layer 102. In the present embodiment, the curing process for curing the grinding layer material includes a lighting process, a heating process, a pressurizing process or a static process. In detail, the curing process includes, for example, irradiating or heating the grinding layer material to produce a polymerization reaction to achieve curing; or, for example, including a natural polymerization reaction of the reactants in the grinding layer material to achieve curing; or, for example, including pressurizing the grinding layer material to cause the light-transmitting material to produce a polymerization reaction to achieve curing. In one embodiment, the coating material used to form the coating 104b is the same as the grinding layer material used to form the grinding layer 102. In another embodiment, the coating material used to form the coating portion 104 b is different from the polishing layer material used to form the polishing layer 102 .

[0082] Finally, please also refer to Fig. 6E and Fig. 6F , the mold 30 is removed to obtain a polishing pad 100 having a detection window 104, wherein the detection window 104 includes a central portion 104a and a covering portion 104b surrounding the central portion 104a, wherein the covering portion 104b is joined to the polishing layer 102, and the ratio of the area of ​​the central portion 104a of the detection window 104 to the area of ​​the covering portion 104b is between about 0.03 and about 5.00, thereby improving the bonding strength between the detection window 104 and the polishing layer 102.

[0083] Figure 7 is a cross-sectional schematic diagram of the manufacturing process of the polishing pad according to another embodiment of the present invention. Figure 7 and Fig. 6F , Figure 7 The polishing pad 100 ′ shown in FIG. Fig. 6F, so the same or similar components are represented by the same or similar symbols, and the relevant descriptions are not repeated. In detail, the main difference between the method of manufacturing the polishing pad 100' and the method of manufacturing the polishing pad 100 is that: in the process of manufacturing the polishing pad 100', after the polishing layer 102 and the detection window 104 are formed, the base layer 106 is formed under the covering portion 104b of the polishing layer 102 and the detection window 104. In one embodiment, for example, a continuous base layer material is first formed under the polishing layer 102 and the detection window 104, and then a portion of the base layer material corresponding to the central portion 104a of the detection window 104 is removed to form the base layer 106. In addition, in one embodiment, before forming the base layer 106 below the coating 104b of the grinding layer 102 and the detection window 104, an adhesive layer (not shown) can be selectively formed below the coating 104b of the grinding layer 102 and the detection window 104 to bond the base layer 106 to the coating 104b of the grinding layer 102 and the detection window 104. The adhesive layer is, for example, an adhesive layer, which includes (but is not limited to): carrier-free adhesive, double-sided adhesive, UV curing adhesive, hot melt adhesive, moisture curing adhesive or pressure sensitive adhesive (PSA), and the material of the adhesive layer is, for example, acrylic adhesive, epoxy resin adhesive or polyurethane adhesive. However, the present invention is not limited to this. In other embodiments, the base layer 106 can be directly formed below the coating 104b of the grinding layer 102 and the detection window 104 by coating, spraying, stacking or printing, without the need for an adhesive layer, and the process of removing part of the base layer material can be reduced.

[0084] Figure 8 1 is a flow chart of a grinding method according to an embodiment of the present invention. The grinding method is applicable to grinding an object. In detail, the grinding method can be applied to the grinding process of manufacturing industrial components, such as components used in the electronics industry, which may include semiconductors, integrated circuits, micro-electromechanical, energy conversion, communications, optics, storage disks, and displays. The objects used to make these components may include semiconductor chips, IIIV chips, storage component carriers, ceramic substrates, polymer substrates, and glass substrates, but are not intended to limit the scope of the present invention.

[0085] Please refer to Figure 8 First, step S10 is performed to provide a polishing pad. Specifically, in this embodiment, the polishing pad includes the polishing layer 100 or 100' in any of the above embodiments. The polishing pad 100 and the polishing pad 100' have been described in detail above, so they will not be repeated here.

[0086] Next, step S12 is performed to apply pressure to the object, so that the object is pressed onto the polishing pad and contacts the polishing pad. Specifically, as described above, the object contacts the polishing surface PS in the polishing layer 102. In addition, the method of applying pressure to the object is, for example, to use a carrier capable of holding the object.

[0087] Then, step S14 is performed to provide relative motion between the object and the polishing pad so as to polish the object with the polishing pad to achieve the purpose of flattening. Specifically, the method of providing relative motion between the object and the polishing pad is, for example, to rotate the polishing platform to drive the polishing pad fixed on the polishing platform to rotate.

[0088] In summary, in the polishing pad of the present invention, the detection window includes a central portion and a covering portion surrounding the central portion, the covering portion is joined to the polishing layer, and the ratio of the area of ​​the central portion to the area of ​​the covering portion is between about 0.03 and about 5.00, thereby improving the bonding strength between the detection window and the polishing layer.

[0089] In addition, in the polishing pad of the present invention, the material selection for the covering portion of the detection window is to overcome the stress problem during the polishing process by selecting a material that has a high degree of bonding with the polishing layer and the center portion of the detection window. This also allows for greater freedom in the selection and matching of the polishing layer material and the center portion of the detection window material, thereby better achieving the polishing quality required by the object.

[0090] Although the present invention has been disclosed as above in the form of an implementation method, it is not intended to limit the present invention. Any technician in the relevant technical field can make some changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the definition of the attached claims.

Claims

1. A polishing pad comprising: Grinding layer; as well as At least one detection window is located in the grinding layer, wherein the at least one detection window includes a central portion and a covering portion surrounding the central portion, the covering portion is joined to the grinding layer, and the ratio of the area of ​​the central portion to the area of ​​the covering portion is between about 0.03 and about 5.

00. 2 . The polishing pad according to claim 1 , wherein a top surface of the central portion is coplanar with a top surface of the covering portion and a top surface of the polishing layer. 3 . The polishing pad according to claim 1 , wherein a bottom surface of the central portion is coplanar with a bottom surface of the covering portion and a bottom surface of the polishing layer. The polishing pad according to claim 1 , wherein the central portion is in direct contact with the cover portion. 5 . The polishing pad of claim 1 , wherein a ratio of a hardness of the central portion to a hardness of the cover portion is no greater than about 1.

8. 6 . The polishing pad according to claim 1 , wherein the core portion is made of a first material and the cover portion is made of a second material, the first material being different from the second material. 7 . The polishing pad according to claim 6 , wherein the polishing layer is made of a third material, and the third material is the same material as the second material. 8 . The polishing pad according to claim 6 , wherein the polishing layer is made of a third material, and the third material is different from the second material. 9 . The polishing pad according to claim 6 , wherein the first material is a light-transmitting material under visible light. 10 . The polishing pad according to claim 1 , wherein an outer contour of the central portion is the same as an outer contour of the covering portion. The polishing pad according to claim 1 , wherein an outer contour of the central portion and an outer contour of the covering portion are different in shape. 12 . The polishing pad according to claim 1 , wherein the outer contour of the covering portion is an irregular shape or a regular geometric shape. 13 . The polishing pad according to claim 1 , wherein the shape of the outer contour of the central portion is an irregular shape or a regular geometric shape. The polishing pad according to claim 1 , wherein a side surface of the central portion is a rough surface. The polishing pad according to claim 1 , wherein a side surface of the covering portion is a rough surface. 16 . The polishing pad according to claim 1 , further comprising a base layer disposed below the polishing layer.

17. A method for manufacturing a polishing pad, comprising: A detection window is formed, including: Presetting the center portion in the first mold; and Filling the first mold with a coating material and performing a first curing process to form a coating portion that covers the central portion; Pre-placing the detection window in the second mold; and A polishing layer material is poured into the second mold and a second curing process is performed to form a polishing layer bonded to the covering portion. 18 . The method for manufacturing a polishing pad according to claim 17 , wherein a top surface of the central portion is coplanar with a top surface of the covering portion and a top surface of the polishing layer. 19 . The method for manufacturing a polishing pad according to claim 17 , wherein a bottom surface of the central portion is coplanar with a bottom surface of the covering portion and a bottom surface of the polishing layer. 20 . The method for manufacturing a polishing pad according to claim 17 , wherein the central portion is in direct contact with the cover portion. 21 . The method for manufacturing a polishing pad according to claim 17 , wherein a ratio of an area of ​​the central portion to an area of ​​the covering portion is between about 0.03 and about 5.

00. 22 . The method for manufacturing a polishing pad according to claim 17 , wherein a ratio of a hardness of the central portion to a hardness of the covering portion is no greater than about 1.

8.

23. The method for manufacturing a polishing pad according to claim 17, wherein the coating material is the same as the polishing layer material.

24. The method for manufacturing a polishing pad according to claim 17, wherein the coating material is different from the polishing layer material. 25 . The method for manufacturing a polishing pad according to claim 17 , wherein the central portion has a predetermined outer contour shape, and the outer contour shape is an irregular shape or a regular geometric shape.

26. The method for manufacturing a polishing pad according to claim 25, wherein a method for forming the center portion comprises: The light-transmitting material is poured into the third mold and a third curing process is performed.

27. The method for manufacturing a polishing pad according to claim 26, wherein the method for forming the center portion further comprises: The central portion of a portion is removed to form a shape having the predetermined outer contour.

28. The method for manufacturing a polishing pad according to claim 26, wherein the coating material is different from the light-transmitting material.

29. The method for manufacturing a polishing pad according to claim 26, wherein the light-transmitting material transmits light under visible light. 30 . The method for manufacturing a polishing pad according to claim 26 , wherein the first curing process, the second curing process, and the third curing process respectively comprise a light irradiation process, a heating process, a pressurization process, or a static process. 31 . The method for manufacturing a polishing pad according to claim 26 , wherein an outer contour of the first mold is the same as an outer contour of the third mold. 32 . The method for manufacturing a polishing pad according to claim 26 , wherein an outer contour of the first mold is different from an outer contour of the third mold.

33. The method for manufacturing a polishing pad according to claim 26, wherein forming the detection window further comprises: A portion of the covering portion is removed to form a predetermined shape. 34 . The method for manufacturing a polishing pad according to claim 33 , wherein the predetermined shape is an irregular shape or a regular geometric shape.

35. A grinding method comprising: Providing a polishing pad, wherein the polishing pad is the polishing pad according to any one of claims 1 to 16; Applying pressure to the object so as to press it onto the polishing pad; as well as Relative motion is provided to the object and the polishing pad to perform a polishing process.