Production process of decorative gypsum board based on phase change microcapsule technology
By introducing glass fiber mesh and embedded parts into the gypsum board and combining phase change energy storage materials, the problems of simple structure and single function of the gypsum board are solved, and higher structural strength and temperature adjustment capabilities are achieved, and buildings are improved energy-saving effect.
Patent Information
- Application Number
- CN202411079334.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
The existing gypsum board has simple structure and is easy to damage, has a single function and cannot adjust the building temperature.
Using a production process based on phase change microcapsule technology, the structural strength is enhanced by adding glass fiber mesh and embedded parts to the gypsum board, and the phase change energy storage material is combined with gypsum, and the retarder, water reducing agent and composite excitation is used. The agent controls the solidification time and improves the overall performance of gypsum board.
The structural strength of the gypsum board is enhanced, the stable heat release of temperature changes is achieved, and the energy storage capacity and energy saving effect of the building is improved.
Smart Images

Figure CN118990785A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of gypsum board production, in particular to a production process of decorative gypsum board based on phase change microcapsule technology. Background Art
[0002] Gypsum board is a material made of building gypsum as the main raw material. It is a building material with light weight, high strength, thin thickness, easy processing, good sound insulation, heat insulation and fire resistance. It is one of the new lightweight boards that are currently being developed. Gypsum board has been widely used in various buildings such as residences, office buildings, shops, hotels and industrial plants for interior partitions, wall coverings (instead of wall plastering), ceilings, sound-absorbing panels, ground base panels and various decorative panels. It is not suitable for indoor installation in bathrooms or kitchens.
[0003] However, the existing gypsum board structure is too simple. It is not only easy to be damaged during use, but also easy to be damaged during the production of phase change energy storage gypsum board (especially curved and other special-shaped gypsum boards). At the same time, the composition of the gypsum board is too simple and the function is single, and it does not have the effect of regulating the building temperature. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a production process for decorative gypsum board based on phase change microcapsule technology to solve the problems of the existing gypsum board having a simple structure, being easily damaged, having a single function, and not being able to adjust the building temperature.
[0005] To achieve the above objectives, the present invention is implemented by the following technical scheme: A production process of decorative gypsum board based on phase change microcapsule technology, comprising the following steps:
[0006] S1, making gypsum slurry, mixing desulfurized building gypsum, cement, lime powder and latex powder in proportion to form a composite binder, making vitrified microspheres, expanded perlite and hollow microspheres in proportion to make light aggregate, making octadecane wax and expanded perlite in proportion to make phase change material, and mixing the composite binder, light aggregate, phase change material, admixture and water to form phase change energy storage gypsum slurry;
[0007] S2, cleaning the mold, spraying a mixed solution of soapy water and ammonia water on the inner side of the arc mold, and scraping the inner side of the arc mold with a wooden scraper to scrape off the plaster residue in the arc mold, and finally rinsing the inner side of the arc mold with clean water;
[0008] S3, making the surface layer of the gypsum board, after the arc-shaped mold is dry, applying a release agent on the inner side of the arc-shaped mold, and then applying a first gypsum layer on the inner side of the arc-shaped mold, and waiting for the first gypsum layer to solidify;
[0009] S4, stacking, placing a first glass fiber mesh on the first gypsum layer, placing a number of T-shaped embedded parts on the surface of the first glass fiber mesh, and reinforcing them with short fiber felt products, applying a second gypsum layer on the first glass fiber mesh, the second gypsum layer completely covers the bottom plate of the embedded parts, after the second gypsum layer solidifies, placing a second glass fiber mesh on the second gypsum layer, and applying a third gypsum layer on the second glass fiber mesh, after the third gypsum layer solidifies, placing a third glass fiber mesh on the third gypsum layer, and applying a fourth gypsum layer on the third glass fiber mesh, and waiting for the fourth gypsum layer to solidify;
[0010] S5. Smoothing and demoulding: Use a small scraper to smooth the plaster solidified on the arc-shaped mold, and demould it one and a half hours after the plaster is made to avoid deformation caused by heating of the plaster product.
[0011] Preferably, the components of the composite adhesive component are: 150-200 parts of desulfurized building gypsum, 5-8 parts of cement, 3-6 parts of lime powder, and 3 parts of latex powder.
[0012] Preferably, the components of the lightweight aggregate are: 70-90 parts of vitrified microspheres, 30-40 parts of expanded perlite, and 40-60 parts of hollow microspheres. The three lightweight hollow structural materials are mixed in proportion, which can reduce water absorption and improve compressive strength while maintaining a low thermal conductivity of the lightweight aggregate.
[0013] Preferably, the main component of the phase change material is: 30-40 parts of octadecane wax, which is an organic phase change material with adjustable phase change point, high latent heat of phase change (200 J / g), stable performance, non-toxic and non-corrosive, cheap, no supercooling or precipitation. With the increase of the amount of octadecane wax, the compressive strength, bonding strength and softening coefficient of the thermal insulation mortar are correspondingly improved, while the water absorption rate is correspondingly reduced, and the thermal conductivity is slightly increased. This is due to the fact that octadecane wax has certain tensile strength, adhesion, flexibility and waterproof sealing. When the amount of octadecane wax is small, the water absorption rate and thermal conductivity are relatively low because the open pores of the expanded perlite are not completely closed by the octadecane wax. When the open pores are completely closed or even when the octadecane wax is in excess, the water absorption rate is the lowest, but the thermal conductivity is increased, and the compressive strength and bonding strength are also reduced.
[0014] Preferably, the components of the admixture are: 0.3-0.5 parts of retarder, 0.5-1 parts of water reducing agent, 2-3 parts of composite activator, 2-3 parts of wood fiber. Compared with cement, the initial setting and final setting time of desulfurized building gypsum is much shorter, and retarders are commonly used to adjust the setting time of gypsum. Generally, the addition of retarders such as citric acid, polyphosphates, etc. will reduce the strength of gypsum to varying degrees, and the strength loss will increase with the increase in the amount added.
[0015] The composite activator contains early strength components. The addition of the composite activator can greatly promote the early hydration speed of desulfurized gypsum, increase the content of hydrated calcium silicate C-S-H gel, and also increase the content of Ca(OH)2, which promotes the reaction of desulfurized gypsum. As the hydration reaction proceeds further, the fibrous C-S-H and needle-shaped Aft increase significantly, and the gypsum crystals are connected and bonded with the surface hydration products, which helps to increase the strength. The addition of water reducer can reduce the mixing water consumption of thermal insulation gypsum slurry, improve the softening coefficient and fluidity of thermal insulation gypsum slurry, and reduce the slump and linear shrinkage.
[0016] Preferably, when preparing the phase change material, the expanded perlite is added to a water bath heating reactor at a temperature of 80°C and a vacuum negative pressure of 0.5 to 0.6 MPa. The reactor is evacuated for 20 minutes, and then the melted octadecane wax is added. The evacuation is continued at a negative pressure of 0.9 to 1.0 MPa and the temperature is kept at this temperature for 30 minutes so that the octadecane wax liquid is completely adsorbed by the open pores of the expanded perlite. The reactor is then unloaded and cooled to prepare the phase change material.
[0017] The present invention provides a production process of decorative gypsum board based on phase change microcapsule technology, which has the following beneficial effects:
[0018] 1. The present invention arranges a plurality of glass fiber meshes and embedded parts in the gypsum board, and utilizes the glass fiber meshes to enhance the structural strength of the gypsum board, so that the special-shaped gypsum board is not easily damaged during demoulding and use, and at the same time utilizes the embedded parts to facilitate the installation and disassembly of the special-shaped gypsum board;
[0019] 2. The present invention combines phase change energy storage materials with gypsum, which can not only stabilize the temperature change during the aging and heat release of gypsum, but also effectively improve the energy storage capacity and energy-saving effect of the building;
[0020] 3. The present invention can effectively control the setting time of the gypsum slurry by adding a retarder, a water reducing agent, a composite activator and wood fiber to the gypsum slurry, making the production of the gypsum board more convenient, while helping to increase the strength of the gypsum board and improving the overall performance of the gypsum board. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a structural schematic diagram of the gypsum board of the present invention;
[0022] Figure 2 It is a structural schematic diagram of the arc mold of the present invention.
[0023] In the figure:
[0024] 1. The first gypsum layer; 2. The first glass fiber mesh; 3. The embedded parts; 4. The second gypsum layer; 5. The second glass fiber mesh; 6. The third gypsum layer; 7. The third glass fiber mesh; 8. The fourth gypsum layer; 9. The arc mold. DETAILED DESCRIPTION
[0025] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] Example 1
[0027] See also Figure 1-2 This embodiment provides a new technical solution, which is a production process of decorative gypsum board based on phase change microcapsule technology. The production process includes the following steps:
[0028] S1, making gypsum slurry, mixing desulfurized building gypsum, cement, lime powder and latex powder in proportion to form a composite binder, making vitrified microspheres, expanded perlite and hollow microspheres in proportion to make light aggregate, making octadecane wax and expanded perlite in proportion to make phase change material, and mixing the composite binder, light aggregate, phase change material, admixture and water to form phase change energy storage gypsum slurry;
[0029] S2, cleaning the mold, spraying a mixed solution of soapy water and ammonia water on the inner side of the arc mold 9, and scraping the inner side of the arc mold 9 with a wooden scraper to scrape off the plaster residue in the arc mold 9, and finally rinsing the inner side of the arc mold 9 with clean water;
[0030] S3, making the surface layer of the gypsum board, after the arc-shaped mold 9 is dried, applying a release agent on the inner side of the arc-shaped mold 9, and then applying a first gypsum layer 1 on the inner side of the arc-shaped mold 9, and waiting for the first gypsum layer 1 to solidify;
[0031] S4, stacking, placing a first glass fiber mesh 2 on the first gypsum layer 1, placing a number of T-shaped embedded parts 3 on the surface of the first glass fiber mesh 2, and reinforcing them with short fiber felt products, applying a second gypsum layer 4 on the first glass fiber mesh 2, the second gypsum layer 4 completely covers the bottom plate of the embedded parts 3, after the second gypsum layer 4 solidifies, placing a second glass fiber mesh 5 on the second gypsum layer 4, and applying a third gypsum layer 6 on the second glass fiber mesh 5, after the third gypsum layer 6 solidifies, placing a third glass fiber mesh 7 on the third gypsum layer 6, and applying a fourth gypsum layer 8 on the third glass fiber mesh 7, and waiting for the fourth gypsum layer 8 to solidify;
[0032] S5, leveling and demoulding, using a small scraper to level the gypsum solidified on the arc-shaped mold 9, and demoulding after the gypsum is made for one and a half hours to avoid deformation caused by heating of the gypsum product.
[0033] The components of the composite adhesive are: 150-200 parts of desulfurized building gypsum, 5-8 parts of cement, 3-6 parts of lime powder, and 3 parts of latex powder. Desulfurized building gypsum is the main inorganic cementing material. Its chemical composition is roughly the same as that of natural building gypsum. All technical indicators of desulfurized building gypsum meet the requirements of GB9776-88 "Building Gypsum". Its flexural strength and compressive strength exceed the standards of superior products. Therefore, it can be used as the main cementing material for excellent thermal insulation gypsum slurry. The organic-inorganic dual-adhesive composite binder is mainly composed of desulfurized building gypsum, supplemented by alkaline admixtures - cement and lime powder, and latex powder as a modified binder. When its mix ratio is: m (desulfurized building gypsum) ∶ m (cement) ∶ m (lime powder) ∶ m (latex powder) = 88 ∶ 5 ∶ 4 ∶ 3, its dosage (kg) in the volume (m3) of thermal insulation gypsum slurry has the following effect on the main properties: Under the condition that other factors in the basic formula remain unchanged, when the content of the composite adhesive group in the phase change energy storage gypsum slurry is 140 (kg / m 3 ), the compressive strength of the phase change energy storage gypsum slurry is 0.35MPa, the bonding strength is 54kPa, and the dry density is 325kg / m 3 The water absorption rate is 28% and the thermal conductivity is 0.068W / (m·K).
[0034] The components of lightweight aggregate are: 70-90 parts of vitrified microspheres, 30-40 parts of expanded perlite, and 40-60 parts of hollow microspheres. Mixing the three lightweight hollow structural materials in proportion can reduce water absorption and increase compressive strength while maintaining a low thermal conductivity coefficient of the lightweight aggregate.
[0035] The main components of the phase change material are: 30-40 parts of octadecane wax. Octadecane wax is an organic phase change material with adjustable phase change point, high phase change latent heat (200 J / g), stable performance, non-toxic and non-corrosive, low price, no supercooling or precipitation phenomenon. Under the condition that other factors in the basic formula remain unchanged, when the content of octadecane wax in the phase change energy storage gypsum slurry is 0%, the compressive strength of the phase change energy storage gypsum slurry is 0.55 MPa, the bonding strength is 81 kPa, the softening coefficient is 0.55, the water absorption rate is 26%, and the thermal conductivity is 0.067 W / (m·K).
[0036] The admixtures include: 0.3-0.5 parts of retarder, 0.5-1 parts of water reducing agent, 2-3 parts of composite activator, and 2-3 parts of wood fiber. Compared with cement, the initial and final setting time of desulfurized building gypsum is much shorter, and retarders are often used to adjust the setting time of gypsum. The addition of general retarders such as citric acid and polyphosphates will reduce the strength of gypsum to varying degrees, and the strength loss will increase with the increase of the added amount. The test results show that the retarding effect of animal protein retarder (SC) is better. When the dosage changes, its retarding time changes steadily, no mutation occurs, and the effect on the strength of gypsum is small.
[0037] The composite activator contains early strength components. The addition of the composite activator can greatly promote the early hydration speed of desulfurized gypsum, increase the content of hydrated calcium silicate C-S-H gel, and also increase the content of Ca(OH)2, which promotes the reaction of desulfurized gypsum. As the hydration reaction proceeds further, the fibrous C-S-H and needle-shaped Aft increase significantly, and the gypsum crystals are connected and bonded with the surface hydration products, which helps to increase the strength. The addition of water reducer can reduce the mixing water consumption of thermal insulation gypsum slurry, improve the softening coefficient and fluidity of thermal insulation gypsum slurry, and reduce the slump and linear shrinkage.
[0038] When preparing the phase change material, the expanded perlite is added into a water bath heating reactor at a temperature of 80°C and a vacuum negative pressure of 0.5-0.6 MPa. The reactor is evacuated for 20 minutes, and then the melted octadecane wax is added. The evacuation is continued at a negative pressure of 0.9-1.0 MPa and the temperature is kept at 30 minutes so that the octadecane wax liquid is completely adsorbed by the open pores of the expanded perlite. The reactor is then unloaded and cooled to make the phase change material.
[0039] Embodiment 2:
[0040] The difference between this embodiment and Embodiment 1 is that, under the condition that other factors in the basic formula remain unchanged, when the content of octadecane wax in the phase change energy storage gypsum slurry is 5%, the compressive strength of the phase change energy storage gypsum slurry is 0.57 MPa, the bonding strength is 87 kPa, the softening coefficient is 0.56, the water absorption rate is 25%, and the thermal conductivity is 0.069 W / (m·K).
[0041] Under the condition that other factors in the basic formula remain unchanged, when the content of the composite adhesive component in the phase change energy storage gypsum slurry is 160 (kg / m 3 ), the compressive strength of the phase change energy storage gypsum slurry is 0.66MPa, the bonding strength is 81kPa, and the dry density is 345kg / m 3 The water absorption rate is 14% and the thermal conductivity is 0.075W / (m·K).
[0042] Embodiment 3:
[0043] The difference between this use example and Example 1 is that, under the condition that other factors in the basic formula remain unchanged, when the content of octadecane wax in the phase change energy storage gypsum slurry is 7.5%, the compressive strength of the phase change energy storage gypsum slurry is 0.66MPa, the bonding strength is 94kPa, the softening coefficient is 0.57, the water absorption rate is 16%, and the thermal conductivity is 0.071W / (m·K).
[0044] Under the condition that other factors in the basic formula remain unchanged, when the content of the composite adhesive component in the phase change energy storage gypsum slurry is 180 (kg / m 3), the compressive strength of the phase change energy storage gypsum slurry is 0.70MPa, the bonding strength is 95kPa, and the dry density is 375kg / m 3 , water absorption is 9% and thermal conductivity is 0.082W / (m·K).
[0045] Embodiment 4:
[0046] The difference between this use example and Example 1 is that, under the condition that other factors in the basic formula remain unchanged, when the content of octadecane wax in the phase change energy storage gypsum slurry is 10%, the compressive strength of the phase change energy storage gypsum slurry is 0.69 MPa, the bonding strength is 105 kPa, the softening coefficient is 0.60, the water absorption rate is 10%, and the thermal conductivity is 0.073 W / (m·K).
[0047] Under the condition that other factors in the basic formula remain unchanged, when the content of the composite adhesive component in the phase change energy storage gypsum slurry is 200 (kg / m 3 ), the compressive strength of the phase change energy storage gypsum slurry is 0.73MPa, the bonding strength is 103kPa, and the dry density is 390kg / m 3 , water absorption is 8% and thermal conductivity is 0.094W / (m·K).
[0048] Embodiment 5:
[0049] The difference between this use example and Example 1 is that, under the condition that other factors in the basic formula remain unchanged, when the content of octadecane wax in the phase change energy storage gypsum slurry is 12.5%, the compressive strength of the phase change energy storage gypsum slurry is 0.58 MPa, the bonding strength is 98 kPa, the softening coefficient is 0.61, the water absorption rate is 9%, and the thermal conductivity is 0.076 W / (m·K).
[0050] With the increase of octadecane wax dosage, the compressive strength, bonding strength and softening coefficient of the thermal insulation mortar increase accordingly, while the water absorption rate decreases accordingly and the thermal conductivity increases slightly. This is due to the fact that octadecane wax has certain tensile strength, bonding properties, flexibility and waterproof sealing properties. When the amount of octadecane wax is small, the water absorption rate and thermal conductivity are relatively low because the open pores of the expanded perlite are not completely closed by the octadecane wax. When the open pores are completely closed or even when the octadecane wax is in excess, the water absorption rate is the lowest, but the thermal conductivity increases, and the compressive strength and bonding strength also decrease.
[0051] In each cubic meter of thermal insulation mortar, with the increase of the amount of composite binder, the compressive strength, bonding strength, dry density and thermal conductivity of the thermal insulation mortar increase accordingly, and the water absorption rate gradually decreases. When the composite binder is 140kg, its compressive strength and bonding strength are too low, while the water absorption rate is high. When the amount exceeds 180kg, although the compressive strength and bonding strength are high and the water absorption rate is low, the thermal conductivity is high and the thermal insulation effect is poor. When the amount is controlled within the range of 160-180kg, the comprehensive performance is better.
[0052] When phase change energy storage decorative gypsum board is used for decoration, especially in areas with large temperature difference between day and night, the solar radiation and convection heat during the day cause the indoor temperature to rise. When the room temperature is higher than the phase change point of the decorative gypsum board, the gypsum board begins to absorb heat due to phase change and stores the heat energy, thereby slowing down the rate of increase of room temperature, lowering the indoor peak temperature, and reducing air conditioning power consumption; at night under air conditioning cooling or natural ventilation conditions, when the room temperature drops to the phase change temperature of the decorative gypsum board, the gypsum board begins to release heat due to reverse phase change, thereby slowing down the rate of decrease of room temperature, and the trough temperature is slightly higher than the control, which reduces the indoor peak-to-valley temperature difference and improves human comfort.
[0053] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A production process of decorative gypsum board based on phase change microcapsule technology, characterized in that: The following steps are involved: S1, making gypsum slurry, mixing desulfurized building gypsum, cement, lime powder and latex powder in proportion to form a composite binder, making vitrified microspheres, expanded perlite and hollow microspheres in proportion to make light aggregate, making octadecane wax and expanded perlite in proportion to make phase change material, and mixing the composite binder, light aggregate, phase change material, admixture and water to form phase change energy storage gypsum slurry; S2, cleaning the mold, spraying a mixed solution of soapy water and ammonia water on the inner side of the arc mold (9), and scraping the inner side of the arc mold (9) with a wooden scraper to scrape off the plaster residue in the arc mold (9), and finally rinsing the inner side of the arc mold (9) with clean water; S3, making a gypsum board surface layer, after the arc-shaped mold (9) is dried, applying a release agent on the inner side of the arc-shaped mold (9), then brushing a first gypsum layer (1) on the inner side of the arc-shaped mold (9), and waiting for the first gypsum layer (1) to solidify; S4, stacking, placing a first glass fiber mesh (2) on the first gypsum layer (1), placing a plurality of T-shaped embedded parts (3) on the surface of the first glass fiber mesh (2), and reinforcing them with short fiber felt products, applying a second gypsum layer (4) on the first glass fiber mesh (2), the second gypsum layer (4) completely covering the bottom plate of the embedded parts (3), and after the second gypsum layer (4) solidifies, placing a second glass fiber mesh (5) on the second gypsum layer (4), and applying a third gypsum layer (6) on the second glass fiber mesh (5), and after the third gypsum layer (6) solidifies, placing a third glass fiber mesh (7) on the third gypsum layer (6), and applying a fourth gypsum layer (8) on the third glass fiber mesh (7), and waiting for the fourth gypsum layer (8) to solidify; S5, leveling and demoulding, using a small scraper to level the gypsum solidified on the arc-shaped mold (9), and demoulding after one and a half hours of gypsum production to avoid deformation caused by heating of the gypsum product.
2. The production process of decorative gypsum board based on phase change microcapsule technology according to claim 1, characterized in that: The components of the composite adhesive group are: 150-200 parts of desulfurized building gypsum, 5-8 parts of cement, 3-6 parts of lime powder and 3 parts of latex powder.
3. The production process of decorative gypsum board based on phase change microcapsule technology according to claim 1, characterized in that: The components of the lightweight aggregate are: 70-90 parts of vitrified microspheres, 30-40 parts of expanded perlite, and 40-60 parts of hollow microspheres.
4. The production process of decorative gypsum board based on phase change microcapsule technology according to claim 1, characterized in that: The main component of the phase change material is 30 to 40 parts of octadecane wax.
5. The production process of decorative gypsum board based on phase change microcapsule technology according to claim 1, characterized in that: The components of the admixture are: 0.3-0.5 parts of retarder, 0.5-1 parts of water reducer, 2-3 parts of composite activator, and 2-3 parts of wood fiber.
6. The production process of decorative gypsum board based on phase change microcapsule technology according to claim 1, characterized in that: When preparing the phase change material, the expanded perlite is added into a water bath heating reactor at a temperature of 80°C and a vacuum negative pressure of 0.5-0.6 MPa. The reactor is evacuated for 20 minutes, and then the melted octadecane wax is added. The evacuation is continued at a negative pressure of 0.9-1.0 MPa and the temperature is kept at 30 minutes so that the octadecane wax liquid is completely adsorbed by the open pores of the expanded perlite. The reactor is then unloaded and cooled to make the phase change material.